A method for preparing zirconium oxychloride
By adding drying steps in the preparation process of zirconium oxychloride to convert silicate colloids and optimizing acid leaching and impurities, the difficulty of filtration of silica sol and the problem of water dilution are solved, the yield and process efficiency of zirconium oxychloride are improved, and the amount of hydrochloric acid is saved. Achieve efficient preparation of zirconium oxychloride.
Patent Information
- Application Number
- CN202210885040.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-26
AI Technical Summary
In the existing preparation method of zirconium oxychloride, silicate generates extremely difficult-to-filter silica sol in the acid leaching and decomposition step, resulting in loss of zirconium oxychloride and reducing yield. The product obtained after pickling and decomposition contains a large amount of water. Dilute the hydrochloric acid concentration, increase the process time and low equipment utilization rate.
After pickling and removing impurities, add heating and drying steps to convert silicate colloids into SiO2 to avoid the formation of silica sols, and use dry materials to perform acid leaching and decomposition, adjust the acidity of zirconium oxychloride solution to reduce hydrochloric acid consumption, and improve the reaction rate and yield , and at the same time, control the particle size of alkali melt decomposition and solid-liquid ratio of water washing and decompression, optimize the pH of the acid washing and decompression liquid, the acid leaching and decompression temperature and hydrochloric acid concentration.
Effectively improve the yield of zirconium oxychloride, save the amount of hydrochloric acid, reduce process time, improve equipment utilization, reduce the amount of mother liquor production, avoid the waste of uncrystallized zirconium oxychloride, and improve the decomposition efficiency and filtration effect.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing zirconium oxychloride, in particular to a method for preparing zirconium oxychloride. Background Art
[0002] Zirconium oxychloride (ZOCl2·8H2O) is a zirconium salt and the basic raw material of zirconium products. It is a white or slightly yellow needle-shaped crystal and the main raw material for manufacturing other zirconium products. It is widely used as an additive, catalyst and waterproofing agent for textiles, leather, rubber, refractory materials and ceramics, as well as a metal surface treatment agent.
[0003] The industrial method for preparing zirconium oxychloride from zircon includes the following steps: (1) alkali fusion decomposition: zircon is decomposed at high temperature using an alkaline decomposition agent containing sodium ions (such as sodium hydroxide or sodium carbonate) to produce sodium zirconate (Na2O3). 2 ZrO 3 ); (2) washing with water to remove impurities: washing with water to remove by-products generated in the reaction, such as sodium silicate and sodium oxide; (3) acid washing to remove impurities: washing the above sodium zirconate with dilute hydrochloric acid to remove the sodium in the sodium zirconate to obtain zirconium hydrate (ZrO(OH) 2 ·nH 2 O) solid; (4) acid leaching and impurity removal: dissolving the product of acid washing and impurity removal in hydrochloric acid, adding a flocculant, settling and filtering to obtain a zirconium oxychloride solution; (5) concentration and crystallization (first crystallization): evaporating the solution and cooling the precipitated zirconium oxychloride crystals; (6) secondary crystallization: dissolving the zirconium oxychloride crystals obtained in the first crystallization process in hydrochloric acid; adding concentrated hydrochloric acid to the solution to adjust the acidity; heating and concentrating; cooling to precipitate crystals.
[0004] The preparation method of the prior art has the following problems: silicate generates silica sol which is extremely difficult to filter in the acidic environment of the acid leaching and impurity removal step, and the silica colloid is difficult to settle, and zirconium oxychloride is wrapped in the colloid, resulting in zirconium oxychloride loss and reducing the yield of zirconium oxychloride. In addition, the product obtained after the acid washing and impurity removal is directly subjected to acid leaching and impurity removal, and the product obtained after the acid washing and impurity removal contains a large amount of water, which will dilute the concentration of hydrochloric acid during the acid leaching and impurity removal, which will increase the consumption of hydrochloric acid on the one hand; on the other hand, it will reduce the reaction rate, increase the process time, and low equipment utilization. Summary of the invention
[0005] Based on this, the present invention provides a method for preparing zirconium oxychloride, which can effectively improve the yield of zirconium oxychloride and effectively save the amount of hydrochloric acid used.
[0006] A method for preparing zirconium oxychloride comprises the following steps:
[0007] (1) alkali melting decomposition, water washing and acid washing to obtain zirconium hydrate solid;
[0008] (2) heating and drying the zirconium hydrate solid obtained in step (1); the heating and drying temperature is 100 to 250° C.;
[0009] (3) subjecting the dried zirconium hydrate obtained in step (2) to acid leaching and impurity removal to obtain a zirconium oxychloride solution;
[0010] (4) Using concentrated hydrochloric acid to adjust the acidity of the zirconium oxychloride solution obtained in step (3), cooling, crystallizing, washing, and dehydrating to obtain zirconium oxychloride.
[0011] The preparation method of zirconium oxychloride of the present invention adds a heating and drying step after the pickling and impurity removal step. If the drying temperature is too high, oxidation will occur to form oxides. If the temperature is too low, dehydration will be incomplete and the drying time will be long. During drying, the silicate colloid generated in the pickling and impurity removal step is converted into SiO 2 , in the subsequent acid leaching and impurity removal (SiO 2 The zirconium oxychloride (ZrOCl) is a solid substance that is easy to filter) and is directly removed by sedimentation to avoid the formation of silica sol; on the other hand, when the dried product is subjected to acid leaching and impurity removal, the concentration of the crystallized zirconium in the solution is increased, and the acidity of the solution will not be diluted, which can save the amount of concentrated hydrochloric acid used in the crystallization process, and at the same time can increase the reaction rate, reduce the process time consumption, and improve the equipment utilization efficiency. In addition, the use of concentrated hydrochloric acid to adjust the acidity of zirconium oxychloride eliminates the concentration process, saves the energy consumption of the concentration process, and uses dry materials for acid leaching and impurity removal to obtain a high-concentration zirconium oxychloride solution, which can effectively reduce the amount of mother liquor produced, avoid the waste of uncrystallized zirconium oxychloride in the mother liquor, further improve the yield, and at the same time can reduce the amount of concentrated hydrochloric acid used to adjust the acidity.
[0012] Furthermore, the particle size of the zircon sand decomposed by alkali melting in step (1) is less than 100 microns. The smaller the particle size of the zircon sand, the higher its specific surface area and the higher its reactivity. Controlling the particle size of the zircon sand can effectively improve its decomposition efficiency.
[0013] Furthermore, in step (1), the water washing and impurity removal adopts countercurrent washing, and the water-solid-liquid ratio of washing is controlled to be 1:(1-10). By adopting countercurrent washing, a smaller amount of washing liquid can be used to achieve a more satisfactory washing effect. A too high water-solid-liquid ratio produces a large amount of waste liquid; a too low water-solid-liquid ratio has a low washing effect and incomplete washing.
[0014] Furthermore, in the pickling and impurity removal step in step (1), the pH of the feed solution is controlled at 1.0 to 3.0. The purpose of pickling and impurity removal is to remove sodium and impurities such as calcium, magnesium, aluminum, iron, titanium, and silicon in sodium zirconate. The solid compound obtained is zirconium hydrate (ZrO(OH) 2 ·nH 2O), the zirconium hydrate will be accelerated to dissolve when the pH is less than 1, reducing the yield, so the pH of the feed solution is controlled to be not less than 1. When the pH is greater than 3, sodium and other impurities cannot be effectively removed.
[0015] Furthermore, the heating and drying temperature in step (2) is 100-250° C. If the drying temperature is too high, oxidation will occur to form oxides, and if the temperature is too low, dehydration will be incomplete and the drying time will be long.
[0016] Furthermore, the acid leaching and impurity removal in step (3) includes heating and dissolving the dried zirconium hydrate obtained in step (2) with 4.0-7.0 mol / L hydrochloric acid, adding a flocculant, settling, and filtering while hot. If the hydrochloric acid concentration is too low, the reaction rate is low, the dissolution time is too long, and the acidity of the obtained solution is too low, and a large amount of hydrochloric acid is required to adjust the acidity of the subsequent crystallization; if the hydrochloric acid concentration is too high, it is difficult to control the viscosity of the zirconium oxychloride, which affects the subsequent filtration process.
[0017] Furthermore, the temperature of the heating and dissolving is 60-80° C. A lower temperature can effectively reduce the solubility of the silicate compound in the solution, but zirconium oxychloride in the solution will also precipitate at too low a temperature, so controlling the temperature at 60-80° C. can achieve the best impurity removal effect.
[0018] Furthermore, the flocculant is one of polymethacrylate, polyamine, polyacrylamide, polyethylene oxide, polyvinyl alcohol and gelatin.
[0019] Furthermore, the mass concentration of concentrated hydrochloric acid in step (4) is 30-35%. If the concentration of hydrochloric acid is too low, the ability to adjust the acidity is limited.
[0020] Furthermore, in step (4), 5.0-7.5 mol / L hydrochloric acid is used for washing, and the washing temperature is ≤30°C. If the acidity of the washing acid is too high, it will affect the operating environment of personnel and is not conducive to the control of production costs. If the acidity of the washing acid is too low, the solubility of zirconium is high and the yield is difficult to guarantee. If the temperature is too high, the product will dissolve too much during washing, reducing the yield.
[0021] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing zirconium oxychloride, comprising the following steps:
[0023] (1) Alkaline melting decomposition, water washing and acid washing to obtain zirconium hydrate solid.
[0024] (2) heating and drying the zirconium hydrate solid obtained in step (1).
[0025] (3) The dried zirconium hydrate obtained in step (2) is subjected to acid leaching to remove impurities, thereby obtaining a zirconium oxychloride solution.
[0026] (4) Using concentrated hydrochloric acid to adjust the acidity of the zirconium oxychloride solution obtained in step (3), cooling and crystallizing, solid-liquid separation, washing and drying to obtain zirconium oxychloride.
[0027] Preferably, the alkali fusion decomposition in step (1) is as follows: zircon sand: caustic soda flakes = 1: 1.30-1.60 is put into an alkali fusion furnace for alkali fusion to generate sodium zirconate, the reaction temperature is controlled at 550-650°C, the reaction time is controlled at 10-30 minutes, and the low temperature insulation time is controlled at 12-24 hours. The particle size of the zircon sand is less than 100 microns.
[0028] Preferably, the water washing and impurity removal in step (1) adopts countercurrent washing to remove excess alkali, sodium silicate and other soluble impurities, controls the water washing solid-liquid ratio to 1:1-10, washes 3-5 times, and uses a diaphragm filter press to perform solid-liquid separation.
[0029] Preferably, the acid washing and impurity removal in step (1) is: adding dilute hydrochloric acid to the solid product obtained by water washing and impurity removal, controlling the pH of the liquid to be 1.0-3.0, heating to 80-90°C, stirring and washing, filtering and separating, to obtain zirconium hydrate solid.
[0030] Preferably, the drying temperature in step (2) is 100-250°C; on the one hand, the silica colloid generated in the pickling and impurity removal is converted into SiO 2 , so that it can be removed in the next step of acid leaching to remove impurities; on the other hand, the dry zirconium hydrate will not dilute the hydrochloric acid used for dissolution, which can increase the reaction rate and save the consumption of hydrochloric acid.
[0031] Preferably, the acidic impurity removal in step (3) is to react the dried product with a 4.0-7.0 mol / L hydrochloric acid solution, control the zirconium concentration to 100.0-250.0 g / L, and react at a temperature of 60-80° C. to generate a zirconium oxychloride solution, add a flocculant, settle, and filter while hot.
[0032] Preferably, the flocculant in step (3) is selected from the group consisting of polymethacrylate, polyamine, polyacrylamide, polyethylene oxide, polyvinyl alcohol and gelatin.
[0033] Preferably, the concentration of concentrated hydrochloric acid in step (3) is 30-35% (mass concentration), and the acidity of the feed solution is controlled at 4.5-6.5 mol / L.
[0034] Preferably, in step (3), 5.5-7.5 mol / L hydrochloric acid is used for washing, and the washing temperature is ≤30°C.
[0035] Example 1
[0036] Weigh 800.0 g of zircon sand (zirconium and hafnium content ≥ 65.50%; particle size requirement: all pass through a 150-mesh standard sieve), add 1200.0 g of 99% sodium hydroxide, react in a 650° C. high-temperature furnace for 30 minutes, and take out the reactor and cool to room temperature.
[0037] The product was counter-current washed three times with 6500 ml of hot water at 80°C. The alkali concentration in the filtrate was ≤0.30 mol / L. The solid-liquid separation was performed with a diaphragm filter press.
[0038] The filter cake was taken out and 6500 ml of hot water at 80°C was added for pulping. A 2.0 mol / L hydrochloric acid solution was added to adjust the pH of the liquid to 2.0. The pickling liquid was separated by suction filtration. The operation was repeated 3 times to obtain the filter cake after pickling.
[0039] Example 2
[0040] 200 g of the acid-washed filter cake obtained in Example 1 was placed in a 150° C. forced air drying oven and dried for 4.0 hours to obtain 114 g of dried filter cake. The zirconium content of the dried filter cake was determined to be 60.05%.
[0041] Add 400mL of 7.0mol / L hydrochloric acid solution, heat to 80℃, stir to dissolve, acid soak for 30 minutes, then add flocculant - gelatin, stir evenly and keep warm for 40 minutes, filter while hot to obtain zirconium oxychloride solution.
[0042] Slowly add 30% concentrated hydrochloric acid solution to adjust the acidity of zirconium oxychloride solution. When the acidity of the solution reaches 5.5 mol / L, stop adding acid. After the solution temperature drops to room temperature, filter and separate the crystalline zirconium oxychloride. Add 6.0 mol / L hydrochloric acid solution to wash for 30 minutes, and filter and separate the washing liquid. Repeat the washing for 3 times to obtain 125 g of zirconium oxychloride crystals. The impurity content in zirconium oxychloride was analyzed by ICP: ZrO 2 :35.15%;SiO 2 :0.0008%;Fe 2 O 3 :0.0005%; TiO 2 :0.0005%; NaO 2 :0.0005%.
[0043] Comparative Example 1
[0044] Take 200g of the acid-washed filter cake obtained in Example 1, add 480ml of 7.0mol / L hydrochloric acid solution, heat to 80°C, stir to dissolve, acid soak for 30 minutes, then add flocculant - gelatin, stir evenly and keep warm for 40 minutes, and filter while hot to obtain zirconium oxychloride solution.
[0045] Slowly add 30% concentrated hydrochloric acid solution to adjust the acidity of zirconium oxychloride solution. When the acidity of the solution reaches 5.5 mol / L, stop adding acid. After the solution temperature drops to room temperature, filter and separate the crystalline zirconium oxychloride. Add 6.0 mol / L hydrochloric acid solution to the crystalline zirconium oxychloride and wash for 30 minutes. Filter and separate the washing liquid. Repeat the washing for 3 times to obtain 90 g of zirconium oxychloride crystals. The impurity content in zirconium oxychloride was analyzed by ICP: ZrO 2 :34.88%;SiO 2 :0.0015%;Fe 2 O 3 :0.0005%;TiO 2 :0.0005%; NaO 2 :0.0005%.
[0046] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.
Claims
1. A method for preparing zirconium oxychloride, characterized in that: The following steps are involved: (1) alkali melting decomposition, water washing and acid washing to obtain zirconium hydrate solid; (2) heating and drying the zirconium hydrate solid obtained in step (1); (3) subjecting the dried zirconium hydrate obtained in step (2) to acid leaching and impurity removal to obtain a zirconium oxychloride solution; (4) using concentrated hydrochloric acid to adjust the acidity of the zirconium oxychloride solution obtained in step (3), cooling, crystallizing, washing, and drying to obtain zirconium oxychloride; The alkali melting decomposition in step (1) comprises: putting zircon sand into an alkali melting furnace for alkali melting according to a reaction ratio of zircon sand: caustic soda flakes = 1: (1.30-1.60) to generate sodium zirconate, controlling the reaction temperature to 550-650° C.; controlling the reaction time to 10-30 minutes, and the low-temperature insulation time to 12-24 hours; wherein the particle size of the zircon sand is less than 100 microns; the water washing and impurity removal in step (1) adopts countercurrent washing, and the water washing solid-liquid ratio is controlled to 1: (1-10); the acid washing and impurity removal in step (1) comprises: adding dilute hydrochloric acid to the solid product obtained by water washing and impurity removal, controlling the pH of the feed liquid to be 1.0-3.0, heating to 80-90° C., stirring and washing, filtering and separating, and obtaining zirconium hydrate solid; The heating and drying temperature in step (2) is 100 to 250° C.; The acid leaching and impurity removal in step (3) is to react the dried product with a 4.0-7.0 mol / L hydrochloric acid solution, control the zirconium concentration to 100.0-250.0 g / L; the reaction temperature is 60-80° C., and the reaction generates a zirconium oxychloride solution; add a flocculant, settle, and filter while hot; The mass concentration of concentrated hydrochloric acid in step (4) is 30-35%; the acidity of the feed solution is controlled at 4.5-6.5 mol / L; 5.0-7.5 mol / L hydrochloric acid is used for washing in step (4), and the washing temperature is ≤30°C.
2. The method for preparing zirconium oxychloride according to claim 1, characterized in that: The flocculant is one of polymethacrylate, polyamine, polyacrylamide, polyethylene oxide, polyvinyl alcohol and gelatin.