A monodisperse Mo / Co3O4 nanozyme and its preparation method and application

The monodispersed Mo/Co3O4 nanoenzyme prepared by low-temperature calcination under air atmosphere maintains the dodecahedral structure of ZIF-67, and solves the problem of reducing nanoenzyme activity caused by high-temperature calcination in the prior art, achieving rapid sulfite Visual detection has high sensitivity and selectivity to meet the needs of sulfite detection in food.

CN115326735BActive Publication Date: 2024-11-12TEA RESEARCH INSTITUTE CHINESE ACADEMY OF AGRICULTURAL SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210496589.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-09
Publication Date
2024-11-12
Estimated Expiration
2042-05-09

AI Technical Summary

Technical Problem

The prior art is difficult to quickly, visually and highly sensitively detect the content of sulfite in alternative tea drinks, especially due to high-temperature roasting, which causes the collapse of MOF structure, forming amorphous nitrogen-doped carbon material, affecting the catalytic activity and detection efficiency of nanoenzymes. .

Method used

Using ZIF-67 as the carrier and sodium molybdate dihydrate as the molybdenum source, monodispersed Mo/Co3O4 nanoenzyme was prepared under air atmosphere by low temperature calcination conditions to maintain the dodecahedral structure of ZIF-67 and improve the oxidase-like activity. And rapid visual analysis of sulfite is achieved through ultraviolet visible spectrum and naked eye observation.

Benefits of technology

A monodispersed Mo/Co3O4 nanoenzyme prepared by low-temperature calcination under air atmosphere has high oxidase activity and stability, can quickly and visually detect sulfites, have high sensitivity and selectivity, and meet sulfite acid in food. Salt testing requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115326735B_ABST
    Figure CN115326735B_ABST
Patent Text Reader

Abstract

A monodisperse Mo / Co3O4 nanozyme and its preparation method and application belong to the technical field of new nanomaterials. The present invention uses the metal organic framework ZIF-67 as a carrier, loads Mo by stirring at room temperature, and prepares a monodisperse Mo / Co3O4 nanomaterial by low temperature calcination under an air atmosphere. The nanozyme prepared by the method maintains the dodecahedral structure of ZIF-67, is conducive to the transmission of substances, and can further improve its enzyme-like catalytic activity. In the absence of H2O2, it has high oxidase-like activity and good stability. The present invention provides a sulfite colorimetric detection method based on monodisperse Mo / Co3O4 nanozymes, which can realize the visual detection of sulfite content in substitute tea drinks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of novel nanomaterials and specifically relates to a monodispersed Mo / Co 3 O 4 Nanozyme and its preparation method and application. Background Art

[0002] Sulfite has bleaching, antioxidant, and antibacterial effects. As a food additive, it is widely added to foods such as dried fruits, biscuits, and beer. my country's industry standard GH / T 1091-2014 stipulates that the maximum residual limit of sulfite shall not exceed 100 mg kg -1 . Therefore, it is necessary to monitor the content of sulfite in substitute tea. The national food safety standard GB5009.34-2016 "Determination of sulfur dioxide in food" stipulates that the detection method of sulfur dioxide in food is iodine titration. This method is low-cost and only requires glassware, but it is time-consuming and has low sensitivity. In recent years, a high-performance liquid chromatography-tandem mass spectrometry analysis method has been established based on the principle of sulfite and formaldehyde deriving a relatively stable compound-sodium hydroxymethane sulfonate. However, large-scale instruments and equipment are expensive and require experienced operators, which makes it difficult to meet the needs of rapid screening of sulfite content in foods such as substitute tea drinks. Therefore, it is urgent to develop an on-site, visual, and highly sensitive detection method for sulfites in substitute tea drinks.

[0003] In recent years, nanomaterials with enzyme-like activity are called nanozymes, and their preparation and application have attracted widespread attention and research. Compared with natural enzymes, nanozymes show better stability at different temperatures or pH. At the same time, they have the characteristics of simple preparation and low cost. They have good application prospects in the construction of biosensors, detection of environmental pollutants and analysis of food pollutants. Due to the unique size effect and high catalytic activity of monodisperse nanozymes, monodisperse nanozyme sensors have emerged in rapid visual detection. Metal organic framework (MOFs) materials, as a new type of porous materials, have the characteristics of high specific surface area and porosity, and are ideal precursor materials for the preparation of monodisperse nanozyme materials. Invention patent CN 110887795 A discloses a method for preparing molybdenum single-atom nanozyme materials, using MOF materials (ZIF-8) as carriers and molybdenum acetylacetonate as molybdenum source, and synthesizing nanomaterials with molybdenum single atoms loaded on nitrogen-doped carbon substrates by room temperature stirring and high temperature calcination. However, the material is calcined under nitrogen protection, and the temperature is as high as 700-900℃. During the high-temperature calcination process, the MOF structure collapses and forms an amorphous nitrogen-doped carbon material.

[0004] The present invention uses ZIF-67 as a carrier and sodium molybdate dihydrate as a molybdenum source, and prepares monodispersed Mo / Co by calcining at a relatively low temperature in an air atmosphere.3 O 4 Nanozyme. The nanozyme prepared by this method maintains the dodecahedral structure of ZIF-67, which is conducive to the transport of substances and can further improve its enzyme-like catalytic activity. 2 O 2 Under the conditions, it has high oxidase activity and good stability. 3 O 4 The material can be used as an efficient oxidase-like enzyme for rapid and visual detection of sulfite and has great practical application value. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a monodispersed Mo / Co 3 O 4 Nanozyme preparation method and application technical solution. 3 O 4 Nanozymes have high oxidase-like activity and can catalyze the oxidation of 3,3',5,5'-tetramethylbenzidine (TMB) molecules from colorless to blue. Sulfite can inhibit the occurrence of this reaction, and there is a linear relationship between its concentration and absorbance. Through UV-visible spectroscopy and naked eye observation, rapid and visual analysis of sulfite can be achieved, which has great practical application value.

[0006] The present invention is specifically implemented by the following technical solutions:

[0007] On the one hand, the present invention provides a monodispersed Mo / Co 3 O 4 A method for preparing a nanozyme, comprising the following steps:

[0008] (1) Dissolve 2-methylimidazole and cobalt nitrate hexahydrate in methanol, stir vigorously, let stand at room temperature, centrifuge, wash, and dry to obtain the metal organic framework ZIF-67;

[0009] (2) adding the ZIF-67 obtained in step (1) into ethanol and dispersing by ultrasonication to obtain a ZIF-67 dispersion solution;

[0010] (3) dissolving sodium molybdate dihydrate in deionized water, mixing with the ZIF-67 dispersion solution obtained in step (2), heating to reflux, centrifuging, drying, and calcining in air to obtain a monodispersed Mo / Co 3 O 4 Nanozymes.

[0011] Furthermore, in the step (1), the molar mass ratio of 2-methylimidazole to cobalt nitrate hexahydrate is 1:1 to 5:1, and the standing time at room temperature is 24 hours.

[0012] Furthermore, in step (2), the ultrasonic time is 5 to 30 minutes and the ultrasonic power is 50W.

[0013] Furthermore, in step (3), the mass ratio of ZIF-67 to sodium molybdate dihydrate is 1:0.01 to 1:5, the heating reflux temperature is 80°C, the heating reflux time is 2h, the roasting temperature is 200°C to 400°C, and the roasting time is 1h to 3h.

[0014] Another aspect of the present invention provides a monodispersed Mo / Co prepared by any of the above preparation methods. 3 O 4 Nanozymes.

[0015] Another aspect of the present invention provides a monodispersed Mo / Co 3 O 4 Application of nanozymes in visual detection of sulfite.

[0016] Another aspect of the present invention provides a monodispersed Mo / Co 3 O 4 The method for applying nanozymes in visual detection of sulfite comprises the following steps:

[0017] (1) Add boiling water to the crushed substitute tea to brew for extraction, and pass through a membrane to obtain a supernatant;

[0018] (2) Weigh monodispersed Mo / Co 3 O 4 Nanozyme was added with deionized water and ultrasonically dispersed to obtain nanozyme stock solution, which was stored at 4°C for later use;

[0019] (3) adding the nanozyme stock solution, the supernatant obtained in step (1), and 3,3',5,5'-tetramethylbenzidine to the acetic acid-sodium acetate buffer solution in sequence;

[0020] (4) React at room temperature or 37°C, let stand for 20 min, and then analyze using a UV spectrophotometer. Calculate the sulfite content based on the change in the absorption peak intensity at 652 nm.

[0021] Furthermore, in step (2), the monodispersed Mo / Co 3 O 4 The concentration of the nanozyme stock solution was 1 mg / mL -1 .

[0022] Furthermore, in step (3), the pH of the acetic acid-sodium acetate buffer solution is 3.5, and the monodispersed Mo / Co 3 O 4 The volume of nanozyme added is 1 to 10 uL.

[0023] Furthermore, in step (4), the reaction time at room temperature or 37° C. is 10 min.

[0024] The beneficial effects of the present invention are:

[0025] The present invention prepares monodispersed Mo / Co by calcining at a relatively low temperature under air atmosphere. 3 O 4 Nanozymes. The prepared nanozymes have highly dispersed Mo atoms, maintain the porous structure of ZIF-67 dodecahedron, are conducive to the transport of substances, and have high oxidase-like activity. Sulfite can inhibit Mo / Co 3 O 4 The oxidase activity of nanozymes has established an on-site, visual detection method for sulfite, which has the advantages of high sensitivity, good selectivity, simplicity, and rapid visualization. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 :Monodispersed Mo / Co 3 O 4 XRD pattern of nanozyme.

[0027] Figure 2 :Monodispersed Mo / Co 3 O 4 TEM image of nanozyme.

[0028] Figure 3 :Monodispersed Mo / Co 3 O 4 Diagram of the oxidase-like activity of nanozymes.

[0029] Figure 4 :Monodispersed Mo / Co 3 O 4 Diagram of the properties of nanozymes for detecting sulfite. DETAILED DESCRIPTION

[0030] In order to better understand the present invention, a monodispersed Mo / Co 3 O 4 The preparation method and application of nanozymes are further described below through examples, but the application of the present invention is not limited to the following specific examples.

[0031] Example 1: Monodisperse Mo / Co 3 O 4 Preparation of nanozymes

[0032] 2-Methylimidazole and Co(NO) in a molar mass ratio of 1:1 3 ) 2 6H 2O were dissolved in 50 mL of methanol, stirred vigorously for 10 min, and then allowed to stand at room temperature for 24 h. After centrifugation at 10000 rpm and washing several times, the purple solid powder was collected and dried at 60 °C to obtain ZIF-67.

[0033] 1 g ZIF-67 was dissolved in 40 mL ethanol and ultrasonically dispersed for 5 min to obtain a ZIF-67 dispersion solution.

[0034] 0.01 g of Na 2 MoO 4 ·2H 2 O was dissolved in 20 mL of deionized water, and Na 2 MoO 4 The solution was mixed with ZIF-67 solution and refluxed at 80℃ for 2 h under magnetic stirring. After centrifugation, washing and drying, it was further calcined in air at 200℃ for 2 h to obtain monodispersed Mo / Co 3 O 4 Nanomaterials.

[0035] Example 2: Monodisperse Mo / Co 3 O 4 Preparation of nanozymes

[0036] 2-Methylimidazole and Co(NO) in a molar mass ratio of 3:1 3 ) 2 6H 2 O were dissolved in 50 mL of methanol, stirred vigorously for 10 min, and then allowed to stand at room temperature for 24 h. After centrifugation at 10000 rpm and washing several times, the purple solid powder was collected and dried at 60 °C to obtain ZIF-67.

[0037] 1 g ZIF-67 was dissolved in 40 mL ethanol and ultrasonically dispersed for 5 min to obtain a ZIF-67 dispersion solution.

[0038] 0.5 g of Na 2 MoO 4 ·2H 2 O was dissolved in 20 mL of deionized water, and Na 2 MoO 4 The solution was mixed with the ZIF-67 solution and refluxed at 80°C for 2 h under magnetic stirring. After centrifugation, washing, and drying, it was further calcined in air at 300°C for 3 h to obtain monodispersed Mo / Co 3 O 4 Nanomaterials.

[0039] Example 3: Monodisperse Mo / Co 3 O 4 Preparation of nanozymes

[0040] 2-Methylimidazole and Co(NO 3 ) 2 6H 2 O were dissolved in 50 mL of methanol, stirred vigorously for 10 min, and then allowed to stand at room temperature for 24 h. After centrifugation at 10000 rpm and washing several times, the purple solid powder was collected and dried at 60 °C to obtain ZIF-67.

[0041] 1 g ZIF-67 was dissolved in 40 mL ethanol and ultrasonically dispersed for 5 min to obtain a ZIF-67 dispersion solution.

[0042] 0.5 g of Na 2 MoO 4 ·2H 2 O was dissolved in 20 mL of deionized water, and Na 2 MoO 4 The solution was mixed with ZIF-67 solution and refluxed at 80℃ for 2 h under magnetic stirring. After centrifugation, washing and drying, it was further calcined in air at 250℃ for 2 h to obtain monodispersed Mo / Co 3 O 4 Nanomaterials.

[0043] Example 4: Monodisperse Mo / Co 3 O 4 Preparation of nanozymes

[0044] 2-Methylimidazole and Co(NO) in a molar mass ratio of 5:1 were added 3 ) 2 6H 2 O were dissolved in 50 mL of methanol, stirred vigorously for 10 min, and then allowed to stand at room temperature for 24 h. After centrifugation at 10000 rpm and washing several times, the purple solid powder was collected and dried at 60 °C to obtain ZIF-67.

[0045] 1 g ZIF-67 was dissolved in 40 mL ethanol and ultrasonically dispersed for 5 min to obtain a ZIF-67 dispersion solution.

[0046] 2.5 g of Na 2 MoO 4 ·2H 2 O was dissolved in 20 mL of deionized water, and Na 2 MoO 4 The solution was mixed with the ZIF-67 solution and refluxed at 80 °C for 2 h under magnetic stirring. After centrifugation, washing, and drying, it was further calcined in air at 300 °C for 3 h to obtain monodispersed Mo / Co 3 O 4 Nanomaterials.

[0047] Example 5: Monodisperse Mo / Co 3 O 4 Preparation of nanozymes

[0048] 2-Methylimidazole and Co(NO) in a molar mass ratio of 5:1 were added 3 ) 2 6H 2 O were dissolved in 50 mL of methanol, stirred vigorously for 10 min, and then allowed to stand at room temperature for 24 h. After centrifugation at 10000 rpm and washing several times, the purple solid powder was collected and dried at 60 °C to obtain ZIF-67.

[0049] 1 g ZIF-67 was dissolved in 40 mL ethanol and ultrasonically dispersed for 5 min to obtain a ZIF-67 dispersion solution. 2 MoO 4 ·2H 2 O was dissolved in 20 mL of deionized water, and Na 2 MoO 4 The solution was mixed with the ZIF-67 solution and refluxed at 80 °C for 2 h under magnetic stirring. After centrifugation, washing, and drying, it was further calcined in air at 400 °C for 1 h to obtain monodispersed Mo / Co 3 O 4 Nanomaterials.

[0050] Figure 1 The monodispersed Mo / Co prepared in Example 1-5 3 O 4 XRD spectrum of nanozyme. Compared with the narrow and sharp XRD diffraction peaks of the precursor ZIF-67 ( Figure 1 a) Compared with monodispersed Mo / Co 3 O 4 The diffraction peak intensity of nanomaterials becomes weaker and broader ( Figure 1 b), indicating that when Mo is doped, the crystallinity decreases, causing more defects, which is conducive to the exposure of active centers and improves catalytic activity. At the same time, no characteristic peaks of Mo are found in the XRD spectrum, only Co 3 O 4 19.0 o , 31.2 o , 36.9 o , 38.5 o , 44.8 o , 55.7 o , 59.3 o and 65.2 oThe characteristic peaks correspond to the (111), (220), (311), (222), (400), (422), (511) and (400) crystal planes (PDF: 42-1467), indicating that Mo is in a monodisperse state and is evenly dispersed on the ZIF-67 support. When the mass ratio of ZIF-67 to sodium molybdate dihydrate is 1:0.01 to 1:5, Mo can be monodispersed on the ZIF-67 support. At the same time, the calcination temperature is 200 o C~400 o C can obtain monodispersed Mo / Co 3 O 4 Materials, different pyrolysis temperatures will not cause Mo to agglomerate to form MoO 3 .

[0051] Figure 2 For Example 3 monodispersed Mo / Co 3 O 4 TEM image of monodispersed Mo / Co 3 O 4 The morphology and size are uniform, maintaining the dodecahedral cubic porous structure of the precursor ZIF-67, which is conducive to the transmission of substances. Compared with the original size, it is slightly reduced to about 600nm. There is a certain degree of shrinkage inside the MOF, with a hollow thin-walled structure. This is conducive to causing more defects, exposing active centers, and improving catalytic activity. Figure 2 The measured lattice spacing shown in d is 0.244 nm, corresponding to Co 3 O 4 (311) crystal plane, which is consistent with the monodisperse Mo / Co 3 O 4 The XRD results are consistent with those of Figure 2 In d, it can be observed that the Mo element is uniformly dispersed on the support, which further confirms that Mo is monodispersed on the support, allowing more active centers to participate in the catalytic reaction.

[0052] Figure 3 The monodispersed Mo / Co prepared in Example 3 3 O 4 The characteristic absorption peak of TMB catalyzed by nanozymes at 652 nm verifies the monodisperse Mo / Co 3 O 4 Ultra-high oxidase-like activity of nanomaterials. Monodispersed Mo / Co 3 O 4 The nanomaterial directly oxidizes TMB molecules under dissolved oxygen conditions, changing the color of the solution from colorless to blue, exhibiting ultra-high oxidase-like properties.

[0053] Example 6

[0054] Take 3g of substitute tea and brew it for 5min, then drain the tea into a tea bowl. After cooling to room temperature, filter it through a 0.45 μm aqueous filter membrane for later use.

[0055] Add 1 μL of 1 mg / mL prepared in Example 2 to 790 μL of NaAc-HAc buffer (0.2 M, pH 3.5). -1 Monodisperse Mo / Co 3 O 4 Nanozyme, then add 200 μL 0.1 μM-200 μM sulfite solution (substitute tea supernatant) and 200 μL TMB (3 mM) in sequence, react at room temperature for 10 min, stand at room temperature for 20 min, and analyze the changes in the intensity of the ultraviolet absorption peak at 652 nm.

[0056] Example 7

[0057] Take 3g of substitute tea and brew it for 5min, then drain the tea into a tea bowl. After cooling to room temperature, filter it through a 0.45 μm aqueous filter membrane for later use.

[0058] Add 5 μL of 1 mg / mL prepared in Example 3 to 790 μL of NaAc-HAc buffer (0.2 M, pH 3.5). -1 Monodisperse Mo / Co 3 O 4 Nanozyme, then add 200 μL 0.1 μM-200 μM sulfite solution (substitute tea supernatant) and 200 μL TMB (3 mM) in sequence, react at room temperature for 10 min, stand at room temperature for 20 min, and analyze the changes in the intensity of the ultraviolet absorption peak at 652 nm.

[0059] Figure 4 The monodispersed Mo / Co prepared in Example 3 3 O 4 The oxidase-like activity of sulfite was used for sulfite detection. Figure 4 b is the standard curve established between UV-visible absorbance at 652 nm and sulfite concentration. The results show that sulfite has good linearity between 0.1-100 μΜ, R 2 The colorimetric platform has good linearity in a wide detection range and a lower detection limit, which can meet the detection needs of sulfite in food such as substitute tea in my country.

[0060] Example 8

[0061] Take 3g of substitute tea and brew it for 5min, then drain the tea into a tea bowl. After cooling to room temperature, filter it through a 0.45 μm aqueous filter membrane for later use.

[0062] Add 10 μL of 1 mg / mL prepared in Example 4 to 790 μL of NaAc-HAc buffer (0.2 M, pH 3.5). -1 Monodisperse Mo / Co 3 O 4 Nanozyme, then 200 μL sulfite solution (surrogate tea supernatant) and 200 μL TMB (3 mM) were added in sequence at 37 o C for 10 min, and then stand at room temperature for 20 min, and then analyze the change of the ultraviolet absorption peak intensity at 652 nm by ultraviolet spectrophotometer.

[0063] 1, 5, 10 mg / kg in tea substitutes -1 The results of different levels of spiked test were 1.07±0.01 mgkg -1 , 4.14±0.06 mgkg -1 and 8.91±0.08 mgkg -1 The recoveries were between 82.8% and 107.1%, all meeting the detection requirements. The RSDs at different spiked levels were all less than 10%, and the results were satisfactory, further demonstrating that the detection method had high accuracy and was feasible for detecting sulfite in substitute tea drinks.

Claims

1. A method for preparing monodisperse Mo / Co3O4 nanozymes, characterized in that The following steps are involved: (1) Dissolve 2-methylimidazole and cobalt nitrate hexahydrate in methanol, stir vigorously, let stand at room temperature, centrifuge, wash, and dry to obtain the metal organic framework ZIF-67; The molar mass ratio of the 2-methylimidazole to cobalt nitrate hexahydrate is 1:1 to 5:1, and the standing time at room temperature is 24 hours; (2) adding the ZIF-67 obtained in step (1) into ethanol and dispersing by ultrasonication to obtain a ZIF-67 dispersion solution; (3) dissolving sodium molybdate dihydrate in deionized water, mixing with the ZIF-67 dispersion solution obtained in step (2), heating to reflux, centrifuging, drying, and calcining in air to obtain a monodispersed Mo / Co3O4 nanozyme; The mass ratio of ZIF-67 to sodium molybdate dihydrate is 1:0.01-1:5, the heating reflux temperature is 80°C, the heating reflux time is 2h, the roasting temperature is 200°C-400°C, and the roasting time is 1h-3h.

2. The preparation method according to claim 1, characterized in that In the step (2), the ultrasonic time is 5 to 30 minutes and the ultrasonic power is 50W.

3. A monodisperse Mo / Co3O4 nanozyme obtained by the preparation method described in any one of claims 1-2.

4. Use of the monodisperse Mo / Co3O4 nanozyme as described in claim 3 in the visualization detection of sulfite.

5. The use according to claim 4, characterized in that The following steps are involved: (1) Add boiling water to the crushed substitute tea to brew for extraction, and pass through a membrane to obtain a supernatant; (2) Weighing monodispersed Mo / Co3O4 nanozymes and adding deionized water, ultrasonically dispersing to obtain nanozyme stock solution, and storing at 4°C for later use; (3) adding the nanozyme stock solution, the supernatant obtained in step (1), and 3,3',5,5'-tetramethylbenzidine to the acetic acid-sodium acetate buffer solution in sequence; (4) React at room temperature or 37°C, let stand for 20 min, and then analyze using a UV spectrophotometer. Calculate the sulfite content based on the change in the absorption peak intensity at 652 nm.

6. The use according to claim 5, characterized in that The concentration of the monodispersed Mo / Co3O4 nanozyme stock solution in step (2) is 1 mg·mL -1 .

7. The use according to claim 5, characterized in that In the step (3), the pH of the acetic acid-sodium acetate buffer solution is 3.5, and the volume of the monodispersed Mo / Co3O4 nanozyme added is 1 to 10 uL.

8. The use according to claim 5, characterized in that The reaction time in step (4) is 10 min at room temperature or 37°C.