Laminated polyester resin coated metal sheet, laminated polyester resin film and can lid

By designing a laminated structure in a resin-coated metal plate, combined with a specific ratio of polyester resin and soft ingredients and heat treatment, the problem of conflicting opening and processability is solved, and a high level of can lid performance is achieved, including opening, Processability and corrosion resistance.

CN115298025BActive Publication Date: 2024-10-15TOYO KOHAN CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180021038.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-03
Filing Date
2021-03-23
Publication Date
2024-10-15
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Existing resin-coated metal plates are prone to feathering and film rupture when opening, making it difficult to balance opening and processability, and their corrosion resistance is insufficient.

Method used

The metal plate is coated with laminated polyester resin, the lower layer contains 2 to 30 mol% of the first copolymer component modified polyester resin, and the upper layer contains a soft component that is incompatible with the main polyester resin, and the content of the soft component in 100 mass% It is 2 to 50 mass% and is optimized through specific layer thickness and heat treatment process.

Benefits of technology

It improves the opening and processability of can lids, inhibits film rupture and resin peeling, and enhances corrosion resistance and adhesion to metal substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115298025B_ABST
    Figure CN115298025B_ABST
Patent Text Reader

Abstract

The present invention provides a laminated polyester resin coated metal sheet which, in addition to having good opening properties when opened, also has various properties at a high level, including suppressing film rupture near a rivet portion provided on a can lid (processability), suppressing resin peeling after retorting treatment after filling with contents (adhesion), and suppressing corrosion of a metal substrate after aging (corrosion resistance). The laminated polyester resin coated metal sheet of the present invention comprises: a metal substrate; a lower layer formed on at least one surface of the metal substrate and comprising a polyester resin (A) modified with 2 to 30 mol % of a first copolymer component; and an upper layer formed on the lower layer and comprising a polyester resin (B) and a softening component (C) incompatible with the polyester resin (B), wherein the content of the softening component (C) is 2 to 50 wt % when the total of the polyester resin (B) and the softening component (C) is 100 wt %.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated polyester resin coated metal plate, a laminated polyester resin film for a metal plate laminate, and a can lid using the same. Background Art

[0002] Conventionally, as can lids for metal cans for beverages and foods, open-ended (EO) lids have been widely used, such as a stay-on-tab (SOT) type that can be easily opened by hand and leaves the opening attached to the can body, and a tear-off type that separates the opening from the can body.

[0003] As a material of such a can lid, a resin-coated metal sheet in which a resin layer such as a polyester resin is formed on a metal base material such as aluminum or steel is known.

[0004] As a requirement for the resin-coated metal sheet used in the can lid, it is required that the opening portion can be opened smoothly. For example, Patent Document 1 discloses a resin-coated metal sheet, the purpose of which is to suppress the occurrence of feathering when formed on the lid and improve the opening property.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 4236514 Summary of the invention

[0008] Problems to be solved by the invention

[0009] In the resin-coated metal sheet disclosed in Patent Document 1, as a resin layer laminated on the metal sheet, a resin layer having a multilayer structure of a lower layer and a surface layer is disclosed, wherein the lower layer is a thermoplastic polyester resin compounded with an olefin polymer, and the surface layer is a thermoplastic polyester with controlled crystallinity and an elongation of 20%. Thus, in Patent Document 1, the resin layer is multilayered for the purpose of achieving both corrosion resistance and processability. However, in the technology of Patent Document 1, there is still a problem regarding opening property (feathering resistance).

[0010] That is, requirements for can lids using resin-coated metal sheets are to achieve both suppression of the feathering phenomenon during opening (opening property) and suppression of film rupture in the can lid (processability).

[0011] Regarding the opening property, when the can lid is opened, the resin layer is cut along the score (score) formed on the can lid. That is, it is required to avoid the occurrence of delamination (stratification) between the metal substrate and the resin layer in the opening portion, and the phenomenon (feathering phenomenon) of the coating resin remaining on the inner surface side stretched near the opening. In order to improve the opening property, it is considered necessary to suppress the softness (elongation) of the resin to a certain extent.

[0012] On the other hand, regarding processability, in addition to the general notching process of the can lid, the rib process for reinforcement and the elongation and drawing process for forming the rivet part are also performed, so the resin layer needs to be able to follow the above-mentioned processing on the metal substrate. Furthermore, when the above-mentioned processing is performed in a heat treatment process such as printing, it is necessary to avoid film rupture, peeling, etc. at the above-mentioned large processing site. In addition, in order to improve such processability, the resin used needs to be soft to a certain extent.

[0013] That is, the above-mentioned processability and opening property can be said to be contradictory characteristics, and in can lids using resin-coated metal sheets, development of a resin that satisfies both of these characteristics is required.

[0014] In addition, as general issues in can lids, it is of course necessary to have performances of suppressing resin peeling after retorting after filling with contents (adhesion) and suppressing corrosion of the metal base material after aging (corrosion resistance).

[0015] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved at a high level by setting the resin layer structure to a predetermined structure in a laminated polyester resin film or a laminated polyester resin-coated metal sheet for can lid production, thereby arriving at the present invention.

[0016] Means for solving problems

[0017] In order to achieve the above-mentioned purpose, a laminated polyester resin coated metal plate in one embodiment of the present invention (1) is characterized in that it comprises a metal substrate and a laminated polyester resin layer formed on at least one surface of the metal substrate, wherein the laminated polyester resin layer comprises, in order from the metal substrate side: a lower layer comprising a polyester resin (A) modified with 2 to 30 mol % of a first copolymer component; and an upper layer comprising a polyester resin (B) and a soft component (C) incompatible with the polyester resin (B), wherein the content of the soft component (C) is 2 to 50 wt % when the total of the polyester resin (B) and the soft component (C) is set to 100 wt %.

[0018] It should be noted that the laminated polyester resin coated metal sheet described in (1) above preferably has (2) the polyester resin (B) being a thermoplastic polyester resin having a glass transition temperature (Tg1) of 60°C or higher and 90°C or lower, the soft component (C) being any one or both of a polyester-based thermoplastic elastomer and a polyolefin, the soft component (C) being dispersed in the polyester resin (B), and when the content (mass %) of the soft component (C) in the upper layer is set to W, the absolute value ΔTg of the difference between the glass transition temperature (Tg1) of the polyester resin (B) and the glass transition temperature (Tg2) of the upper layer satisfies ΔTg<0.5×W.

[0019] In addition, the laminated polyester resin coated metal plate described in (1) or (2) above preferably has (3) the soft component (C) dispersed in the polyester resin (B) in the form of islands, and the average major axis of the soft component (C) dispersed in the form of islands is 0.1 to 5.0 μm, and the average minor axis is 0.01 to 2 μm.

[0020] In the laminated polyester resin-coated metal sheet according to any one of (1) to (3) above, (4) the polyester resin (A) is mainly composed of polyethylene terephthalate and contains isophthalic acid as the first copolymer component.

[0021] In the laminated polyester resin-coated metal sheet described in (4) above, it is preferred that (5) the lower layer further contains 0.01 to 0.5 mol % of a multifunctional component.

[0022] In the laminated polyester resin-coated metal sheet according to any one of (1) to (5) above, it is preferred that (6) the polyester resin (A) has a weight average molecular weight of 40,000 to 80,000.

[0023] In the laminated polyester resin-coated metal sheet according to any one of (1) to (6) above, (7) the polyester resin (A) preferably contains 0.1 to 5.0 mass % of inorganic particles having an average particle size of 0.2 to 5.0 μm.

[0024] In addition, the laminated polyester resin-coated metal sheet described in any one of (1) to (7) above preferably has (8) a total thickness of the upper layer and the lower layer of 10 to 50 μm, a thickness of the upper layer of 5 to 40 μm, and a thickness of the lower layer of 5 to 30 μm.

[0025] In the laminated polyester resin-coated metal sheet described in any one of (1) to (8) above, (9) the lower layer preferably has a breaking elongation of 50% or less in a 50°C environment after heat treatment at 185°C for 10 minutes.

[0026] The laminated polyester resin-coated metal sheet according to any one of (1) to (9) above preferably further comprises (10) a surface layer formed on the side of the upper layer opposite to the metal substrate side and containing a polyester resin.

[0027] In addition, in order to achieve the above-mentioned purpose, a laminated polyester resin film in one embodiment of the present invention (11) is characterized in that it has: a lower layer, which is formed on at least one side of a metal substrate and contains a polyester resin (A) modified with 2 to 30 mol % of a first copolymer component; and an upper layer, which is formed on the lower layer and contains a polyester resin (B) and a soft component (C) incompatible with the polyester resin (B), and when the total of the polyester resin (B) and the soft component (C) is set to 100 mass %, the content of the soft component (C) is 2 to 50 mass %.

[0028] In order to achieve the above object, a can lid (12) according to one embodiment of the present invention is formed by using the laminated polyester resin-coated metal sheet described in any one of (1) to (10).

[0029] In order to achieve the above object, a can lid (13) in another embodiment of the present invention is formed by using the laminated polyester resin film described in (11) above.

[0030] Effects of the Invention

[0031] According to the present invention, for example, a laminated polyester resin coated metal plate, a laminated polyester resin film, and a can lid can be realized which are suitable for use as a can lid and have not only opening properties when opened but also high levels of suppression of film rupture near the rivet portion provided in the can lid (processability). In addition, according to the laminated polyester resin coated metal plate, the laminated polyester resin film, and the can lid of the present invention, various properties such as suppression of resin peeling after retorting treatment after filling with contents (adhesion) and suppression of corrosion of the metal base material after aging (corrosion resistance) can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 1 is a schematic diagram showing a cross section of a laminated polyester resin-coated metal plate 100 according to the present embodiment. DETAILED DESCRIPTION

[0033] Hereinafter, the laminated polyester resin coated metal sheet, the laminated polyester resin film, and the can lid of the present invention will be described using embodiments, but the present invention is not limited to the following embodiments.

[0034] [Laminated polyester resin coated metal sheet]

[0035] First, use Figure 1The laminated polyester resin coated metal plate 100 of the present embodiment is described. The laminated polyester resin coated metal plate 100 of the present embodiment includes a metal substrate MP and a laminated polyester resin layer 200 formed on at least one surface of the metal substrate MP. The laminated polyester resin layer 200 includes a lower layer 10 and an upper layer 20 sequentially formed on the metal substrate MP.

[0036] In other words, the laminated polyester resin coated metal plate 100 of the present embodiment comprises: a metal substrate MP; a lower layer 10 close to the metal substrate MP side, which is formed on at least one surface of the metal substrate MP and contains a polyester resin (A) modified with 2 to 30 mol % of a first copolymer component; and an upper layer 20, which is formed on the lower layer 10 (on the side opposite to the metal substrate MP side), and contains a polyester resin (B) and a soft component (C) incompatible with the polyester resin (B), and when the total of the polyester resin (B) and the soft component (C) is set to 100 mass %, the content of the soft component (C) is 2 to 50 mass %.

[0037] It should be noted that the laminated polyester resin coated metal plate 100 of the present embodiment is not limited to Figure 1 The two-layer structure of the lower layer 10 and the upper layer 20 shown in the figure may be a structure of three or more layers as described in detail later.

[0038] <Metal substrate>

[0039] As the metal substrate MP used for the laminated polyester resin-coated metal plate 100 of the present embodiment, a known metal substrate MP such as an aluminum material or a steel plate that has been conventionally used for easy-open lids can be used.

[0040] As the aluminum material, pure aluminum or aluminum alloy is used. The thickness of the aluminum material varies depending on the size of the cover, etc., and is generally in the range of 0.20-0.50 mm, particularly 0.23-0.30 mm. In addition, a surface treatment film such as chromate treatment, zirconium treatment, phosphoric acid treatment, polyacrylic acid treatment, etc. may be formed on the surface of the aluminum material.

[0041] As the steel sheet, for example, a chromate surface treated steel sheet such as TFS (tin-free steel) with a tin plating amount of 0.3 to 2.8 g / m 2 Various known steel plates such as sputtered steel plates subjected to plating treatment. The thickness of the steel plate is preferably in the range of 0.1 mm to 0.4 mm, particularly 0.12 mm to 0.35 mm.

[0042] <Lower level>

[0043] Next, the lower layer 10 in the laminated polyester resin coated metal sheet 100 of the present embodiment will be described. Figure 1As shown, the lower layer 10 is formed on at least one surface of the metal substrate MP. In addition, the lower layer 10 of the laminated polyester resin layer 200 and the upper layer 20 described later is formed on the side close to the metal substrate MP.

[0044] The polyester resin (A) used in the lower layer 10 of the laminated polyester resin coated metal plate 100 of the present embodiment is a copolymerized polyester resin modified with 2 to 30 mol % of the first copolymer component. Specifically, the polyester resin (A) is preferably a copolymerized resin mainly composed of polyethylene terephthalate.

[0045] As the first copolymer component, at least one selected from the group consisting of isophthalic acid (IA), phthalic acid, p-(β-hydroxyethoxy)benzoic acid, naphthalene 2,6-dicarboxylic acid, diphenoxyethane-4,4′-dicarboxylic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, adipic acid, sebacic acid, trimellitic acid and pyromellitic acid can be cited. Among them, the first copolymer component is preferably isophthalic acid from the viewpoint of processability and adhesion.

[0046] The first copolymer component is preferably contained in the copolymerized polyester resin of the lower layer 10 at 2 to 30 mol%. If the first copolymer component is less than 2 mol%, the adhesion between the metal substrate MP and the lower layer 10 may be reduced, which is not preferred. On the other hand, if the first copolymer component exceeds 30 mol%, it is not only economically undesirable, but also the film forming properties and barrier properties of the lower layer 10 may be reduced, which is not preferred.

[0047] Furthermore, the amount of the first copolymer component in the copolyester resin of the lower layer 10 is more preferably 5 to 15 mol %.

[0048] Furthermore, in the copolymerized polyester resin of the lower layer 10 in the laminated polyester resin-coated metal plate 100 suitable for this embodiment, as the diol components contained, in addition to ethylene glycol, one or more of propylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexanediol, cyclohexanedimethanol, ethylene oxide adducts of bisphenol A, etc. can also be mentioned.

[0049] Furthermore, in the present embodiment, the copolyester resin of the lower layer 10 preferably further contains 0.01 to 0.5 mol% of a second copolymer component (multifunctional component) different from the first copolymer component. The multifunctional component is introduced for the purpose of introducing a crosslinked structure and improving the opening property. It should be noted that when the content of the second copolymer component (multifunctional component) exceeds 0.5 mol%, it is not preferred from the viewpoint of easy generation of gel in the copolyester resin of the lower layer 10 and economical.

[0050] Examples of the polyfunctional component include one or more selected from trimellitic acid, trimellitic anhydride, pyromellitic acid, pyromellitic anhydride, trimethylolpropane, and pentaerythritol. Among them, trimellitic acid (TMA) or pentaerythritol is particularly preferred from the viewpoint of easy availability.

[0051] In the present embodiment, from the viewpoint of adjusting the viscosity of the lower layer resin and the viewpoint of improving the opening property, the weight average molecular weight of the copolyester resin of the lower layer is preferably 40,000 to 80,000. When the weight average molecular weight is less than 40,000, there is a possibility that the film forming property of the resin layer is reduced, so it is not preferred. On the other hand, when the weight average molecular weight exceeds 80,000, the torque in the mixer may be excessively increased during the film forming of the resin layer, which is not preferred. It should be noted that from the same viewpoint, the more preferred weight average molecular weight is 40,000 to 55,000.

[0052] In this embodiment, from the viewpoints of improving the winding shape of the film, avoiding the generation of film wrinkles, and improving the opening property of the lid, the copolyester resin of the lower layer preferably contains 0.1 to 5.0% by mass of inorganic particles having an average particle size of 0.2 μm to 5.0 μm. It should be noted that as these inorganic particles, inorganic particles called so-called lubricants can be used.

[0053] On the other hand, when a method of manufacturing a resin-coated metal sheet by directly extruding a molten resin onto a metal substrate (also referred to as direct coating, etc.) is adopted, stable production can be performed even when the lower layer does not contain the above-mentioned inorganic particles.

[0054] Specifically, organic lubricants such as aliphatic hydrocarbons, higher aliphatic alcohols, fatty acids, fatty acid metal salts, esters or amide derivatives of fatty acids, such as stearamide, oleamide, erucamide, erucic acid amide, behenamide, and ethylenebisoleamide, or inorganic lubricants such as silica, aluminum silicate, and magnesium silicate, zeolite, calcium carbonate, silica, alumina, and barium sulfate, etc., can be used. Common commercially available lubricants.

[0055] As described above, the average particle size of these inorganic particles is preferably 0.2 μm to 5.0 μm, more preferably 1.0 μm to 3.0 μm. In addition, the content of these inorganic particles is preferably 0.1 to 5.0 mass %, more preferably 0.4 to 3.0 mass % in the copolymerized polyester resin of the lower layer in this embodiment.

[0056] The lower layer 10 of the present embodiment preferably has a breaking elongation of 50% or less in an environment of 50° C. after heat treatment at 185° C. for 10 minutes.

[0057] That is, the laminated polyester resin coated metal sheet of the present embodiment is heat-treated during the can lid manufacturing, printing, and steaming. It is generally known that in resin, the elongation at break after heat treatment is lower than the elongation at break before heat treatment. In the present invention, it is found that when the elongation at break of the film of the lower layer 10 at a specific temperature (at 50°C) after heat treatment under the above conditions is less than 50%, the can lid obtained can ensure stable opening even in areas with high temperatures, while also being able to take into account issues such as processability.

[0058] <Upper>

[0059] Next, the upper layer 20 in the laminated polyester resin coated metal plate 100 of the present embodiment will be described. Figure 1 As shown, the upper layer 20 is formed on the side opposite to the metal substrate MP of the lower layer 10. In other words, the lower layer 10 and the upper layer 20 are formed in order from the metal substrate MP. In addition, it can also be said that the metal substrate MP is formed on one side with the lower layer 10 in the middle, and the upper layer 20 is formed on the other side.

[0060] In addition, when applying to a can cover, it is preferable to manufacture the can cover so that the upper layer 20 becomes the content side of the can.

[0061] The resin composition of the upper layer 20 includes a polyester resin (B) as a main component and a softening component (C) that is incompatible with the polyester resin (B). The content of the softening component (C) is 2 to 50% by mass when the total of the polyester resin (B) and the softening component (C) is 100% by mass.

[0062] In the above description, the component with the largest content (mass ratio) among the solid components (non-volatile components excluding volatile substances such as water and solvent) forming the upper layer 20 is defined as the main agent.

[0063] When the content of the soft component (C) is less than 2% by mass, the processability of the laminated polyester resin coated metal sheet of the present embodiment may be reduced, which is not preferred. On the other hand, when the content of the soft component (C) exceeds 50% by mass, the opening property when made into a can lid may be reduced, which is not preferred. In the present embodiment, the content of the soft component (C) is more preferably 5 to 20% by mass.

[0064] From the viewpoint of heat resistance and impact resistance, the polyester resin (B) is preferably a thermoplastic polyester resin. Specific examples of thermoplastic polyester resins include polyethylene terephthalate (PET), polyethylene isophthalate, and polyesters obtained by copolymerizing these with aromatic dicarboxylic acids such as isophthalic acid, terephthalic acid, 2,6-naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, diphenyl sulfone dicarboxylic acid, diphenoxyethane dicarboxylic acid, diphenyl ether dicarboxylic acid, 5-sulfoisophthalic acid, and phthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid; alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid; aliphatic diols such as ethylene glycol, triethylene glycol, polyethylene glycol, polytetramethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, and neopentyl glycol; aromatic diols such as bisphenol A and bisphenol S, and alicyclic diols such as cyclohexanedimethanol. The above-mentioned thermoplastic resins may be used alone or in combination of two or more.

[0065] Among thermoplastic polyesters, thermoplastic polyesters containing ethylene terephthalate and / or ethylene isophthalate as main constituent components are preferred from the viewpoints of cost, flavor, etc. In this case, the main constituent component means that units derived from terephthalic acid components and isophthalic acid components as dicarboxylic acid components in ethylene terephthalate and / or ethylene isophthalate account for 50 mol% or more of all units derived from dicarboxylic acid components.

[0066] In addition, in the thermoplastic polyester used as the polyester resin (B), a multifunctional component selected from a polyacid and a polyol having more than three functions can be copolymerized. By copolymerizing the multifunctional component, when the film is manufactured at high speed, when the molten film is directly laminated on the metal plate at high speed to manufacture the laminated metal plate, the end (ear) of the film shakes, and the tensile resonance (ear swing) of the film thickness variation is reduced, so it is preferred. As a multifunctional component selected from a polyacid and a polyol having more than three functions, trimellitic acid, trimellitic anhydride, pyromellitic acid, pyromellitic anhydride, trimethylolpropane, pentaerythritol, etc. can be cited. The content of these multifunctional components in the thermoplastic polyester is 0.01 to 0.5 mol%, preferably 0.07 to 0.3 mol%. If the content of the multifunctional component is within the above range, it is possible to appropriately improve the tensile resonance reduction effect while suppressing the occurrence of gelation in the thermoplastic polyester.

[0067] The glass transition temperature (Tg1) of the polyester resin (B) used in the upper layer 20 is preferably 60°C or higher and 90°C or lower, more preferably 65°C to 85°C, and even more preferably 70°C to 80°C. When Tg1 is lower than 60°C, the heat resistance of the obtained film is reduced and the flavor may be reduced, which is not preferred. On the other hand, when Tg1 exceeds 90°C, the processability and impact resistance of the obtained film may be reduced, which is not preferred.

[0068] As a method for measuring the glass transition temperature, a known method can be applied, and for example, the glass transition temperature can be measured using a differential scanning calorimeter (DSC) at a temperature increase rate of 10° C. / min.

[0069] The intrinsic viscosity [η] of the thermoplastic polyester used as the polyester resin (B) is preferably 0.5 to 1.4 dl / g, more preferably 0.7 to 1.2 dl / g, and even more preferably 0.8 to 1.0 dl / g. It should be noted that the intrinsic viscosity [η] is a value measured at 30° C. after dissolving in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane = 1 / 1. By setting the intrinsic viscosity [η] to the above range, the impact resistance of the obtained film can be improved, and the moldability when the film is made can be further improved.

[0070] Next, the soft component (C) which is blended in the polyester resin (B) as the main component and is incompatible with the polyester resin (B) in the upper layer 20 of the present embodiment will be described. It should be noted that the term "incompatible" here means that when the upper layer 20 is observed, the boundary between the polyester resin (B) and the soft component (C) can be observed.

[0071] The soft component (C) in the upper layer 20 of the present embodiment is finely dispersed when mixed (blended) with the polyester resin (B) as the main component, and can form a sea-island structure (phase separation). In addition, the soft component (C) can impart rubber elasticity to the polyester resin (B) as the main component at room temperature. Furthermore, when the soft component (C) is mixed (blended) with the polyester resin (B) as the main component, it is preferred that the glass transition temperature (Tg) of the polyester resin (B) is hardly affected.

[0072] From such a viewpoint, in the present embodiment, specifically, either or both of a polyester-based thermoplastic elastomer and a polyolefin can be used as the soft component (C).

[0073] The polyester thermoplastic elastomer used as the soft component (C) preferably has a glass transition temperature (Tg) of room temperature (25°C) or lower, more preferably lower than 20°C, and further preferably lower than 10°C. It should be noted that the lower limit of the glass transition temperature (Tg) of the polyester thermoplastic elastomer used in the present embodiment is not particularly limited, but is preferably -50°C or higher.

[0074] The structure of the polyester thermoplastic elastomer generally includes a hard segment forming a hard crystal structure and a soft segment. Components constituting the hard segment of the polyester thermoplastic elastomer used in the present embodiment include terephthalic acid, isophthalic acid, bisphenol A, bisphenol S, 2,6-naphthalene dicarboxylic acid, ethylene glycol, 1,4-butanediol, and the like.

[0075] In addition, as the components constituting the soft segment, there can be mentioned aliphatic dicarboxylic acids such as adipic acid, sebacic acid, and dimer acid, aliphatic diols such as 1,6-hexanediol, 1,8-octanediol, and 1,10-decanediol, and polyethers such as polyethylene glycol and polytetramethylene glycol. Among them, polyethers are preferred, and polytetramethylene glycol is particularly preferred among the polyethers.

[0076] Moreover, as a preferred polyester-based thermoplastic elastomer, a polyether ester in which a hard segment composed of a dicarboxylic acid and a soft segment composed of a polyether unit are bonded via an ester bond can be cited. Among them, it is preferred that the polyester-based thermoplastic elastomer contains 50% by mass or more of polyether units. The content of the polyether unit in the polyester-based thermoplastic elastomer is more preferably 50 to 70% by mass. When the content of the polyether unit is less than 50% by mass, it is easy to be compatible with the thermoplastic polyester during melt kneading, and the heat resistance of the film is reduced, so it is not preferred.

[0077] The molecular weight of the polyether unit (polyether segment) in the polyester thermoplastic elastomer is not particularly limited, but preferably a polyether unit of 500 to 5000 is used. Furthermore, in order to improve the adhesion to metal, the polyester thermoplastic elastomer may be modified with maleic anhydride or the like. It should be noted that the polyester thermoplastic elastomer may contain at least one polyether unit, and may contain a plurality of polyether units.

[0078] As a particularly preferable polyester-based thermoplastic elastomer in the present embodiment, a resin obtained by copolymerizing polybutylene terephthalate and polytetramethylene glycol (PTMG) can be mentioned.

[0079] Next, the polyolefin in the soft component (C) in the upper layer 20 of the present embodiment is described. As the polyolefin used as the soft component (C), there can be cited low-density polyethylene, medium-density polyethylene, high-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, or chain polyolefin resins such as random copolymers or block copolymers of α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, headed by ethylene / propylene copolymers. In addition, so-called acid-modified polyolefins formed by grafting less than 2% of unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, and itaconic acid and their anhydrides into any of these polyolefins can be used. Ethylene vinyl acetate (EVA), ethylene-vinyl alcohol copolymer (EVOH), etc. can also be used.

[0080] Among the above-mentioned polyolefins, from the viewpoint of film forming properties, the melt flow rate (hereinafter referred to as MFR) MFR is preferably 30 g / 10 min or less.

[0081] Furthermore, an ionomer resin (ionically crosslinked olefin copolymer) or the like in which a part or all of the carboxyl groups in any of the above-mentioned polyolefins are ionically crosslinked with metal cations may also be used.

[0082] Ionomer resin is an ionic salt in which part or all of the carboxyl groups in the copolymer of ethylene and α, β-unsaturated carboxylic acid are neutralized by metal cations, and the degree of neutralization, that is, the ion concentration, affects its physical properties. Generally, the melt flow rate (hereinafter referred to as MFR) of the ionomer resin is affected by the ion concentration. If the ion concentration is large, the MFR is small. In addition, the melting point is affected by the carboxyl concentration. The larger the carboxyl concentration, the lower the melting point. Therefore, the ionomer resin used in the present invention is of course not limited to this. It is preferred that the MFR is less than 15 g / 10 minutes, and particularly preferably in the range of 5 g / 10 minutes to 0.5 g / 10 minutes, and the melting point is less than 100°C, and particularly preferably in the range of 97°C to 80°C.

[0083] As metal cations in the ionomer resin, Na + , K + , Li + 、Zn + , Z 2+ Mg 2+ , Ca 2+ 、Co 2+ 、Ni 2+ , Mn 2+ , Pb 2+ , Cu 2+ In this embodiment, the substance neutralized by zinc can be preferably used because of its high degree of crosslinking and low moisture sensitivity. In addition, part of the remaining carboxyl groups that have not been neutralized by metal ions can also be esterified with a lower alcohol.

[0084] In the upper layer 20 of the present embodiment, the relationship between the glass transition temperature (Tg1) of the above-mentioned polyester resin (B) and the glass transition temperature (Tg2) after mixing the above-mentioned soft component (C) with the polyester resin (B) as the main agent, when the content (mass %) of the above-mentioned soft component (C) in the upper layer 20 is set to W, preferably satisfies the following formula (1).

[0085] ΔTg<0.5×W ··· (1)

[0086] Here, ΔTg is the absolute value of the difference between Tg1 and Tg2.

[0087] The present inventors have conducted intensive studies and found that, when a soft component (C) is mixed with a polyester resin (B) as a main component in the upper layer 20, a so-called "sea-island structure" is formed in which the soft component (C) is dispersed in the polyester resin (B) of the upper layer in an island shape. In this case, it was found that by making the soft component (C) incompatible with the polyester resin (B) and satisfying the above formula (1) with respect to the content of the soft component (C), the change in Tg after blending the soft component is suppressed, thereby satisfying the opening property and processability.

[0088] In the above formula (1), when ΔTg is 0.5×W or more, if the content of the polyester thermoplastic elastomer is increased to improve impact resistance, the Tg of the film decreases and the heat resistance decreases, so that the impact resistance and heat resistance of the film cannot be achieved at the same time.

[0089] In addition, it is particularly preferable to satisfy the following formula (2).

[0090] ΔTg<0.2×W ··· (2)

[0091] In addition, in the upper layer of the laminated polyester resin film of this embodiment, the soft component (C) is preferably dispersed in the polyester resin (B) of the upper layer in the form of islands, and the average major axis of the soft component dispersed in the form of islands is 0.1 to 5.0 μm, and the average minor axis is 0.01 to 2 μm.

[0092] Regarding the above average major axis and average minor axis, if either value exceeds the above numerical range, the dispersed particle size of the soft component is large and the aspect ratio is large, so the opening property when made into a can lid may be reduced, which is not preferred.

[0093] The laminated polyester resin film of this embodiment can be added with additives such as light stabilizers, impact modifiers, compatibilizers, lubricants, plasticizers, antistatic agents, reaction catalysts, anti-coloring agents, free radical inhibitors, plasticizers, antistatic agents, end-capping agents, antioxidants, heat stabilizers, release agents, flame retardants, antibacterial agents, and mildewproofing agents.

[0094] Next, the thickness of the laminated polyester resin layer 200 in the present embodiment is described. The thickness of the laminated polyester resin layer 200 in the present embodiment is preferably in the range of 10 μm to 50 μm. When the thickness of the laminated polyester resin layer 200 exceeds 50 μm, it is not preferred from the perspective of economy and opening. On the other hand, when the thickness of the laminated polyester resin layer 200 is less than 10 μm, the processability and barrier properties when molded into a can lid may be reduced, so it is not preferred.

[0095] In addition, in the laminated polyester resin layer 200 of the present embodiment, the thickness ratio of the lower layer 10 to the upper layer 20 is preferably in the range of lower layer:upper layer=1:5 to 3:1 in terms of satisfying both opening property and processability. That is, if the lower layer is thicker than the above range, the opening property and impact resistance may become insufficient, and if the lower layer is thinner than the above range, the processability and corrosion resistance may become insufficient. It should be noted that the thickness ratio of the lower layer 10 to the upper layer 20 is more preferably in the range of lower layer:upper layer=1:3 to 1:1.

[0096] The thickness of each layer is not limited thereto, and the upper layer 20 is preferably in the range of 5 to 40 μm, particularly 5 to 15 μm. When the upper layer 20 is less than 5 μm, the processability when molding into a can lid may be reduced, which is not preferred.

[0097] The thickness of the lower layer 10 is preferably in the range of 5 to 30 μm, particularly 10 to 25 μm. If the thickness of the lower layer 10 is less than 5 μm, the opening property of the can lid may be deteriorated, which is not preferred.

[0098] The laminated polyester resin layer 200 of the present embodiment may include layers other than the lower layer 10 and the upper layer 20 described above. That is, as described above, when the laminated polyester resin layer 200 of the present embodiment is applied to a can lid, it is preferable to manufacture the can lid in such a manner that the upper layer 20 is on the side close to the contents of the can. In this case, for example, a surface layer 30 composed of a polyester resin can be provided on the side of the upper layer 20 that is further opposite to the metal substrate side (the side of the contents of the can). For example, by providing a polyethylene terephthalate layer as the surface layer 30, the flavor of the film can be improved, or by providing a polyethylene naphthalate layer, the barrier properties of the film can be improved.

[0099] In this embodiment, in order to improve the flavor, that is, to avoid the flavor change of the can content or to avoid the adsorption of the aroma components contained in the can content, it is preferred to form a surface layer 30. For these purposes, in this embodiment, a polyethylene terephthalate layer is preferably used as the surface layer 30. The polyethylene terephthalate layer used as the surface layer 30 may contain a copolymer component, for example, it may contain 5 mol% or less of isophthalic acid. The thickness of such a surface layer 30 is preferably in the range of 0.1 to 10 μm.

[0100] [Method for producing laminated polyester resin coated metal sheet]

[0101] The laminated polyester resin coated metal plate 100 of the present invention can be manufactured by a method (direct extrusion method) of directly extruding a molten resin film onto a metal substrate MP and extruding and integrating it between laminating rollers. In this case, the resin flows from the extruders are merged in a multi-layer die by using an extruder for the upper layer resin and an extruder for the lower layer resin, so that the lower layer resin is on the metal substrate side, and the resin is extruded from a T-die into a film.

[0102] The method for manufacturing the laminated polyester resin coated metal plate 100 is not limited to the above method. For example, a film having a lower layer 10 and an upper layer 20 may be manufactured by a known method, and then the film may be thermally bonded to the metal substrate MP in a manner such that the lower layer 10 is on the metal substrate MP side.

[0103] [Laminated polyester resin film]

[0104] The laminated polyester resin film in this embodiment can be manufactured by a known method as described above. For example, an extruder for the resin to be the upper layer 20 and an extruder for the resin to be the lower layer 10 are used, and the resin flows from each extruder are merged in a multi-layer die, and the resin is extruded from the T-die into a film, and then wound up by a known method, thereby obtaining a laminated polyester resin film. By using the laminated polyester resin film of this embodiment, the laminated polyester resin coated metal plate 100 can be manufactured by thermally bonding the lower layer 10 to the metal substrate MP side.

[0105] [Can lid]

[0106] The can lid of this embodiment can be formed by using the laminated polyester resin coated metal sheet 100 described above, so that the surface formed with the lower layer 10 and the upper layer 20 described above becomes the inner surface side of the can lid. It should be noted that the shape of the can lid of this embodiment can be set as a known easy-open lid of a pull-open method or a retaining pull-tab method. In addition, the manufacturing method of the can lid can apply a known method, so the description is omitted here.

[0107] Example

[0108] Next, the present invention will be described in more detail using the following examples, but the present invention is not limited thereto. It should be noted that the evaluation method of each characteristic is as follows.

[0109] [Evaluation and measurement methods]

[0110] (Method for producing laminated polyester resin coated metal sheet)

[0111] TFS (tin-free steel) with a plate thickness of 0.22 mm was used as the metal substrate. The resin materials of the upper and lower layers shown in Table 1 were supplied to a twin-screw extruder, and extruded at a temperature suitable for the resin material at the barrel and the T-die, thereby obtaining a film, which was laminated on the above-mentioned aluminum alloy plate heated to 250°C, and immediately water-cooled to obtain a laminated polyester resin-coated metal plate. At this time, the thickness of the resin on the inner surface of the cover was made to be the thickness shown in Table 2. After coating the side of the obtained single-sided laminated material that became the outer surface of the cover, the coating sintering was performed at 185°C for 10 minutes.

[0112] (Can cover manufacturing method)

[0113] The EO cap was formed from a 95.0 mm diameter blank of the laminated polyester resin coated metal sheet, and the outer surface of the cap was scored (residual pressure 75 μm), rivet-processed, and provided with an opening lug to produce the cap.

[0114] (Evaluation of opening property)

[0115] The lid obtained as described above was subjected to a steaming treatment at 120°C for 60 minutes. Then, the lid was opened by hand at a temperature of about 50°C, and the periphery of the opening was visually observed for evaluation. As evaluation criteria, the length of the peeling between the plate and the film (delamination length) when the lid was opened and the maximum elongation of the film at the opening were measured, and the evaluation was performed as follows. The results are shown in Table 2.

[0116] Delamination length◎: 0.5mm or less

[0117] ○: More than 0.5 mm and less than 1.0 mm

[0118] ×: more than 1.0 mm

[0119] Film elongation: 0.5mm or less

[0120] ○: More than 0.5 mm and less than 1.0 mm

[0121] ×: more than 1.0 mm

[0122] (Processability Evaluation)

[0123] Evaluation was performed using the current value when a voltage of 6.30 V was applied to the entire inner surface of the obtained can lid for 4.0 seconds.

[0124] ◎:0.01mA or less

[0125] ○: More than 0.01mA and less than 0.5mA

[0126] ×: more than 0.5mA

[0127] <Glass transition temperature (Tg)>

[0128] After melting using a differential scanning calorimeter (trade name "DSC8500", manufactured by Perkin Elmer Co., Ltd.), the solution was cooled to -50°C at 200°C / min. Then, the extrapolated start temperature of glass transition observed when the temperature was raised from -50°C to 280°C at 10°C / min was defined as the glass transition temperature (Tg).

[0129] <Major and minor diameters of the soft component dispersed in the upper layer>

[0130] The cross section of the film is observed with a scanning electron microscope, and the major and minor axes of the polyester thermoplastic elastomer or polyolefin dispersed in a 10 μm square are measured and averaged to determine the average major and minor axes.

[0131] <Examples 1 to 10>

[0132] In Examples 1 to 9, a thermoplastic elastomer (polytetramethylene glycol copolymerized polybutylene terephthalate) is used as a softening component in the upper layer. Examples 4 to 6 and 8 contain trimellitic acid (TMA) as a multifunctional component in the lower layer. In Example 9, a lubricant is added to the lower layer. In Example 10, a polyolefin (MFR: 0.9, melting point 80°C, Zn cross-linked ionomer) is used as a softening component in the upper layer. Example 11 is a three-layer structure in which a 2.0 μm PET / IA2 (isophthalic acid 2 mol% copolymerized polyethylene terephthalate resin) layer is formed on the surface.

[0133] As shown in the Examples, the laminated polyester resin film, the laminated polyester resin-coated metal sheet, and the can lid of the present invention all have excellent opening properties and processability.

[0134] <Comparative Examples 1 to 6>

[0135] Comparative Examples 1 to 3 used conventionally known two-layer films. In Comparative Examples 4 to 6, the configuration of the lower layer and the upper layer was reversed from that of the present invention. The laminated polyester resin films, laminated polyester resin coated metal sheets, and can lids of the present invention shown in the comparative examples did not have both opening properties and processability.

[0136] Table 1

[0137]

[0138] Table 2

[0139]

[0140] Industrial Applicability

[0141] The present invention can cope with complex and severe cover manufacturing processes while satisfying product requirements, and can be suitably used in the field of metal processing.

[0142] Description of Reference Numerals

[0143] MP Metal Substrate

[0144] 100-layer polyester resin coated metal sheet

[0145] 10 Lower Level

[0146] 20 Upper

[0147] 30 Surface

[0148] 200 layers of polyester resin

Claims

1. A laminated polyester resin coated metal sheet, characterized in that: A method of manufacturing a metal substrate, and a laminated polyester resin layer formed on at least one surface of the metal substrate, wherein the laminated polyester resin layer has, in order from the metal substrate side: a lower layer comprising a polyester resin (A) modified with 2 to 30 mol% of a first copolymerization component; and An upper layer comprising a polyester resin (B) and a soft component (C) incompatible with the polyester resin (B), wherein the soft component (C) is a polyester-based thermoplastic elastomer, the polyester-based thermoplastic elastomer is phase-separated in the polyester resin (B) and dispersed in an island shape, and the content of the polyester-based thermoplastic elastomer is 2 to 50% by mass when the total of the polyester resin (B) and the polyester-based thermoplastic elastomer is 100% by mass. The soft component (C) dispersed in the form of islands has an average major axis of 0.1 to 5.0 μm and an average minor axis of 0.01 to 2 μm.

2. The laminated polyester resin coated metal sheet according to claim 1, wherein The polyester resin (B) is a thermoplastic polyester resin having a glass transition temperature (Tg1) of 60° C. or higher and 90° C. or lower. When the content (mass %) of the soft component (C) in the upper layer is W, the absolute value ΔTg of the difference between the glass transition temperature (Tg1) of the polyester resin (B) and the glass transition temperature (Tg2) of the upper layer satisfies the following formula (1): ΔTg<0.5×W · · · (1).

3. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein: The polyester resin (A) is mainly composed of polyethylene terephthalate and contains isophthalic acid as the first copolymer component.

4. The laminated polyester resin coated metal sheet according to claim 3, wherein The lower layer further comprises 0.01 to 0.5 mol% of a multifunctional component.

5. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein The weight average molecular weight of the polyester resin (A) is 40,000 to 80,000.

6. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein The polyester resin (A) contains 0.1 to 5.0 mass % of inorganic particles having an average particle size of 0.2 to 5.0 μm.

7. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein: The total thickness of the upper layer and the lower layer is 10 to 50 μm, the thickness of the upper layer is 5 to 40 μm, and the thickness of the lower layer is 5 to 30 μm.

8. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein After the lower layer is heat treated at 185° C. for 10 minutes, the elongation at break in an environment of 50° C. is 50% or less.

9. The laminated polyester resin coated metal sheet according to claim 1 or 2, wherein The invention further comprises a surface layer formed on the side of the upper layer opposite to the metal substrate side and containing a polyester resin.

10. A laminated polyester resin film comprising: a lower layer formed on at least one surface of the metal substrate, comprising a polyester resin (A) modified with 2 to 30 mol % of a first copolymerization component; and An upper layer formed on the lower layer, comprising a polyester resin (B) and a soft component (C) incompatible with the polyester resin (B), wherein the soft component (C) is a polyester-based thermoplastic elastomer, the polyester-based thermoplastic elastomer is phase-separated in the polyester resin (B) and dispersed in an island shape, and the content of the polyester-based thermoplastic elastomer is 2 to 50% by mass when the total of the polyester resin (B) and the polyester-based thermoplastic elastomer is 100% by mass. The soft component (C) dispersed in the form of islands has an average major axis of 0.1 to 5.0 μm and an average minor axis of 0.01 to 2 μm.

11. A can lid using the laminated polyester resin-coated metal sheet according to any one of claims 1 to 9.

12. A can lid using the laminated polyester resin film according to claim 10.

Citation Information

Patent Citations

  • Polyester resin for metal coating and method for producing the same

    CN101646712A

  • Thermoplastic resin-coated metal plate and can body and can lid made from same

    CN105324242A

  • Metal sheet coated with thermoplastic resin and can obtained therefrom

    CN1503730A

  • Resin film for metal plate laminate, laminate metal plate, and its manufacturing method

    JP2001341258A

  • Can lid resin film, and can lid resin film covered-metal plate covered with can lid resin film and can lid using the same