A heterogeneous structure composite material supported platinum particle catalyst and preparation method thereof

By using SnS2 and SnO2 heterostructures as supports in low-temperature proton exchange membrane fuel cells, the stability and conductivity issues of the cathode catalyst were solved, the oxygen reduction performance and stability of the catalyst were improved, and the service life of the cell was extended.

CN115295815BActive Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210909651.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-12-06
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

In existing low-temperature proton exchange membrane fuel cell cathode catalysts, platinum particles have poor stability and conductivity, resulting in poor catalytic performance, especially severe catalyst degradation during start-up/shutdown operations and potential cycling.

Method used

A heterostructure formed by SnS2 and SnO2 is used as a support. SnO2 is generated in situ by partial oxidation of SnS2, forming a heterostructure composite material to support platinum particles. The strong metal-support interaction (SMSI) between SnO2 and SnS2 is used to improve the stability and conductivity of the catalyst.

Benefits of technology

The method improves the oxygen reduction catalytic performance of the catalyst, enhances the bonding strength between platinum particles and the support, extends the service life of the catalyst, and is simple, environmentally friendly, and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115295815B_ABST
    Figure CN115295815B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field related to cathode catalysts of low-temperature proton exchange membrane fuel cells, and discloses a heterogeneous structure composite material supported platinum particle catalyst and a preparation method. The catalyst includes a carrier and platinum particles attached to the carrier. The preparation method includes the following steps: S1 selects tin salt and organic sulfide to be dispersed in deionized water, performs a hydrothermal reaction, and dries the reaction product of the hydrothermal reaction to obtain SnS 2 Nanosheets; S2 SnS 2 The nanosheets are dispersed to form a uniform dispersion, an oxidant is added to the dispersion, and then a hydrothermal reaction is performed to obtain SnS 2 and SnO 2 The heterogeneous structure is formed; S3 disperses the heterogeneous structure in a reducing agent, adds a platinum source, heats, and dries to obtain a desired heterogeneous structure composite material loaded with platinum particles. The present invention solves the problems of poor stability and poor conductivity of non-carbon material loaded platinum particles in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to cathode catalysts of low-temperature proton exchange membrane fuel cells, and more specifically, relates to a heterogeneous structure composite material supported platinum particle catalyst and a preparation method thereof. Background Art

[0002] Low-temperature proton exchange membrane fuel cell (PEMFC) is a device that efficiently converts chemical energy such as hydrogen into electrical energy. It has the advantages of high conversion efficiency, low starting temperature, and cleanliness. It can make a huge contribution to my country's realization of carbon neutrality goals.

[0003] In proton exchange membrane fuel cells, the activation overpotential of the anode Pt catalyst is only tens of millivolts even at high current density, while the activation overpotential of the cathode Pt catalyst exceeds 300mV. Therefore, the quality of the cathode catalytic performance greatly affects the battery performance. At present, commercial platinum carbon (Pt / C) is the most widely used cathode catalyst in commercial applications, but this catalyst faces the problem of poor stability. The specific reasons are as follows: 1) The migration and merging of Pt on the carbon carrier to form larger particles. 2) Electrochemical Ostwald ripening. 3) Pt particles dissolve and then redeposit in the ion conductor. 4) Separation and agglomeration of Pt particles caused by corrosion of the carbon carrier. The reasons for carrier corrosion are mainly attributed to the following two points: first, carbon itself is oxidized during the potential cycle (0-1.5V); second, during the start / stop operation, a reverse current mechanism occurs, that is, the anode H2 will be mixed with a part of the air, and HOR (hydrogen oxidation reaction) and ORR (oxygen reduction reaction) reactions will occur on the anode side. At the same time, carbon corrosion and oxygen evolution reactions occur on the cathode side, resulting in a potential difference of up to 1.4 V, which in turn causes severe corrosion of the carbon carrier. Therefore, the potential cycle process and start / stop operation of the fuel cell will aggravate the attenuation of the catalyst.

[0004] Some recent studies have shown that replacing the carbon support with an oxide resistant to high-potential electrochemical corrosion can effectively protect the Pt particles. At the same time, due to the strong metal-support interaction (SMSI), the migration and agglomeration of Pt is seriously hindered, which greatly improves the stability of the catalyst. However, the main problem at present is that the poor conductivity and low specific surface area of ​​the oxide make it meet the needs of being a catalyst carrier. Therefore, it is a more conventional method to improve its conductivity by introducing a conductive auxiliary carrier to form a heterostructure composite carrier. The present invention provides a method for forming a heterostructure composite material by self-oxidation of a conductive auxiliary carrier, and at the same time provides ideas for developing high-activity and high-stability cathode catalysts of related structures. Summary of the invention

[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a method for solving the problems of poor stability and poor conductivity of platinum particles loaded with non-carbon materials in the prior art.

[0006] To achieve the above-mentioned purpose, according to one aspect of the present invention, a heterogeneous structure composite material supported platinum particle catalyst is provided, the catalyst comprising a carrier and platinum particles attached to the carrier, the carrier is a heterogeneous structure formed by SnS2 and SnO2, wherein SnS2 is used as a precursor, and SnO2 is particles grown in situ on the SnS2 after partial oxidation of SnS2.

[0007] Further preferably, the loading amount of the platinum particles accounts for .

[0008] More preferably, the size of the platinum particles is 4 nm to 6 nm.

[0009] According to another aspect of the present invention, there is provided a method for preparing the above-mentioned catalyst, the method comprising the following steps:

[0010] S1: dispersing a tin salt and an organic sulfide in deionized water to form a mixed solution, then subjecting the mixed solution to a hydrothermal reaction, and drying the reaction product of the hydrothermal reaction to obtain SnS2 nanosheets;

[0011] S2: dispersing the SnS2 nanosheets in deionized water to form a uniform dispersion, adding an oxidant to the dispersion, and then performing a hydrothermal reaction, wherein the SnS2 is partially oxidized in the hydrothermal reaction to form SnO2 supported on the SnS2, and drying to obtain a heterogeneous structure formed by SnS2 and SnO2;

[0012] S3: dispersing the heterogeneous structure in a reducing agent, adding a platinum source, heating the reaction so that the platinum source is reduced to platinum nanoparticles and loaded on the heterogeneous structure, and drying to obtain the desired heterogeneous structure composite material loaded with platinum particles catalyst.

[0013] Further preferably, in step S1, the tin salt is tin chloride, stannous chloride or tin oxalate, the organic sulfide is thiourea or thioacetamide, and the molar ratio of the tin salt to the organic sulfide is 1:(4-6).

[0014] Further preferably, in step S1, the temperature of the hydrothermal reaction is 180°C to 230°C, and the time is 8h to 12h.

[0015] Further preferably, in step S2, the oxidant is hydrogen peroxide or nitric acid, and the mass concentration thereof is 20% to 40%.

[0016] Further preferably, in step S2, the temperature of the hydrothermal reaction is 140° C. to 180° C., and the reaction time is 1 h to 4 h.

[0017] Further preferably, in step S3, the platinum source is chloroplatinic acid, potassium chloroplatinate or ammonium chloroplatinate, and the reducing agent is ethylene glycol or sodium borohydride.

[0018] Further preferably, in step S3, the heating temperature is 120° C. to 160° C., and the heating time is 1 h to 2 h.

[0019] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:

[0020] 1. The present invention uses SnS2 nanosheets partially loaded with SnO2 as a carrier of platinum particles. Compared with the prior art method of using only SnS2 as a carrier, the SnS2 nanosheets react in situ on SnS2 to generate SnO2, and the SnO2 is coated on the surface of SnS2, so that the SnS2 carrier remains stable during the redox process, and the carrier structure does not collapse, thereby preventing the platinum particles from falling off, thereby ensuring the activity of the catalyst; compared with the method of using only SnO2 as a carrier, the formed SnS2-SnO2 band gap is wider, the electron transmission is faster, the conductivity of the carrier is better, and thus the activity of the catalyst is better;

[0021] 2. In the present invention, SnS2 nanosheets partially loaded with SnO2 are used as carriers of platinum particles, wherein SnO2 is obtained by in-situ growth of partial oxidation of SnS2, and SnO2 is coated on the surface of SnS2. SnO2 has a stronger bond with platinum particles than SnS2, thereby improving the stability of the catalyst. In addition, since SnS2 and SnO2 have different bandgap widths and different valence band heights, electronic orbital coupling will be formed, and electrons will be transferred from SnS2, a material with a high valence band, to SnO2, another material with a low valence band, thereby accelerating electron transmission, and the conductivity of the heterogeneous material is better, that is, the conductivity of the obtained catalyst is better;

[0022] 3. The present invention provides a non-carbon heterogeneous structure corrosion-resistant carrier. Since there is no carbon in the material, the degradation of the carrier is avoided; the Pt nanoparticles are mainly loaded on the heterogeneous interface formed by SnS2 and SnO2, and the remaining Pt particles are loaded on the SnO2 nanoparticles. There is a strong metal-carrier interaction between the non-carbon heterogeneous structure carrier and the Pt nanoparticles. By regulating the oxidation time of SnS2, a suitable carrier with more heterogeneous interfaces and higher conductivity can be obtained, thereby improving the stability and activity of the catalyst. At the same time, SnS2 itself has certain oxygen reduction properties, and using it as a carrier for loading Pt further improves the activity of the catalyst;

[0023] 4. The heterogeneous structure carrier-supported Pt particle catalyst prepared by the present invention has excellent oxygen reduction catalytic performance. Compared with commercial platinum-carbon catalysts, the heterogeneous structure carrier-supported Pt particle catalyst has a 3-fold increase in specific mass activity under oxygen reduction reaction, and also has excellent stability. The electrochemical active area is not lost under 10,000 cycles of 1-1.5V potential cycles, and the electrochemical active area loss is less than 20% after 50,000 cycles of 1-1.5V potential cycles, while the commercial platinum-carbon catalyst loses more than 40% of its electrochemical active area under 10,000 cycles of 1-1.5V potential cycles;

[0024] 5. The present invention adjusts the proportion of the reducing agent to make the reduced Pt particles uniform in size, 4-6 nm. Compared with the organic phase method commonly used in this field, the synthesis method is simpler, has lower raw material costs and is more environmentally friendly. Most importantly, the Pt particles synthesized in situ by the synthesis method have better contact with the carrier and stronger interaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a preparation flow chart of a non-carbon heterogeneous structure composite material supported platinum particle catalyst constructed according to an embodiment of the present invention;

[0026] Figure 2 1 is a transmission electron micrograph of a catalyst prepared according to Example 1 of the present invention, wherein (a) is a transmission electron micrograph of the catalyst with a scale of 50 nm, and (b) is a transmission electron micrograph of the catalyst with a scale of 100 nm;

[0027] Figure 3 is an X-ray diffraction pattern of the catalyst prepared according to Example 1 of the present invention;

[0028] Figure 4 This is a comparison chart of the electrochemical performance of the catalyst prepared according to Example 1 of the present invention and commercial platinum-carbon;

[0029] Figure 5 is a 1-1.5V high potential cycle stability diagram of the catalyst prepared according to Example 1 of the present invention;

[0030] Figure 6 is a transmission electron microscope image of the catalyst prepared according to Example 2 of the present invention;

[0031] Figure 7 is an X-ray diffraction pattern of the catalyst prepared according to Example 2 of the present invention;

[0032] Figure 8 is an X-ray diffraction pattern of a carrier constructed according to Example 3 of the present invention;

[0033] Fig. 9is an X-ray diffraction pattern of the catalyst prepared according to Example 3 of the present invention;

[0034] Fig.10 is an X-ray diffraction pattern of a carrier constructed according to Example 4 of the present invention;

[0035] Fig.11 is an X-ray diffraction pattern of the catalyst prepared according to Example 4 of the present invention;

[0036] Fig.12 is an X-ray diffraction pattern of a carrier constructed according to Example 5 of the present invention;

[0037] Fig.13 is an X-ray diffraction pattern of the catalyst prepared according to Example 5 of the present invention;

[0038] Fig.14 is an X-ray diffraction pattern of a carrier constructed according to Example 6 of the present invention;

[0039] Fig.15 is an X-ray diffraction pattern of the catalyst prepared according to Example 6 of the present invention;

[0040] Fig.16 is an X-ray diffraction pattern of a carrier constructed according to Example 7 of the present invention;

[0041] Fig.17 It is an X-ray diffraction pattern of the catalyst prepared according to Example 7 of the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0043] A method for preparing a heterogeneous structure composite non-carbon material-supported platinum particle catalyst, wherein a non-carbon corrosion-resistant material is used as a catalyst carrier, that is, corrosion-resistant SnO2 is composited with SnS2 with good conductivity, and used as a carrier for supporting Pt nanoparticles, so that the catalyst has good stability and durability. The final catalyst is SnS2 nanosheets partially supported by SnO2, which are supported by Pt nanoparticles of uniform size. Due to the SMSI effect between SnO2 and Pt, the degradation of the carrier and Pt particles is reduced at the same time, and the activity and stability of the fuel cell cathode catalyst are improved. The synthesis process is simple, energy-saving and emission-reducing, easy to mass produce, and the service life of the fuel cell is extended.

[0044] The heterostructure uses SnS2 as a precursor, and forms SnO2 particles loaded on SnS2 nanosheets through partial oxidation, thus forming a heterogeneous interface; Figure 2 The platinum particle size obtained from the transmission electron microscope image of the catalyst is: the platinum particle size is 4-6nm, and the platinum loading accounts for 10% to 20% of the total weight of the catalyst.

[0045] like Figure 1 As shown, a method for preparing a heterogeneous structure composite material supported platinum particle catalyst comprises the following steps:

[0046] (1) dispersing the tin salt and the organic sulfur-containing compound in deionized water respectively, and forming a uniform, clear and transparent liquid through ultrasonic treatment;

[0047] (2) mixing two uniformly dispersed transparent liquids, ultrasonically dispersing the mixture, placing the mixture in a reaction kettle, subjecting the mixture to a hydrothermal reaction, collecting the product by centrifugation, and then drying the product in a freeze dryer;

[0048] (3) dispersing the product obtained in step (2) in deionized water and forming a uniform dispersion by ultrasonic treatment;

[0049] (4) adding an oxidant to the uniform dispersion obtained in step (3), transferring the mixture to a reactor for hydrothermal reaction, collecting the product by centrifugation after the reaction, and freeze-drying the product to obtain a reaction product;

[0050] (5) dispersing the reaction product obtained in step (4) in a mixed solution of a reducing agent, adding a certain amount of a platinum source, heating the solution and condensing and refluxing, collecting the product by centrifugation after the reaction is completed, and obtaining the final product after freeze-drying.

[0051] Preferably, the tin salt in step (1) is tin chloride pentahydrate; the mass concentration of hydrogen peroxide in step (4) is 30%; and the platinum source in step (5) is chloroplatinic acid or potassium chloroplatinate.

[0052] In step (1), the tin salt is tin chloride, stannous chloride, tin oxalate, etc., the organic sulfide is thiourea, thioacetamide, etc., and the molar ratio of the tin salt to the organic sulfide is 1:4 to 1:6.

[0053] In step (4), the oxidant is hydrogen peroxide, nitric acid, etc., and its mass concentration is 20-40%.

[0054] In step (5), the platinum source is at least one of chloroplatinic acid, potassium chloroplatinate, and ammonium chloroplatinate, and the reducing agent is at least one of ethylene glycol and sodium borohydride.

[0055] The ultrasonic dispersion time in step (1) and step (3) is 15 min to 20 min; the ultrasonic dispersion time in step (2) is 30-60 min.

[0056] Preferably, the rotation speed of the centrifugal treatment in step (2), step (4) and step (5) is 9000-11000 rpm, and the centrifugation time is 10-20 min.

[0057] Preferably, the washing liquid used for centrifugation is a mixture of deionized water and ethanol, and the volume ratio of deionized water to ethanol is 4:1.

[0058] Preferably, in step (2), the temperature of the hydrothermal reaction is 180°C to 230°C, and the reaction time is 8h to 12h; in step (4), the temperature of the hydrothermal reaction is 140°C to 180°C, and the reaction time is 1h to 4h.

[0059] Preferably, in step (4), when the reducing agent is ethylene glycol, the volume ratio of ethylene glycol to water is 3:1 to 1:1, the condensation reflux temperature is 120-160°C, the heating rate is 10°C / min, and the time is 1-2h. The ratio of ethylene glycol to water is optimized to make the Pt particles uniform in size, 4-6nm. Compared with the commonly used organic phase method in this field, the synthesis method is simpler, the raw material cost is lower, and it is more environmentally friendly. Most importantly, the Pt particles synthesized in situ by the synthesis method have better contact with the carrier and stronger interaction.

[0060] Starting from the potential-pH diagram of the material, the present invention selects a SnO2 material that can still stably exist under the conditions of potential 0-1.5V and pH=0 as the main material of the carrier. This greatly improves the stability of the catalyst under the operating conditions of the fuel cell, especially under extreme conditions of start-stop and variable load. The stability is far superior to that of current commercial catalysts, which is very important for promoting the large-scale application of fuel cells.

[0061] A non-carbon heterogeneous structure composite carrier of the present invention avoids the degradation of carbon materials in potential cycling and start / stop operation, and greatly improves the stability of the catalyst. SnS2 is used as a transition material for SnO2 to obtain a partially oxidized SnS2 / SnO2 heterogeneous structure material, which greatly improves the conductivity of the carrier and overcomes the disadvantage of low conductivity of the oxide. In addition, since there is no carbon in the material, the degradation of the carrier is avoided, and the presence of the oxide also ensures the stability of the carrier itself. At the same time, due to the presence of the heterogeneous interface, the electron transfer in the carrier is greatly accelerated, and the activity of the oxygen reduction reaction is improved. Finally, due to the SMSI effect between the oxide and Pt, the degradation of the Pt particles is limited, which greatly improves the stability of the catalyst. At the same time, the material synthesis process is controllable, can be prepared on a large scale, and is easy to promote industrialization.

[0062] There is a strong metal-carrier interaction between the non-carbon heterostructure carrier synthesized in the present invention and the Pt nanoparticles. By regulating the oxidation time of SnS2, a suitable carrier with more heterogeneous interfaces and higher conductivity can be obtained, thereby improving the stability and activity of the catalyst. At the same time, SnS2 itself has certain oxygen reduction performance, and using it as a carrier for loading Pt further improves the activity of the catalyst.

[0063] The present invention will be further described below with reference to specific embodiments.

[0064] Example 1

[0065] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0066] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0067] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0068] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in a mixed solution of 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid, wherein the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm, wash it three times with a mixed solution of deionized water and ethanol in a volume ratio of 4:1, and freeze-dry it to obtain the final catalyst product.

[0069] Figure 2 The transmission electron microscope image of the catalyst prepared in this example is shown in FIG. Figure 3 The X-ray diffraction pattern of the catalyst prepared in this example is shown in FIG. Figure 2 Middle (a), Figure 2 (b) and Figure 3It can be seen that some SnO2 particles are loaded on the SnS2 nanosheets, and Pt particles of uniform size of about 4nm are loaded on the heterogeneous structure material. The electrochemical performance comparison of this catalyst and commercial platinum carbon catalyst is shown in the figure Figure 4 ,Depend on Figure 4 It can be seen that compared with commercial platinum-carbon catalysts, the Pt particle catalyst loaded on a heterogeneous structure carrier has a 3-fold increase in specific mass activity under the oxygen reduction reaction, and its performance is significantly better than that of commercial platinum-carbon catalysts.

[0070] Figure 5 It is a performance diagram of the heterogeneous structure catalyst under 1-1.5V high potential cycling conditions. The electrochemical active area is not lost under 10,000 cycles of 1-1.5V potential cycling. After 50,000 cycles of 1-1.5V potential cycling, it only decays by 8mV, and the electrochemical active area loss is less than 20%. The electrochemical active area loss of the commercial platinum-carbon catalyst is more than 40% under 10,000 cycles of 1-1.5V potential cycling, indicating that the catalyst prepared in Example 1 has excellent stability.

[0071] Comparative Example 1

[0072] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea separately, disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0073] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 200°C for 8 hours, the obtained solution was centrifuged at 9000rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0074] S3: Weigh 16 mg of SnS2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0075] Figure 6 is a transmission electron microscope image of the catalyst prepared in Comparative Example 1, Figure 7The X-ray diffraction diagram of the catalyst prepared in Comparative Example 1 shows that the catalyst prepared in this embodiment is a hexagonal nanosheet carrier loaded with Pt particles of about 4 nm, which is a control sample of pure SnS2 loaded with Pt particles that has not been oxidized to SnO2. From the X-ray diffraction diagram and the transmission electron micrograph, it can be seen that the structures of the oxidized SnS2 / SnO2 and SnS2 remain unchanged.

[0076] Example 2

[0077] S1: Weigh 350 mg of tin chloride pentahydrate and 304 mg (molar ratio 1:4) of thiourea respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0078] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 210°C for 9 hours, the obtained solution was centrifuged at 9000 rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0079] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0080] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0081] Figure 8 is the X-ray diffraction pattern of SnS2 obtained in Example 3; Fig. 9 The X-ray diffraction pattern of the catalyst prepared in Example 3 shows that the catalyst prepared in this example is Pt particles supported by a hexagonal nanosheet carrier.

[0082] Example 3

[0083] S1: 350 mg of tin chloride pentahydrate and 456 mg (molar ratio 1:6) of thiourea were respectively weighed and dispersed in 20 mL of deionized water, and ultrasonically dispersed in an ultrasonic machine for 15 min.

[0084] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 230°C for 12 hours, the resulting solution was centrifuged at 9000 rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0085] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0086] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0087] Fig.10 is the X-ray diffraction pattern of SnS2 obtained in Example 3; Fig.11 The X-ray diffraction diagram of the catalyst prepared in Example 4 shows that the catalyst prepared in this example is Pt particles supported by a hexagonal nanosheet carrier.

[0088] Example 4

[0089] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea separately, disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0090] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 230°C for 8 hours, the resulting solution was centrifuged at 9000 rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0091] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0092] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0093] Fig.12 is a transmission electron microscope image of the catalyst prepared in Example 2, Fig.13 This is the X-ray diffraction diagram of the catalyst prepared in Example 5. From the analysis of the diagram, it can be seen that the catalyst prepared in this example is Pt particles supported by hexagonal nanosheet carriers.

[0094] Example 5

[0095] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea separately, disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0096] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 180°C for 9 hours, the obtained solution was centrifuged at 9000 rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0097] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0098] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0099] Fig.14 is a transmission electron microscope image of the catalyst prepared in Example 2, Fig.15 This is the X-ray diffraction diagram of the catalyst prepared in Example 6. From the analysis of the diagram, it can be seen that the catalyst prepared in this example is Pt particles supported by a hexagonal nanosheet carrier.

[0100] Example 6

[0101] S1: Weigh 1.8 g of tin chloride pentahydrate and 2.25 mg of thiourea respectively, disperse them in 50 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0102] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, then placed in a 100mL reactor. After hydrothermal reaction at 180°C for 10 hours, the obtained solution was centrifuged at 9000rpm to obtain the material, which was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then the obtained pure SnS2 was dried in a freeze dryer.

[0103] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 140°C for 90 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0104] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0105] Fig.16is a transmission electron microscope image of the catalyst prepared in Example 2, Fig.17 This is the X-ray diffraction diagram of the catalyst prepared in Example 7. From the analysis of the diagram, it can be seen that the catalyst prepared in this example is Pt particles supported by hexagonal nanosheet carriers.

[0106] Example 7

[0107] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0108] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0109] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 20% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 60 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0110] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 120°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0111] Example 8

[0112] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0113] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0114] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 40% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 4 h. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0115] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 120°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 2 hours. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0116] Example 9

[0117] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0118] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0119] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 30% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 240 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0120] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 160°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0121] Example 10

[0122] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0123] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0124] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 20% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 160°C for 200 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0125] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0126] Embodiment 11

[0127] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0128] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0129] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 20% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 240 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0130] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 120°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1 hour. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0131] Example 12

[0132] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0133] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0134] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 20% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 240 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0135] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 160°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 2 hours. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0136] Example 13

[0137] S1: Weigh 350 mg of tin chloride pentahydrate and 380 mg of thiourea (molar ratio 1:5) respectively and disperse them in 20 mL of deionized water, and ultrasonically disperse them in an ultrasonic machine for 15 min.

[0138] S2: The two transparent liquids of S1 were mixed and ultrasonicated for 15 minutes, added into a 100 mL reactor, and hydrothermaled at 190°C for 12 hours. Subsequently, the resulting solution was centrifuged at 9000 rpm for 10 minutes, and the centrifugal product was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain pure SnS2.

[0139] S3: Weigh 100 mg of pure SnS2 and disperse it in 40 mL of deionized water. After ultrasonic dispersion in an ultrasonic machine for 30 min, add 150 microliters of 20% H2O2, and then transfer the mixed solution into a 100 mL reactor and hydrothermal it at 180°C for 240 min. Subsequently, the obtained solution was centrifuged at 9000 rpm for 10 min, and the obtained material was washed three times with a mixture of deionized water and ethanol in a volume ratio of 4:1, and then freeze-dried to obtain SnS2 / SnO2 material.

[0140] S4: Weigh 16 mg of SnS2 / SnO2 and ultrasonically disperse it in 7.5 mL of ethylene glycol, 1.5 mL of deionized water and 1 mL of chloroplatinic acid solution, where the concentration of the chloroplatinic acid solution is 10 mg / mL. Heat the dispersion to 130°C at a heating rate of 10°C / min for condensation and reflux, and keep warm for 1.5 hours. Then centrifuge the obtained solution at 9000 rpm to obtain the material, wash it three times with a mixture of water and ethanol in a volume ratio of 4:1, and then dry the collected powder in a freeze dryer to obtain the final catalyst material.

[0141] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heterogeneous structure composite material supported platinum particle catalyst, characterized in that: The catalyst comprises a carrier and platinum particles attached to the carrier, wherein the carrier is a heterogeneous structure formed by SnS2 and SnO2, wherein the SnS2 nanosheets are used as precursors, and the SnO2 is particles that are in-situ grown on the SnS2 nanosheets after partial oxidation of the SnS2 nanosheets.

2. The heterogeneous structure composite material supported platinum particle catalyst according to claim 1, characterized in that: The loading amount of the platinum particles accounts for 10% to 20% of the total weight of the catalyst.

3. A heterogeneous structure composite material supported platinum particle catalyst as claimed in claim 1 or 2, characterized in that: The size of the platinum particles is 4 nm to 6 nm.

4. The method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: S1: dispersing a tin salt and an organic sulfide in deionized water to form a mixed solution, then subjecting the mixed solution to a hydrothermal reaction, and drying the reaction product of the hydrothermal reaction to obtain SnS2 nanosheets; S2: dispersing the SnS2 nanosheets in deionized water to form a uniform dispersion, adding an oxidant to the dispersion, and then performing a hydrothermal reaction, wherein the SnS2 is partially oxidized in the hydrothermal reaction to form SnO2 supported on the SnS2, and drying to obtain a heterogeneous structure formed by SnS2 and SnO2; S3: dispersing the heterostructure in a reducing agent, adding a platinum source, heating the reaction so that the platinum source is reduced to platinum nanoparticles and loaded on the heterostructure, and drying to obtain the desired heterostructure composite material loaded with platinum particles catalyst.

5. The preparation method according to claim 4, characterized in that: In step S1, the tin salt is tin chloride, stannous chloride or tin oxalate, the organic sulfide is thiourea or thioacetamide, and the molar ratio of the tin salt to the organic sulfide is 1:(4-6).

6. The preparation method according to claim 4, characterized in that: In step S1, the temperature of the hydrothermal reaction is 180°C to 230°C, and the time is 8h to 12h.

7. The preparation method according to claim 4, characterized in that: In step S2, the oxidant is hydrogen peroxide or nitric acid, and the mass concentration thereof is 20% to 40%.

8. The preparation method according to claim 4, characterized in that: In step S2, the temperature of the hydrothermal reaction is 140°C to 180°C, and the reaction time is 1h to 4h.

9. The preparation method according to claim 4, characterized in that: In step S3, the platinum source is chloroplatinic acid, potassium chloroplatinate or ammonium chloroplatinate, and the reducing agent is ethylene glycol or sodium borohydride.

10. The preparation method according to claim 4, characterized in that: In step S3, the heating temperature is 120°C to 160°C, and the heating time is 1h to 2h.