Silicon wafer texturing and cleaning process, solar cell and preparation method thereof

By optimizing the texturing liquid formula and process parameters, combined with a multi-step cleaning process, the problem of poor uniformity of the texture structure on the silicon wafer surface has been solved, the yield and efficiency of heterojunction solar cells have been improved, and the occurrence of "water column marks" has been reduced. Black bad.

CN115312628BActive Publication Date: 2024-10-11TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211066218.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-01
Publication Date
2024-10-11
Estimated Expiration
2042-09-01

AI Technical Summary

Technical Problem

During the preparation process of heterojunction solar cells, the textured structure on the surface of the silicon wafer has poor uniformity, resulting in low product efficiency and yield. The traditional texturing cleaning process has the problem of "water jet printing", blackening and high isolation ratio.

Method used

By optimizing the texturing liquid formula and process parameters, combined with rough polishing and flower basket structure adjustment, the uniformity of the texture structure on the surface of the silicon wafer is improved. A multi-step cleaning process is adopted, including rough polishing, ozone cleaning, pre-cleaning, texturing, and post-processing. Cleaning, smoothing, passivation, washing and drying.

Benefits of technology

It significantly improves the uniformity of the texture structure on the surface of the silicon wafer, reduces the blackening defects of "water column printing", and improves product yield and battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115312628B_ABST
    Figure CN115312628B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon wafer texturing and cleaning process, a solar cell and a preparation method thereof. The silicon wafer texturing and cleaning process comprises the following steps: texturing the silicon wafer with a texturing liquid; wherein the texturing liquid comprises, by volume, 4.5 to 7 parts of an alkali metal hydroxide solution with a mass fraction of 40% to 50%, 1 part of a texturing additive, and 160 to 175 parts of water; the texturing treatment temperature is 83°C to 86°C, and the texturing treatment time is 450s to 700s. The silicon wafer texturing and cleaning process can effectively improve the uniformity of the velvet structure on the surface of the silicon wafer by optimizing and adjusting the formula of the texturing liquid and the texturing process parameters, solve the problem of too high isolation ratio of "water column prints" of solar cells prepared by traditional processes, and improve product yield and battery efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell generation, in particular to a silicon wafer texturing and cleaning process, a solar cell and a preparation method thereof. Background Art

[0002] Heterojunction (HJT) cells were first developed by Japan's Sanyo Corporation in 1990. Over the past 30 years, the industry has progressed through its embryonic stage, laboratory phase, initial commercialization, and gradual industrialization. A heterojunction is a special PN junction formed by depositing an amorphous silicon thin film on crystalline silicon. It is a type of N-type cell.

[0003] Heterojunction cells combine the advantages of crystalline silicon cells and thin-film cells, offering high conversion efficiency, low process temperatures, high stability, low degradation, and bifacial power generation. This technology is truly disruptive. From the dominance of aluminum back surface field (BSF) cells before 2015, to the rise of PERC (Passivated Emitter and Rear Cell) cells in 2015, which became the mainstream in the market, heterojunction cell technology has undergone two generations of evolution.

[0004] Currently, PERC cell conversion efficiency has reached its ceiling, and TOPCon (Tunnel Oxide Passivated Contact) cells have limited room for improvement. Market attention is gradually shifting to technologies such as HJT. Compared to PERC and TOPCon cells, HJT cells offer significant potential and are poised to become the mainstream third-generation cell technology. However, the biggest challenge facing HJT cells is cost. The high investment in raw materials and equipment required for HJT production has become the primary factor hindering its rapid development. Continuously improving product yield and production efficiency is a crucial prerequisite for large-scale mass production.

[0005] During the production of heterojunction solar cells, silicon wafers undergo a series of texturing and cleaning steps: rough polishing, ozone cleaning, pre-cleaning, texturing, post-cleaning, rounding, hydrofluoric acid passivation, slow pulling, and drying. The main purpose of the texturing step is to utilize the anisotropic etching properties of low-concentration alkaline solutions, which have different etching rates for crystalline silicon in different crystal orientations, to form a densely distributed "pyramid" structure of anti-reflective texture on the surface of the silicon wafer.

[0006] Due to the unique structure of heterojunction solar cells, the interface after texturing must be well matched with the amorphous silicon interface. Therefore, the requirements for silicon wafer surface cleanliness, uniformity, and stability of the textured surface are significantly higher than those for conventional monocrystalline silicon solar cells. However, traditional silicon wafer texturing and cleaning processes and equipment produce silicon wafers with poor textured surface uniformity, which seriously affects product efficiency, yield, and production capacity. Summary of the Invention

[0007] Based on this, it is necessary to provide a silicon wafer texturing and cleaning process, a solar cell and a preparation method thereof that can effectively improve the uniformity of the silicon wafer texture structure, improve product yield and battery efficiency.

[0008] The technical solutions proposed by the present invention are as follows:

[0009] According to one aspect of the present invention, a silicon wafer texturing and cleaning process is provided, comprising the following steps:

[0010] Use texturing liquid to texturing silicon wafers;

[0011] Among them, the texturing solution includes 4.5 to 7 parts of alkali metal hydroxide solution with a mass fraction of 40% to 50%, 1 part of texturing additive, and 160 to 175 parts of water by volume; the texturing treatment temperature is 83°C to 86°C, and the texturing treatment time is 450s to 700s.

[0012] In some embodiments, the texturing treatment is carried out in a texturing tank, which contains the texturing solution, and the volume of the texturing tank is 265L~275L; after each texturing treatment of 320~400 silicon wafers, 5.5L~8L of the texturing solution is discharged, and 150mL~200mL of the texturing additive, 6.5L~8.5L of water and 300mL~500mL of alkali metal hydroxide solution with a mass fraction of 40%~50% are added to the texturing tank.

[0013] In some embodiments, the circulation flow rate of the texturing solution during the texturing process is 26 L / min to 32 L / min.

[0014] In some embodiments, during the texturing process, the silicon wafer is placed on the bottom support rod of the flower basket, the flower basket is placed in the texturing solution, the diameter of the bottom support rod is 14mm to 16mm, and a through hole with a diameter of 2mm to 4mm is vertically opened on the bottom support rod.

[0015] In some embodiments, before texturing the silicon wafer with the texturing solution, the silicon wafer texturing cleaning process further includes the following steps:

[0016] performing a rough polishing treatment on the silicon wafer using a rough polishing solution;

[0017] The rough polishing solution comprises, by volume, 12 to 15 parts of an alkali metal hydroxide solution having a mass fraction of 40% to 50% and 220 to 250 parts of water; and the rough polishing treatment time is 70s to 80s.

[0018] In some embodiments, the rough polishing treatment is carried out in a rough polishing tank, which contains the rough polishing solution, and the volume of the rough polishing tank is 230L to 260L; after each rough polishing treatment of 320 to 400 silicon wafers, 4L to 6L of the rough polishing solution is discharged, and 1000mL to 1200mL of an alkali metal hydroxide solution with a mass fraction of 40% to 50% and 5L to 6.5L of water are added to the rough polishing tank.

[0019] In some embodiments, after the silicon wafer is subjected to rough polishing treatment using a rough polishing solution and before the silicon wafer is subjected to texturing treatment using a texturing solution, the silicon wafer texturing cleaning process further includes the following steps:

[0020] performing ozone cleaning on the silicon wafer after the rough polishing treatment using a solution containing hydrofluoric acid, hydrochloric acid and ozone; and

[0021] The silicon wafer after ozone cleaning is pre-cleaned using a solution containing sodium hydroxide and hydrogen peroxide.

[0022] In some embodiments, after texturing the silicon wafer with the texturing solution, the silicon wafer texturing cleaning process further includes the following steps:

[0023] Post-cleaning the silicon wafer after the texturing treatment using a solution containing sodium hydroxide and hydrogen peroxide;

[0024] Using a solution containing hydrofluoric acid, hydrochloric acid and ozone to perform a rounding treatment on the silicon wafer after the post-cleaning treatment;

[0025] Passivating the smoothed silicon wafer using a solution containing hydrofluoric acid; and

[0026] The silicon wafer after the passivation treatment is sequentially subjected to water washing treatment, slow pulling dehydration treatment and drying treatment.

[0027] According to another aspect of the present invention, there is provided a method for preparing a solar cell, comprising the following steps:

[0028] Providing a silicon wafer, and performing texturing and cleaning on the silicon wafer using the silicon wafer texturing and cleaning process of the present invention; and

[0029] The silicon wafer after texturing and cleaning is made into a solar cell.

[0030] In some embodiments, the silicon wafer after texturing and cleaning is made into a solar cell, comprising the following steps:

[0031] forming an intrinsic amorphous silicon layer on the silicon wafer after texturing and cleaning;

[0032] forming a doped amorphous silicon layer on the intrinsic amorphous silicon layer;

[0033] forming a transparent conductive film on the doped amorphous silicon layer; and

[0034] An electrode is formed on the transparent conductive film.

[0035] According to another aspect of the present invention, a solar cell is provided. The solar cell is prepared by the above-mentioned preparation method of the present invention.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The present invention can effectively improve the uniformity of the velvet structure on the surface of silicon wafers by optimizing and adjusting the formula of the velvet solution and the velvet process parameters, alleviate the problem of excessively high isolation ratio of "water column marks" in battery cells prepared by traditional processes, and improve product yield and battery efficiency.

[0038] By optimizing and adjusting the rough polishing solution and the process parameters of the rough polishing treatment, combined with the adjustment of the texturing solution formula and texturing process parameters, the uniformity of the texture structure on the surface of the silicon wafer after texturing can be further improved, further improving product yield and battery efficiency.

[0039] By optimizing and adjusting the structure of the flower basket, the uniformity of the velvet structure on the silicon wafer surface can be further improved, and the product yield and battery efficiency can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the process flow of the silicon wafer texturing and cleaning process of the present invention;

[0041] Figure 2 It is a structural schematic diagram of the velvet making tank and the flower basket in the present invention;

[0042] Figure 3 It is a structural schematic diagram of the bottom support rod of the flower basket in the present invention.

[0043] Description of reference numerals:

[0044] 10. Texturing tank; 11. Flow balancing plate; 20. Flower basket; 21. Bottom support rod; 22. Flower basket teeth; 23. Through hole; 100. Silicon wafer; 111. Liquid inlet hole. DETAILED DESCRIPTION

[0045] To make the above-mentioned objects, features, and advantages of the present invention more readily apparent, specific embodiments of the present invention are described in detail below. The following description sets forth numerous specific details to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art may make similar modifications without departing from the scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0046] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one such feature. In the description of the present invention, "plurality" means at least two, such as two, three, etc., unless otherwise specifically defined.

[0047] In the present invention, unless otherwise specified or limited, the terms "installed," "connected," "connect," "fixed," etc. should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection, electrical connection; direct connection, or indirect connection through an intermediate medium; internal communication between two components, or interaction between two components, unless otherwise specified. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0049] The silicon wafers produced by the traditional silicon wafer texturing and cleaning process have the problem of poor uniformity of the texturing structure, resulting in a high proportion of black isolation of the "water column mark" on the battery cell, which seriously affects the efficiency, yield and production capacity of the product.

[0050] Through research, the inventors discovered that one of the main causes of the above-mentioned problems is the unreasonable ratio of the texturing solution and the design of the process parameters when texturing the silicon wafer. This causes the silicon wafer to react slowly during the texturing process, resulting in large differences in the textured surface area. Moreover, as the number of production batches increases, the differences in the textured surface area become more obvious. The inconsistent texture structure on the silicon wafer surface will cause uneven deposition and passivation in the subsequent coating process, and ultimately form a black "water column mark", which seriously affects the efficiency and yield of the product. Frequent replacement of the texturing solution will lead to liquid waste and increased production costs.

[0051] In order to solve the above problems, some embodiments of the present invention provide a silicon wafer texturing and cleaning process, which includes the following steps arranged in sequence: rough polishing, ozone cleaning, pre-cleaning, texturing, post-cleaning, smoothing, passivation, water washing, slow pulling and dehydration, and drying. The process flow diagram is shown below: Figure 1 shown.

[0052] Among them, in the texturing process, in the texturing tank 10 (its structure is shown in FIG. Figure 2 ) is used to perform texturing on the silicon wafer 100, and the texturing tank 10 is filled with texturing liquid.

[0053] The texturing solution mainly includes an alkali metal hydroxide solution, a texturing additive and water. During the texturing treatment, the silicon wafer 100 is placed in the texturing solution in the texturing tank 10. The alkaline texturing solution has anisotropic corrosion properties on the silicon wafer 100 with different corrosion rates at different crystal orientations, forming a densely distributed "pyramid" structured anti-reflection velvet surface on the surface of the silicon wafer 100.

[0054] It can be understood that the silicon wafer 100 used is a crystalline silicon wafer, such as a single crystal silicon wafer; the texturing additive used can be a commercially available silicon wafer texturing additive.

[0055] In some embodiments, the texturing solution used in the texturing step comprises, by volume, 4.5 to 7 parts of a 40% to 50% alkali metal hydroxide solution, 1 part of a texturing additive, and 160 to 175 parts of water. Furthermore, the temperature of the texturing solution during the texturing step is 83°C to 86°C, and the texturing treatment time is controlled to be 450 to 700 seconds.

[0056] The inventors studied the texturing process and adjusted the composition and process parameters of the texturing solution. They found that when 4.5 to 7 parts of 40% to 50% by mass alkali metal hydroxide solution, 1 part of a texturing additive and 160 to 175 parts of water are used in the texturing solution; and the temperature of the texturing treatment is controlled at 83°C to 86°C, and the time of the texturing treatment is controlled at 450s to 700s, the reaction rate between the texturing solution and the silicon wafer 100 can be effectively improved, the difference in the texturing area on the surface of the silicon wafer 100 can be reduced, the uniformity of the texturing structure can be improved, and the blackening defect of the "water column mark" of the battery cell can be improved, thereby improving the efficiency, yield and production capacity of the product.

[0057] In some embodiments, the volume of the texturing tank 10 is 265L~275L; after each texturing treatment of 320~400 pieces (4 baskets) of silicon wafers 100, 5.5L~8L of texturing liquid in the texturing tank 10 is discharged, and 150mL~200mL of texturing additives, 6.5L~8.5L of water and 300mL~500mL of alkali metal hydroxide solution with a mass fraction of 40%~50% are added to the texturing tank 10.

[0058] The present invention further improves the size of the texturing tank 10, setting the volume of the texturing tank 10 to 265L~275L. Compared with the conventional method, the volume of the texturing tank 10 is larger, which increases the circulation space of the texturing solution, further improves the uniformity of the reaction between the texturing solution and the silicon wafer 100, and improves the uniformity of the velvet structure.

[0059] By discharging 5.5L to 8L of the texturing solution after texturing a certain amount of silicon wafers 100, and adding 150mL to 200mL of the texturing additive and 6.5L to 8.5L of water, the reaction activity of the texturing solution can be improved, and the regular discharge of sodium silicate and other impurities deposited at the bottom of the texturing tank 10 can be increased, thereby further improving the uniformity of the velvet surface structure.

[0060] In some embodiments, the circulating flow rate of the texturing solution during the texturing process is controlled to be 26L / min to 32L / min. This circulating flow rate is greater than that of traditional texturing processes, can reduce the residual solution on the surface of the silicon wafer 100, and can also improve the uniformity of the textured surface structure. By combining the above-mentioned optimization of the texturing solution composition, improvement of the volume of the texturing tank 10, and optimization of the texturing process parameters, the activity of the texturing solution can be effectively improved, the reaction efficiency and rate of the texturing process can be improved, the difference in the textured surface pyramids of the silicon wafer 100 can be reduced, and the blackening defect of the "water column mark" of the solar cell can be reduced.

[0061] It can be understood that the volume fraction of alkali metal hydroxide solution in the texturing solution can be but not limited to 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts; the alkali metal hydroxide can be one or more of sodium hydroxide, potassium hydroxide, etc.; the volume fraction of water in the texturing solution can be but not limited to 160 parts, 162 parts, 164 parts, 166 parts, 168 parts, 170 parts, 172 parts, 175 parts; the temperature of the texturing solution can be but not limited to 83°C, 84°C, 85°C, 86°C; the texturing treatment time can be but not limited to 450s, 480s, 500s, 530s, 560s, 600s, 650s, 680s, 700s; the volume of the texturing tank 10 can be but not limited to 265L, 267L, 269L, 271L, 273L, 275L; the texturing solution discharged from the texturing tank 10 each time can be but not limited to 5 .5L, 5.8L, 6.0L, 6.5L, 7.0L, 7.5L, 8L; the texturing additive added to the texturing tank 10 each time may be but not limited to 150mL, 160mL, 170mL, 180mL, 190mL, 200mL; the water added to the texturing tank 10 each time may be but not limited to 6.5L, 7.0L, 7.5L, 8.0L, 8.5L; the amount of alkali metal hydroxide solution added each time may be but not limited to 300mL, 320mL, 340mL, 360mL, 380mL, 400mL, 420mL, 440mL, 460mL, 480mL, 500mL; the circulation flow rate of the texturing solution may be but not limited to 26L / min, 27L / min, 28L / min, 29L / min, 30L / min, 31L / min, 32L / min.

[0062] The inventors further discovered that, in addition to factors such as the texturing solution, texturing process parameters, and the structural dimensions of the texturing tank 10, the structural arrangement of the flower basket 20 (the carrier used to load the silicon wafer 100) also affects the uniformity of the textured surface structure of the silicon wafer 100. In conventional texturing cleaning processes, due to the irrational design of the flower basket gear rods that load the silicon wafer 100, when the texturing solution circulates from the bottom of the tank upward to the silicon wafer 100, the bottom support rods 21 block too much of the silicon wafer 100. This results in inconsistent reaction rates between the blocked and unblocked areas of the silicon wafer 100 and the texturing solution, resulting in textured surface differences.

[0063] In this regard, in some embodiments of the present invention, during the texturing process, the silicon wafer 100 is placed on the bottom support rod 21 of the flower basket 20, the flower basket 20 is placed in the texturing solution, and the diameter of the bottom support rod 21 of the flower basket 20 is set to 14mm~16mm, and a plurality of through holes 23 are vertically opened on the bottom support rod 21, and the aperture of the through hole 23 is 2mm~4mm.

[0064] See also Figure 2 and Figure 3 The bottom of the texturing tank 10 is provided with a flow equalizer 11, which is provided with a plurality of liquid inlet holes 111. The bottom of the flower basket 20 is provided with a bottom support rod 21, and the upper side of the bottom support rod 21 is provided with a plurality of spaced flower basket teeth 22, and the bottom support rod 21 is provided with a plurality of through holes 23 vertically.

[0065] During the texturing process, the flower basket 20 loaded with silicon wafers is placed in the texturing tank 10, and the texturing tank 10 is placed in the texturing outer tank (not shown in the figure). The texturing liquid enters the texturing tank 10 from the liquid inlet 111 and then escapes to the texturing outer tank. This cycle is repeated to perform texturing on the silicon wafers.

[0066] During the texturing process, when the texturing solution circulates into the texturing tank 10, it circulates from the bottom of the tank 10 to the basket 20 holding the silicon wafer for a flushing reaction. According to the principles of fluid mechanics, because the bottom support rod 21 blocks the silicon wafer 100 to a certain extent, a considerable area of ​​stagnant liquid gap and Karman vortexes will appear behind the support rod, periodically generating two series of parallel counter-rotating vortices, which resonate with the silicon wafer 100, causing the silicon wafer 100 to constantly shake and stick, resulting in frequent friction. At the same time, the texturing solution cannot circulate in time, resulting in insufficient reaction of the silicon wafer 100. The larger the diameter of the bottom support rod 21, the more obvious this effect.

[0067] The present invention improves the size of the bottom support rod 21 of the flower basket 20, sets the diameter of the bottom support rod 21 to 14mm~16mm, and vertically opens a plurality of through holes 23 with an aperture of 2mm~4mm on the bottom support rod 21; the diameter of the bottom support rod 21 is smaller than that of the bottom support rod 21 of the traditional flower basket 20, which can enhance the circulation effect of the texturing solution; by setting the above-mentioned through holes 23 on the bottom support rod 21, the texturing solution can directly pass through the through holes 23 to reach the surface of the silicon wafer 100, thereby improving the Karman vortex caused by the bottom support rod 21, reducing the influence of insufficient local circulation of the texturing solution on the uniformity of the texture structure of the silicon wafer 100, and thus improving the poor "water column mark" of the battery cell.

[0068] Furthermore, the bottom support rod 21 of the flower basket 20 is preferably made of PVDF material with strong wear resistance and smooth surface, which can reduce the flow resistance of the texturing solution.

[0069] It can be understood that the diameter of the bottom support rod 21 can be but not limited to 14mm, 14.5mm, 15mm, 15.5mm, 16mm; the aperture of the through hole 23 can be but not limited to 2mm, 2.5mm, 3mm, 3.5mm, 4mm.

[0070] On the other hand, according to the inventor's research, in addition to the above-mentioned texturing solution composition, texturing tank 10 and flower basket 20 structure and texturing process parameters, the rough polishing step before the texturing step will also affect the uniformity of the texturing surface structure of the silicon wafer 100 after texturing.

[0071] Specifically, according to the experimental verification results, when the corrosion degree of the rough polishing solution used in the rough polishing treatment step is closer to the center of the silicon wafer 100, the purity of the silicon wafer 100 after rough polishing is higher, the hardness is higher, the effect of subsequent etching and texturing additives becomes weaker, the amount of corrosion of the surface of the silicon wafer 100 in the rough polishing tank increases, and the reaction rate in the texturing tank becomes slower. When the circulation is not timely during the texturing process, the texturing structure on the surface of the silicon wafer 100 will be relatively different.

[0072] Based on this, the present invention optimizes and adjusts the composition and process parameters of the rough polishing solution during the rough polishing process prior to the texturing process. Specifically, the silicon wafer 100 is subjected to rough polishing in a rough polishing tank containing a rough polishing solution comprising, by volume, 12 to 15 parts alkali metal hydroxide solution (40% to 50% by mass) and 220 to 250 parts water. The rough polishing process is performed for a controlled duration of 70 to 80 seconds.

[0073] Compared to the rough polishing step of the traditional texturing and cleaning process, the rough polishing solution used in the rough polishing step of the present invention has a lower content of alkali metal hydroxide, which can reduce the corrosion depth of the silicon wafer 100; the rough polishing time is extended compared to the traditional rough polishing time, which can improve the uniformity of corrosion on the silicon wafer 100 and improve the quality of the silicon wafer 100 after rough polishing. In this way, by adjusting the formula of the rough polishing solution and the rough polishing process in the rough polishing step, the rough polishing corrosion depth is reduced and the corrosion uniformity quality is improved, which is conducive to the use of a higher activity texturing solution to produce velvet and pyramids in the subsequent texturing step. By combining the above-mentioned rough polishing step with the texturing step, the uniformity of the velvet structure on the silicon wafer surface can be further improved, and the battery cell yield can be improved.

[0074] In some embodiments, the volume of the rough polishing tank used in the rough polishing step is 230L to 260L; after rough polishing 320 to 400 silicon wafers (4 baskets), 4L to 6L of the rough polishing solution is discharged from the rough polishing tank, and 1000mL to 1200mL of a 40% to 50% by mass alkali metal hydroxide solution and 5L to 6.5L of water are added to the rough polishing tank. Compared with the traditional rough polishing step, the rough polishing process of the present invention uses a lower amount of alkali metal hydroxide, a higher amount of water, and a higher amount of rough polishing solution for regular discharge. This increases the timed discharge of corrosive silicon impurities and other impurities deposited at the bottom of the rough polishing tank, reduces the amount of rough polishing corrosion, improves the corrosion uniformity, accelerates the reaction rate of the subsequent texturing process, reduces the difference in the texture surface, and improves the "water column mark" blackening of the cell.

[0075] It can be understood that the volume fraction of the alkali metal hydroxide solution in the rough polishing liquid can be but not limited to 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts, 15 parts; the volume fraction of water in the rough polishing liquid can be but not limited to 220 parts, 225 parts, 230 parts, 235 parts, 240 parts, 245 parts, 250 parts; the rough polishing treatment time can be but not limited to 70s, 72s, 74s, 76s, 78s, 80s; the rough polishing liquid discharged each time can be The amount of alkali metal hydroxide solution added to the rough throwing solution each time may be 1000mL, 1050mL, 1100mL, 1150mL, 1200mL; the amount of water added to the rough throwing solution each time may be 5L, 5.2L, 5.4L, 5.6L, 5.8L, 6.0L, 6.2L, 6.5L.

[0076] In some embodiments, after the silicon wafer 100 is rough-polished in the rough-polishing tank and before the silicon wafer 100 is textured in the textured tank, the silicon wafer texturing cleaning process further includes the following steps: ozone cleaning the rough-polished silicon wafer 100 using a solution containing hydrofluoric acid, hydrochloric acid, and ozone to remove organic matter and metallic impurities from the surface of the rough-polished silicon wafer 100; and pre-cleaning the ozone-cleaned silicon wafer 100 using a solution containing sodium hydroxide and hydrogen peroxide to further remove organic matter and dirt from the surface of the silicon wafer 100. The above-mentioned ozone cleaning and pre-cleaning steps are conducive to ensuring the effectiveness of the subsequent textured treatment.

[0077] In some embodiments, after the silicon wafer 100 is textured in the texture tank 10, the silicon wafer texture cleaning process further includes the following steps: post-cleaning the textured silicon wafer 100 with a solution containing sodium hydroxide and hydrogen peroxide to remove the textured liquid and metal impurities on the surface of the textured silicon wafer 100; smoothing the post-cleaned silicon wafer 100 with a solution containing hydrofluoric acid, hydrochloric acid and ozone to polish the pyramid texture structure after textured; passivating the smoothed silicon wafer 100 with a solution containing hydrofluoric acid to remove the oxide layer and the surface passivation layer on the surface of the silicon wafer 100; and sequentially washing, slowly pulling and dehydrating, and drying the passivated silicon wafer 100 to remove the liquid, dehydrate, and remove surface water droplets on the surface of the silicon wafer 100.

[0078] It should be noted that the ozone cleaning, pre-cleaning treatment, post-cleaning treatment, smoothing treatment, passivation treatment, water washing treatment, slow pulling dehydration treatment and drying treatment in the present invention can adopt conventional reagent ratios and process parameters, and are not specifically limited here.

[0079] Some embodiments of the present invention also provide a method for preparing a heterojunction solar cell, which includes the following steps: providing a silicon wafer, and using the above-mentioned silicon wafer texturing and cleaning process of the present invention to texturize and clean the silicon wafer 100; forming an intrinsic amorphous silicon layer on the silicon wafer 100 after texturizing and cleaning; forming an doped amorphous silicon layer on the intrinsic amorphous silicon layer; forming a transparent conductive film on the doped amorphous silicon layer; and forming an electrode on the transparent conductive film.

[0080] In one specific example, an n-type single crystal silicon wafer is used as a silicon wafer, and a pyramid textured structure is formed on the front and back sides of the n-type single crystal silicon wafer through the silicon wafer textured cleaning process of the present invention; then, an intrinsic amorphous silicon layer is formed on the front and back sides of the silicon wafer 100; a doped amorphous silicon layer is formed on the intrinsic amorphous silicon layer on the front and back sides, and the doping types of the two doped amorphous silicon layers are different; a transparent conductive film (usually an ITO film) is formed on the doped amorphous silicon layer on the front and back sides, respectively; and then, electrodes are prepared on the transparent conductive films on the front and back sides.

[0081] The heterojunction solar cell prepared by the above-mentioned preparation method has good uniformity of the silicon wafer texture structure due to the adoption of the above-mentioned silicon wafer texture making and cleaning process of the present invention, effectively improving the blackening defect of the "water column mark" of the cell. The heterojunction solar cell has a high product yield and high cell efficiency.

[0082] The present invention will be further described below with reference to specific examples and comparative examples, but they should not be construed as limiting the scope of protection of the present invention.

[0083] Example 1:

[0084] N-type monocrystalline silicon wafers were placed in a rough polishing tank filled with a rough polishing solution. The tank had a capacity of 235 L. The initial composition of the rough polishing solution, by volume, was 13 parts 45% sodium hydroxide solution and 225 parts water. The rough polishing time for each wafer was 75 seconds. After every 360 wafers, 4 L of the rough polishing solution was removed and 1000 mL of the sodium hydroxide solution and 5 L of water were added to the tank.

[0085] The silicon wafer 100 after the rough polishing treatment is placed in an ozone cleaning tank and subjected to ozone cleaning in a solution containing hydrofluoric acid, hydrochloric acid and ozone, and then placed in a pre-cleaning tank and subjected to pre-cleaning in a solution containing sodium hydroxide and hydrogen peroxide.

[0086] The silicon wafers 100 that have undergone pre-cleaning are placed in a texturing tank 10 and texturing treatment is carried out in a texturing solution. The texturing solution is calculated by volume as follows: 5 parts of 45% sodium hydroxide solution by mass, 1 part of a texturing additive, and 165 parts of water; the texturing temperature is 83°C, and the texturing time for each silicon wafer 100 is 600 seconds. The volume of the texturing tank 10 is 265L; after texturing 360 silicon wafers 100, 5.6L of the texturing solution is discharged, and 150mL of the texturing additive, 6.5L of water, and 300mL of the above-mentioned sodium hydroxide solution are added to the texturing tank 10. The texturing solution is circulated during the texturing process, and the circulation flow rate of the texturing solution is 26L / min. During the texturing process, the silicon wafers are placed on a flower basket 20. The diameter of the support rod 21 at the bottom of the flower basket 20 is 14mm, and a through hole 23 with a diameter of 2mm is vertically opened on the bottom support rod 21.

[0087] The silicon wafer 100 after the texturing treatment is placed in a post-cleaning tank and post-cleaned in a solution containing sodium hydroxide and hydrogen peroxide. It is then placed in a smoothing tank and smoothed in a solution containing hydrofluoric acid, hydrochloric acid, and ozone. It is then placed in a passivation tank and passivated in a solution containing hydrofluoric acid. The passivated silicon wafer 100 is then sequentially placed in a water washing tank, a slow pulling tank, and a drying tank for washing, slow pulling dehydration, and drying, respectively, to obtain a silicon wafer 100 with a textured surface.

[0088] An intrinsic amorphous silicon layer is deposited on the front and back sides of the obtained silicon wafer 100; a doped amorphous silicon layer is deposited on the intrinsic amorphous silicon layer on the front and back sides, respectively, and the doping types of the doped amorphous silicon layers on the front and back sides are different; a transparent conductive film is deposited on the doped amorphous silicon layer on the front and back sides; and electrodes are then prepared on the transparent conductive films on the front and back sides by screen printing or electroplating, thereby forming a heterojunction solar cell.

[0089] The prepared heterojunction solar cells were tested for their water column isolation ratio and cell efficiency. The testing method employed simulated sunlight exposure and the photoelectric induction principle of an IV tester, under standard conditions, to determine the presence of defects and power generation capacity. The test results are shown in Table 1.

[0090] Example 2:

[0091] N-type monocrystalline silicon wafers were placed in a rough polishing tank filled with a rough polishing solution. The tank had a capacity of 240 L. The initial composition of the rough polishing solution, by volume, was 14 parts 46% sodium hydroxide solution and 236 parts water. The rough polishing time for each wafer was 77 seconds. After every 360 wafers, 4.5 L of the rough polishing solution was removed and 1050 mL of the sodium hydroxide solution and 5.9 L of water were added to the tank.

[0092] The silicon wafer 100 after the rough polishing treatment is placed in an ozone cleaning tank and subjected to ozone cleaning in a solution containing hydrofluoric acid, hydrochloric acid and ozone, and then placed in a pre-cleaning tank and subjected to pre-cleaning in a solution containing sodium hydroxide and hydrogen peroxide.

[0093] The silicon wafers 100 that have undergone pre-cleaning treatment are placed in the texturing tank 10 and texturing treatment is carried out in the texturing solution. The texturing solution is calculated by volume as follows: 6.1 parts of 46% sodium hydroxide solution, 1 part of texturing additive, and 168 parts of water; the texturing treatment temperature is 84°C, and the texturing treatment time for each silicon wafer 100 is 650s. The volume of the texturing tank 10 is 269L; after each texturing treatment of 360 silicon wafers 100, 6.5L of texturing solution is discharged, and 170mL of texturing additive, 7.6L of water, and 400mL of the above-mentioned sodium hydroxide solution are added to the texturing tank 10. The texturing solution is circulated during the texturing treatment, and the circulation flow rate of the texturing solution is 29L / min. During the texturing process, the silicon wafer 100 is placed on a flower basket. The diameter of the bottom support rod 21 of the flower basket 20 is 14.5 mm, and a through hole 23 with a diameter of 2.5 mm is vertically opened on the bottom support rod 21.

[0094] The silicon wafer 100 after the texturing treatment is placed in a post-cleaning tank and post-cleaned in a solution containing sodium hydroxide and hydrogen peroxide. It is then placed in a smoothing tank and smoothed in a solution containing hydrofluoric acid, hydrochloric acid, and ozone. It is then placed in a passivation tank and passivated in a solution containing hydrofluoric acid. The passivated silicon wafer 100 is then sequentially placed in a water washing tank, a slow pulling tank, and a drying tank for washing, slow pulling dehydration, and drying, respectively, to obtain a silicon wafer 100 with a textured surface.

[0095] An intrinsic amorphous silicon layer is deposited on the front and back sides of the obtained silicon wafer 100; a doped amorphous silicon layer is deposited on the intrinsic amorphous silicon layer on the front and back sides, respectively, and the doping types of the doped amorphous silicon layers on the front and back sides are different; a transparent conductive film is deposited on the doped amorphous silicon layer on the front and back sides; and electrodes are then prepared on the transparent conductive films on the front and back sides by screen printing or electroplating, thereby forming a heterojunction solar cell.

[0096] The prepared heterojunction solar cells were tested for their water column isolation ratio and cell efficiency. The testing method was the same as in Example 1. The test results are shown in Table 1.

[0097] Example 3:

[0098] N-type monocrystalline silicon wafers were placed in a rough polishing tank filled with a rough polishing solution. The tank had a capacity of 258 L. The initial composition of the rough polishing solution, by volume, was 15 parts 46% sodium hydroxide solution and 246 parts water. The rough polishing time for each wafer was 80 seconds. After every 360 wafers, 6 L of the rough polishing solution was removed and 1200 mL of the sodium hydroxide solution and 6.5 L of water were added to the tank.

[0099] The silicon wafer 100 after the rough polishing treatment is placed in an ozone cleaning tank and subjected to ozone cleaning in a solution containing hydrofluoric acid, hydrochloric acid and ozone, and then placed in a pre-cleaning tank and subjected to pre-cleaning in a solution containing sodium hydroxide and hydrogen peroxide.

[0100] The pre-cleaned silicon wafer 100 is placed in the texturing tank 10 and texturing treated in a texturing solution. The texturing solution is calculated by volume as follows: 7 parts of 46% sodium hydroxide solution, 1 part of texturing additive, and 175 parts of water; the texturing temperature is 85°C, and the texturing time for each silicon wafer 100 is 690 seconds. The volume of the texturing tank 10 is 275L; after texturing 360 silicon wafers 100, 8L of texturing solution is discharged, and 200mL of texturing additive, 8.5L of water, and 500mL of the above sodium hydroxide solution are added to the texturing tank 10. The texturing solution is circulated during the texturing process, and the circulation flow rate of the texturing solution is 32L / min. During the texturing process, the silicon wafer 100 is placed on a flower basket 20. The diameter of the support rod 21 at the bottom of the flower basket 20 is 16mm, and a through hole 23 with a diameter of 4mm is vertically opened on the bottom support rod 21.

[0101] The silicon wafer 100 after the texturing treatment is placed in a post-cleaning tank and post-cleaned in a solution containing sodium hydroxide and hydrogen peroxide. It is then placed in a smoothing tank and smoothed in a solution containing hydrofluoric acid, hydrochloric acid, and ozone. It is then placed in a passivation tank and passivated in a solution containing hydrofluoric acid. The passivated silicon wafer 100 is then sequentially placed in a water washing tank, a slow pulling tank, and a drying tank for washing, slow pulling dehydration, and drying, respectively, to obtain a silicon wafer 100 with a textured surface.

[0102] An intrinsic amorphous silicon layer is deposited on the front and back sides of the obtained silicon wafer 100; a doped amorphous silicon layer is deposited on the intrinsic amorphous silicon layer on the front and back sides, respectively, and the doping types of the doped amorphous silicon layers on the front and back sides are different; a transparent conductive film is deposited on the doped amorphous silicon layer on the front and back sides; and electrodes are then prepared on the transparent conductive films on the front and back sides by screen printing or electroplating, thereby forming a heterojunction solar cell.

[0103] The prepared heterojunction solar cells were tested for their water column isolation ratio and cell efficiency. The testing method was the same as in Example 1. The test results are shown in Table 1.

[0104] Comparative Example 1:

[0105] N-type monocrystalline silicon wafers were placed in a rough polishing tank filled with a rough polishing solution. The tank had a capacity of 225 L. The initial composition of the rough polishing solution, by volume, was 20 parts by mass of 55% sodium hydroxide solution and 210 parts by mass of water. The rough polishing time for each wafer was 55 seconds. After every 360 wafers, 2 L of the rough polishing solution was removed and 1800 mL of the aforementioned sodium hydroxide solution and 3 L of water were added to the rough polishing tank.

[0106] The silicon wafer 100 after the rough polishing treatment is placed in an ozone cleaning tank and subjected to ozone cleaning in a solution containing hydrofluoric acid, hydrochloric acid and ozone, and then placed in a pre-cleaning tank and subjected to pre-cleaning in a solution containing sodium hydroxide and hydrogen peroxide.

[0107] The silicon wafer 100 that has undergone pre-cleaning is placed in the texturing tank 10 and texturing treatment is carried out in the texturing solution. The texturing solution is calculated by volume as follows: 8 parts of 55% sodium hydroxide solution by mass, 1 part of texturing additive, and 180 parts of water; the texturing temperature is 78°C, and the texturing time for each silicon wafer 100 is 750 seconds. The volume of the texturing tank 10 is 260L; after texturing 360 silicon wafers 100, 3L of texturing solution is discharged, and 130mL of texturing additive, 5L of water, and 300mL of the above sodium hydroxide solution are added to the texturing tank 10. The texturing solution is circulated during the texturing process, and the circulation flow rate of the texturing solution is 19L / min. During the texturing process, the silicon wafer 100 is placed on the flower basket 20. The diameter of the support rod 21 at the bottom of the flower basket 20 is 22mm, and there is no through hole 23 on the bottom support rod 21.

[0108] The silicon wafer 100 after the texturing treatment is placed in a post-cleaning tank and post-cleaned in a solution containing sodium hydroxide and hydrogen peroxide. It is then placed in a smoothing tank and smoothed in a solution containing hydrofluoric acid, hydrochloric acid, and ozone. It is then placed in a passivation tank and passivated in a solution containing hydrofluoric acid. The passivated silicon wafer 100 is then sequentially placed in a water washing tank, a slow pulling tank, and a drying tank for washing, slow pulling dehydration, and drying, respectively, to obtain a silicon wafer 100 with a textured surface.

[0109] An intrinsic amorphous silicon layer is deposited on the front and back sides of the obtained silicon wafer 100; a doped amorphous silicon layer is deposited on the intrinsic amorphous silicon layer on the front and back sides, respectively, and the doping types of the doped amorphous silicon layers on the front and back sides are different; a transparent conductive film is deposited on the doped amorphous silicon layer on the front and back sides; and electrodes are then prepared on the transparent conductive films on the front and back sides by screen printing or electroplating, thereby forming a heterojunction solar cell.

[0110] The prepared heterojunction solar cells were tested for their water column isolation ratio and cell efficiency. The testing method was the same as in Example 1. The test results are shown in Table 1.

[0111] Comparative Example 2:

[0112] N-type monocrystalline silicon wafers were placed in a rough polishing tank filled with a rough polishing solution. The tank had a capacity of 220 L. The initial composition of the rough polishing solution, by volume, was 21 parts 58% sodium hydroxide solution and 205 parts water. The rough polishing time for each wafer was 50 seconds. After every 360 wafers, 1 L of the rough polishing solution was removed and 1900 mL of the sodium hydroxide solution and 2 L of water were added to the tank.

[0113] The silicon wafer 100 after the rough polishing treatment is placed in an ozone cleaning tank and subjected to ozone cleaning in a solution containing hydrofluoric acid, hydrochloric acid and ozone, and then placed in a pre-cleaning tank and subjected to pre-cleaning in a solution containing sodium hydroxide and hydrogen peroxide.

[0114] The pre-cleaned silicon wafers 100 are placed in a texturing tank 10 and texturing treated in a texturing solution. The texturing solution consists of 8.5 parts by volume of a 58% sodium hydroxide solution, 1 part texturing additive, and 189 parts by volume of water. The texturing temperature is 77°C, and the texturing time for each silicon wafer 100 is 770 seconds. The volume of the texturing tank 10 is 254L. After texturing 360 silicon wafers 100, 3.5L of texturing solution is discharged, and 135mL of texturing additive, 5.5L of water, and 300mL of the aforementioned sodium hydroxide solution are added to the texturing tank 10. The texturing solution is circulated during the texturing process, with a circulation flow rate of 18L / min. During the texturing process, the silicon wafers 100 are placed on a flower basket 20. The diameter of the support rod 21 at the bottom of the flower basket 20 is 21mm, and no through-hole 23 is provided on the bottom support rod 21.

[0115] The silicon wafer 100 after the texturing treatment is placed in a post-cleaning tank and post-cleaned in a solution containing sodium hydroxide and hydrogen peroxide. It is then placed in a smoothing tank and smoothed in a solution containing hydrofluoric acid, hydrochloric acid, and ozone. It is then placed in a passivation tank and passivated in a solution containing hydrofluoric acid. The passivated silicon wafer 100 is then sequentially placed in a water washing tank, a slow pulling tank, and a drying tank for washing, slow pulling dehydration, and drying, respectively, to obtain a silicon wafer 100 with a textured surface.

[0116] An intrinsic amorphous silicon layer is deposited on the front and back sides of the obtained silicon wafer 100; a doped amorphous silicon layer is deposited on the intrinsic amorphous silicon layer on the front and back sides, respectively, and the doping types of the doped amorphous silicon layers on the front and back sides are different; a transparent conductive film is deposited on the doped amorphous silicon layer on the front and back sides; and electrodes are then prepared on the transparent conductive films on the front and back sides by screen printing or electroplating, thereby forming a heterojunction solar cell.

[0117] The prepared heterojunction solar cells were tested for their water column isolation ratio and cell efficiency. The testing method was the same as in Example 1. The test results are shown in Table 1.

[0118] Table 1 Yield and electrochemical performance of heterojunction solar cells of various embodiments and comparative examples

[0119] Water column mark isolation ratio (%) Battery efficiency (%) Example 1 0.02% 23.87% Example 2 0.03% 23.88% Example 3 0.01% 23.86% Comparative Example 1 3.34% 23.78% Comparative Example 2 3.01% 23.77%

[0120] As shown in Table 1, the heterojunction solar cells prepared in the embodiment of the present invention have a significantly lower proportion of water column mark defects on the production line compared to the control example, and the water column mark isolation ratio has dropped from approximately 3% in the control example to below 0.04%, significantly improving the yield. Testing the electrical performance of the cell shows that the efficiency of the cell in the embodiment of the present invention is approximately 0.09% higher than that of the control example. The main reason for the improved cell efficiency is that the velvet surface of the silicon wafer 100 in the embodiment of the present invention is more uniform, and the coating passivation deposition effect is better, thereby improving the cell efficiency.

[0121] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0122] The above-described embodiments merely represent several implementation methods of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art may make several modifications and improvements without departing from the concept of the present invention, and these modifications and improvements fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be based on the appended claims, and the description and drawings may be used to interpret the content of the claims.

Claims

1. A silicon wafer texturing and cleaning process, characterized in that: The steps include: The silicon wafer is subjected to texturing treatment using a texturing liquid; The texturing solution includes, by volume, 4.5 to 7 parts of alkali metal hydroxide solution with a mass fraction of 40% to 50%, 1 part of a texturing additive, and 160 to 175 parts of water; the texturing treatment temperature is 83° C. to 86° C., and the texturing treatment time is 450s to 700s; The texturing treatment is carried out in a texturing tank, the texturing solution is contained in the texturing tank, and the volume of the texturing tank is 265L-275L; after texturing 320-400 silicon wafers, 5.5L-8L of the texturing solution is discharged, and 150mL-200mL of the texturing additive, 6.5L-8.5L of water and 300mL-500mL of alkali metal hydroxide solution with a mass fraction of 40%-50% are added to the texturing tank; During the texturing process, the circulation flow rate of the texturing liquid is 26L / min to 32L / min.

2. The silicon wafer texturing and cleaning process according to claim 1, characterized in that: During the texturing treatment, the silicon wafer is placed on the bottom support rod of the flower basket, and the flower basket is placed in the texturing solution. The diameter of the bottom support rod is 14mm-16mm, and a through hole with a diameter of 2mm-4mm is vertically opened on the bottom support rod.

3. The silicon wafer texturing and cleaning process according to claim 1 or 2, characterized in that: Before the silicon wafer is subjected to texturing treatment using the texturing solution, the silicon wafer texturing cleaning process further includes the following steps: Performing rough polishing treatment on the silicon wafer using a rough polishing solution; The rough polishing solution comprises, by volume, 12 to 15 parts of alkali metal hydroxide solution with a mass fraction of 40% to 50% and 220 to 250 parts of water; the rough polishing treatment time is 70s to 80s.

4. The silicon wafer texturing and cleaning process according to claim 3, characterized in that: The rough polishing treatment is carried out in a rough polishing tank, which is filled with the rough polishing solution, and the volume of the rough polishing tank is 230L to 260L; after each rough polishing treatment of 320 to 400 silicon wafers, 4L to 6L of the rough polishing solution is discharged, and 1000mL to 1200mL of an alkali metal hydroxide solution with a mass fraction of 40% to 50% and 5L to 6.5L of water are added to the rough polishing tank.

5. The silicon wafer texturing and cleaning process according to claim 4, characterized in that: After the silicon wafer is subjected to rough polishing treatment with a rough polishing liquid and before the silicon wafer is subjected to texturing treatment with a texturing liquid, the silicon wafer texturing cleaning process further comprises the following steps: Using a solution containing hydrofluoric acid, hydrochloric acid and ozone to ozone clean the silicon wafer after the rough polishing treatment; and The silicon wafer after ozone cleaning is pre-cleaned with a solution containing sodium hydroxide and hydrogen peroxide.

6. The silicon wafer texturing and cleaning process according to claim 3, characterized in that: After the silicon wafer is subjected to texturing treatment using the texturing solution, the silicon wafer texturing cleaning process further comprises the following steps: Post-cleaning the silicon wafer after the texturing treatment using a solution containing sodium hydroxide and hydrogen peroxide; Using a solution containing hydrofluoric acid, hydrochloric acid and ozone to perform a rounding treatment on the silicon wafer after the post-cleaning treatment; Passivating the silicon wafer after the rounding treatment by using a solution containing hydrofluoric acid; as well as The silicon wafer after the passivation treatment is sequentially subjected to water washing treatment, slow pulling dehydration treatment and drying treatment.

7. A method for preparing a solar cell, characterized in that: The steps include: Providing a silicon wafer, and performing texturing and cleaning on the silicon wafer using the silicon wafer texturing and cleaning process according to any one of claims 1 to 6; and The silicon wafer after texturing and cleaning is made into a solar cell.

8. The method for preparing a solar cell according to claim 7, characterized in that: The silicon wafer after texturing and cleaning is made into a solar cell, comprising the following steps: forming an intrinsic amorphous silicon layer on the silicon wafer after texturing and cleaning; forming a doped amorphous silicon layer on the intrinsic amorphous silicon layer; forming a transparent conductive film on the doped amorphous silicon layer; and An electrode is formed on the transparent conductive film.

9. A solar cell, characterized in that: The solar cell is prepared by the preparation method described in claim 7 or 8.