Method for producing hydrogel article containing carbon dioxide

By preparing and adjusting the loss tangent value of the hydrogel, and sealing and cross-linking it in a high carbonic acid gas atmosphere, the problems of low carbonic acid gas concentration and low production efficiency in the existing technology are solved, and the rapid and efficient production of carbonic acid gas-containing gels is achieved. Hydrogel items.

CN115335026BActive Publication Date: 2024-10-18KAO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180024759.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-10-18
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

It is difficult to effectively increase the concentration of carbonic acid gas in hydrogels with existing technology, and the efficiency of manufacturing hydrogel articles containing carbonic acid gas in industrial production is low, and it takes a long time to absorb carbonic acid gas.

Method used

By preparing a hydrogel containing water-soluble polymers, cross-linking agents and water, and adjusting the loss tangent value in the dynamic viscoelasticity measurement so that the loss tangent at 1 Hz is above 0.46, then in a gas with a high concentration of carbonic acid gas It is sealed and cross-linked in the atmosphere until the loss tangent is less than 0.46 to achieve the purpose of efficiently absorbing carbonic acid gas.

Benefits of technology

The invention realizes rapid and productive manufacturing of hydrogel articles containing carbonic acid gas, improves the concentration and absorption efficiency of carbonic acid gas, and reduces production time and space occupation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115335026B_ABST
    Figure CN115335026B_ABST
Patent Text Reader

Abstract

A method for producing a hydrogel article containing carbon dioxide, comprising steps (1) to (3). (1) Preparing an article containing a hydrogel, wherein the hydrogel contains a water-soluble polymer, a crosslinking agent for the water-soluble polymer, and water, and wherein the loss tangent of the hydrogel at 1 Hz in a dynamic viscoelasticity measurement is greater than 0.46. (2) When the loss tangent of the hydrogel at 1 Hz in the dynamic viscoelasticity measurement in the hydrogel article is greater than 0.46, adjusting the composition of the surrounding gas atmosphere of the hydrogel article so that the concentration of carbon dioxide in the surrounding gas atmosphere becomes greater than 10% by volume, and sealing the hydrogel article in a package. (3) Crosslinking the hydrogel until the loss tangent of the hydrogel at 1 Hz in the dynamic viscoelasticity measurement in the hydrogel article is less than 0.46, thereby obtaining a hydrogel article containing carbon dioxide sealed in a package.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a water-containing gel article containing carbon dioxide. Background Art

[0002] As prior art related to the process of making a viscous substance contain a dissolved gas, for example, the techniques described in Patent Documents 1 and 2 are known. Patent Document 1 describes a technique in which a viscous substance is introduced into a pressure box filled with a dissolved gas and under high pressure conditions, and the dissolved gas is dissolved in the viscous substance by stirring with a stirrer or by using a porous body.

[0003] Patent document 2 describes a technology in which carboxymethyl cellulose and dried aluminum hydroxide gel are mixed to prepare a hydrogel stock solution, the hydrogel is matured to promote the ionic crosslinking reaction of the hydrogel, thereby obtaining a crosslinked hydrogel sheet, and then the hydrogel sheet is sealed in a package having a carbon dioxide concentration of 90% or more, thereby dissolving the carbon dioxide in the hydrogel sheet.

[0004] [Prior art literature]

[0005] Patent Literature

[0006] Patent Document 1: JP2014-62087A

[0007] Patent document 2: US2020 / 100991A1 Summary of the invention

[0008] The present invention provides a method for producing a hydrogel article containing carbon dioxide, which comprises the following steps (1) to (3).

[0009] (1) A step of preparing an article containing a hydrogel, wherein the hydrogel contains (A) a water-soluble polymer, (B) a crosslinking agent for the water-soluble polymer, and (C) water, and wherein the loss tangent of the hydrogel at 1 Hz in a dynamic viscoelasticity measurement is 0.46 or more.

[0010] (2) A process of adjusting the composition of the surrounding gas atmosphere of the article containing the hydrogel so that the concentration of carbon dioxide gas in the surrounding gas atmosphere of the article containing the hydrogel becomes 10% by volume or more, and sealing the article containing the hydrogel in a packaging body, when the loss tangent of the hydrogel in the dynamic viscoelasticity measurement at 1 Hz is greater than 0.46.

[0011] (3) A step of cross-linking the hydrogel until the loss tangent of the hydrogel in the hydrogel-containing article at 1 Hz in a dynamic viscoelasticity measurement is less than 0.46, thereby obtaining the hydrogel article containing carbon dioxide sealed in the package. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic diagram showing a preferred apparatus for carrying out the method of the present invention. DETAILED DESCRIPTION

[0013] In recent years, a hydrogel containing dissolved carbonic acid gas has been applied to various parts of the human body in order to promote blood circulation or beautify the body. The techniques described in the above-mentioned Patent Documents 1 and 2 are used in this case. In order to efficiently impart carbonic acid gas to the human body, it is necessary to increase the concentration of carbonic acid gas contained in the hydrogel. In addition, when industrial production is desired, a method for efficiently manufacturing hydrogel articles containing carbonic acid gas is required. However, according to the techniques described in Patent Documents 1 and 2, it is difficult to increase the concentration of carbonic acid gas that can be contained in the hydrogel, or even if the concentration of carbonic acid gas can be increased, it takes time to reach a high concentration. In addition, there is room for improvement in terms of efficiently manufacturing hydrogel articles containing carbonic acid gas.

[0014] Therefore, the present invention relates to a method for producing a hydrogel article containing carbon dioxide that can eliminate the disadvantages of the above-mentioned prior art.

[0015] The present invention is described below based on its preferred embodiments. The present invention provides a method for producing a hydrogel article containing carbon dioxide. As will be apparent from the following description, the present invention can produce a hydrogel article containing carbon dioxide that is sealed in a package. The hydrogel article containing carbon dioxide has a hydrogel containing carbon dioxide. The hydrogel contains carbon dioxide.

[0016] The carbon dioxide-containing hydrogel article having the above-mentioned composition is preferably produced by a method comprising the following steps (1) to (3).

[0017] (1) Process for preparing an article containing a hydrogel.

[0018] (2) A step of sealing an article containing the hydrogel together with carbon dioxide gas in a package.

[0019] (3) Cross-linking step of the hydrogel.

[0020] Hereinafter, these steps will be described respectively.

[0021] (1) Process for preparing articles containing hydrogel

[0022] In this step, a hydrogel is prepared. The hydrogel contains (A) a water-soluble polymer, (B) a crosslinking agent for the water-soluble polymer, and (C) water. The details of the water-soluble polymer and the crosslinking agent for the water-soluble polymer will be described below. The components (A) to (C) are mixed to obtain a hydrogel. Various mixers can be used for mixing.

[0023] The preparation of the hydrogel can be carried out at room temperature or under heating conditions. In this specification, "room temperature" refers to ambient temperature, which refers to the temperature in the state where the environment in which the production method is carried out is not intentionally heated or cooled, and generally refers to a temperature range of 10°C to 35°C.

[0024] The preparation of the hydrogel may be carried out under atmospheric pressure, or under a pressure condition increased or decreased compared to atmospheric pressure. Preferably, a pressure of [atmospheric pressure - 0.1 MPa] or higher is used.

[0025] In this specification, "atmospheric pressure" refers to ambient pressure, refers to the pressure in a state where the environment in which the present production method is carried out is not intentionally pressurized or depressurized, and refers to standard atmospheric pressure (1 atmosphere = 0.1 MPa).

[0026] In this process, in order to make it easy for the hydrogel to contain carbon dioxide, it is preferred to prepare the hydrogel by mixing a water-soluble polymer, a cross-linking agent and water under atmospheric pressure. In this way, the obtained hydrogel can contain a plurality of bubbles. That is, a hydrogel containing bubbles can be easily obtained. By making the hydrogel contain bubbles, a large amount of carbon dioxide can be easily contained in the hydrogel in the later-described process (2). In addition, the hydrogel prepared in this process is in an uncross-linked state, specifically, it is a hydrogel having a loss tangent at 1 Hz in the dynamic viscoelasticity measurement (hereinafter also referred to as "loss tangent (1 Hz)") of 0.46 or more. Details on the measurement conditions of the loss tangent will be described below.

[0027] In addition, depending on the type of the target hydrogel article containing carbon dioxide gas, it may be undesirable to generate bubbles in the hydrogel from the viewpoint of making the article difficult to peel off from the attachment surface and from the viewpoint of making the article have excellent followability to the attachment surface. In this case, the hydrogel can be prepared under reduced pressure conditions.

[0028] From the perspective of efficient production, regardless of the pressure and temperature when preparing the hydrogel, the time for mixing the above-mentioned (A) to (C) components is preferably from 1 minute to 60 minutes, and more preferably from 5 minutes to 30 minutes. The stirring speed during mixing can be appropriately changed according to the amount of the hydrogel to be prepared. For example, in the case of preparing 1 kg of hydrogel, from the perspective of containing more bubbles, the speed is preferably from 10 rpm to 80 rpm (revolutions / minute), more preferably from 20 rpm to 70 rpm, and even more preferably from 30 rpm to 65 rpm. By mixing under such conditions, a plurality of fine bubbles can be generated.

[0029] The type of mixer used is not particularly limited, but from the viewpoint of efficiently introducing a large number of bubbles, the mixer used is preferably a planetary mixer or a wet mixing kneader capable of performing rotation and revolution mixing.

[0030] In this step, in order to improve various properties of the carbon dioxide-containing hydrogel article to be produced, the above-mentioned components (A) to (C) may be mixed with other components. For example, a TRPM8 agonist or an oil may be used.

[0031] In this step, from the viewpoint of making it easy for the hydrogel to contain carbonic acid gas, it is preferred to prepare the hydrogel in such a manner that the ratio of water in the hydrogel becomes high. In this way, in the following step (3), the hydrogel easily contains a large amount of carbonic acid gas. In this step, from the viewpoint of making it easy for the hydrogel to contain carbonic acid gas, the hydrogel is prepared in such a manner that the ratio of water in the hydrogel is more preferably 20 mass % to 95 mass %, more preferably 30 mass % to 92 mass %, further more preferably 40 mass % to 88 mass %, and further preferably 70 mass % to 88 mass %.

[0032] [Step of forming an article containing a hydrogel]

[0033] In this step, the hydrogel obtained in the above-mentioned order is preferably applied to a support, thereby forming a sheet-like article containing a hydrogel layer on one surface of the support (hereinafter also referred to as a "hydrogel article"). Various coating machines can be used for coating the hydrogel. The hydrogel layer is formed by extending the hydrogel on one surface of the support using a coating machine.

[0034] When the hydrogel is stretched by a coating machine, for example, the hydrogel can be sandwiched between two sheets and stretched uniformly. The two sheets sandwiching the hydrogel can be, for example, nonwoven fabrics, resin films such as PET (polyethylene terephthalate) films, etc., which can be independently cited.

[0035] From the viewpoint of forming a smooth hydrogel layer, it is preferred to use a roll coater as the coater, and it is more preferred to use a double-roll coater as the coater. By using such a coater, a fixed strong pressure can be applied while the support passes between the rolls, thereby extending the hydrogel. As a result, a hydrogel layer can be formed while the support carries the hydrogel and the bubbles in the hydrogel are maintained. As such a double-roll coater, for example, a direct gravure coater, a chamber blade coater, a double-roll coater, etc. can be cited.

[0036] When a sheet-like hydrogel article having a hydrogel layer formed on one surface of a support is produced, from the viewpoint of making it easy for the hydrogel to contain carbon dioxide gas, the hydrogel layer in the target hydrogel article containing carbon dioxide gas is preferably coated to a thickness of 0.5 mm or more, more preferably 0.7 mm or more, and even more preferably 1 mm or more. From the viewpoint of making it difficult for the hydrogel article containing carbon dioxide gas to be peeled off from the attachment surface and from the viewpoint of making the article have excellent followability to the attachment surface, the hydrogel layer is preferably coated to a thickness of 5 mm or less, more preferably 3 mm or less, and even more preferably 2 mm or less.

[0037] (2) Step of sealing the hydrogel article in a package

[0038] In this step, the hydrogel article and the carbon dioxide gas are sealed in a package in order to allow the hydrogel in the hydrogel article to absorb carbon dioxide gas. In this case, the hydrogel article may be placed in the package and then the carbon dioxide gas may be sealed in the package, or the operation may be performed in the reverse order. However, from the viewpoint of increasing the daily production volume (daily output), it is preferred to perform the operation of sealing the carbon dioxide gas and sealing the hydrogel article in the package at the same time.

[0039] Since the hydrogel contains a water-soluble polymer and a crosslinking agent for the water-soluble polymer, the crosslinking of the water-soluble polymer begins when the two come into contact. By crosslinking the water-soluble polymer, a dense network structure that becomes the basic skeleton of the hydrogel is formed. The hydrogel formed by chemically crosslinking the water-soluble polymer swells because a large amount of water is retained in the network structure, so it has appropriate elasticity, stretchability, and softness.

[0040] If carbon dioxide is added to the hydrogel after the crosslinking is completed or at the end of the crosslinking, it takes time for the carbon dioxide to be absorbed into the hydrogel. That is, this is not advantageous from the viewpoint of increasing the daily production. Therefore, in the present invention, carbon dioxide is added to the hydrogel at a stage where the degree of crosslinking of the water-soluble polymer is low. Thus, carbon dioxide can be added to the hydrogel in a short time with good productivity, thereby increasing the daily production.

[0041] It is not easy to quantitatively evaluate the degree of crosslinking of water-soluble polymers contained in hydrogels. From this point of view, the present inventors have conducted various studies and found that it is effective to evaluate the degree of crosslinking of water-soluble polymers using the dynamic viscoelastic modulus of hydrogels as a measure. The dynamic viscoelastic modulus includes storage modulus, loss elastic modulus and loss tangent. The present inventors found that among them, using the loss tangent as a measure is the most objective for evaluating the degree of crosslinking of water-soluble polymers.

[0042] In summary, in the present invention, the degree of crosslinking of the water-soluble polymer is evaluated based on the loss tangent of the hydrogel. In a state where the degree of crosslinking of the water-soluble polymer is low, the value of the loss tangent is relatively high, and as the crosslinking proceeds, the value of the loss tangent of the hydrogel becomes lower. Therefore, in the present invention, from the perspective of increasing daily production and making it easy for the hydrogel to contain carbon dioxide, the loss tangent of the hydrogel at 1Hz in the dynamic viscoelasticity measurement is 0.46 or more, preferably 0.48 or more, more preferably 0.50 or more, and further preferably 0.55 or more; in addition, from the perspective of increasing daily production, the loss tangent is preferably 0.90 or less, more preferably 0.80 or less; further, from the perspective of making it easy for the hydrogel to contain carbon dioxide, the loss tangent is further preferably 0.65 or less, and further preferably 0.64 or less, at which time the hydrogel will absorb carbon dioxide. The method for measuring the loss tangent is as follows. In the present invention, the value at a frequency of 1Hz is used as the value of the loss tangent. The reason for this is that this frequency is a frequency that appropriately reflects the cross-linked state of the hydrogel.

[0043] The loss tangent (1 Hz) of the hydrogel in the present invention can be measured by the following method. The measurement is carried out at room temperature and pressure, and the other measurement conditions are as follows. The loss elastic modulus and storage modulus are determined by measurement, and the loss tangent (tanδ value) is calculated based on these values. In addition, when determining the loss tangent of the hydrogel, the hydrogel is cut into a circle with a diameter of 25 mm and fixed on a parallel plate with double-sided tape for measurement.

[0044] The measurement was performed multiple times (3 times or more), and the average value was adopted as the loss tangent (tan δ value).

[0045] · Equipment: Rheometer Physica MCR301 (manufactured by Anton Paar Co., Ltd.)

[0046] ·Specimen: Parallel plate with a diameter of 25 mm

[0047] Normal force: 1N

[0048] Gap interval: 1~2mm

[0049] ·Mass of water-containing gel: 0.5~1.0g

[0050] Frequency: 1Hz

[0051] Strain: 2%

[0052] Temperature: 25℃

[0053] In order to make the hydrogel absorb carbon dioxide, it is preferred to set the surrounding gas atmosphere of the hydrogel article to be rich in carbon dioxide. From this point of view, it is preferred that when the loss tangent of the hydrogel is above the above value, that is, when the water-soluble polymer is not excessively cross-linked, the composition of the surrounding gas atmosphere is adjusted in such a way that the concentration of carbon dioxide in the surrounding gas atmosphere of the hydrogel article is preferably 10% by volume or more. By setting the concentration of carbon dioxide in the surrounding gas atmosphere to above this value, the hydrogel can efficiently absorb carbon dioxide. From this point of view, it is more preferred to set the carbon dioxide concentration in the surrounding gas atmosphere to 30% by volume or more, further preferably to 60% by mass or more, and further more preferably to 80% by volume or more. From the perspective of efficiently absorbing carbon dioxide, the higher the concentration of carbon dioxide in the surrounding gas atmosphere, the better, and its ideal concentration is 100% by volume.

[0054] Regarding the surrounding atmosphere when the hydrogel absorbs carbon dioxide, there is no particular limitation on the type of other gas components as long as it contains carbon dioxide. An industrially convenient method is to mix carbon dioxide into the air to increase the concentration of carbon dioxide in the surrounding atmosphere.

[0055] As for the concentration of carbon dioxide in the surrounding gas atmosphere, as long as the loss tangent of the hydrogel is greater than the above value and temporarily reaches 10% by volume or more, it is sufficient to absorb carbon dioxide efficiently, and the concentration of carbon dioxide thereafter may be lower than 10% by volume. Of course, it goes without saying that the concentration of carbon dioxide in the surrounding gas atmosphere can be maintained at 10% by volume or more during the period when the hydrogel absorbs carbon dioxide.

[0056] This process can be carried out at room temperature or under heating conditions. In addition, this process can be carried out at atmospheric pressure, or under a pressurized condition greater than atmospheric pressure, or under a reduced pressure condition lower than atmospheric pressure. In the present invention, the absorption of carbon dioxide by the hydrogel is carried out in the initial stage of cross-linking of the water-soluble polymer, so that even without heating, carbon dioxide can be efficiently absorbed into the hydrogel. For the same reason, carbon dioxide can be efficiently absorbed into the hydrogel even without pressurization. Heating and / or pressurization are not necessarily conducive to increasing daily production. Therefore, this process is preferably carried out at room temperature and atmospheric pressure. In this way, the target hydrogel article containing carbon dioxide can be obtained with good productivity.

[0057] exist Figure 1 1 shows a structure of an embodiment of an apparatus for carrying out this process. The manufacturing apparatus 10 shown in the figure includes a first film-joining unit 20 , a nozzle unit 30 , a second film-joining unit 40 , and a cutting unit 50 .

[0058] The first film joining unit 20 is a device that joins the side portions of the original film sheet conveyed in the conveying direction MD to each other along the conveying direction MD. Figure 1 As shown, a first original sheet 11 of a non-breathable film conveyed in a conveying direction MD (hereinafter also referred to as the "first film original sheet 11") and a second original sheet 12 of a non-breathable film conveyed in the same direction as the original sheet 11 (hereinafter also referred to as the "second film original sheet 12") respectively have the same width and are supplied to the first film joining portion 20 in an overlapping state in which the positions of the two side edges of the two original sheets 11 and 12 are aligned.

[0059] like Figure 1As shown, the two original sheets 11 and 12 are conveyed by a conveying mechanism (not shown) such as a conveying roller or a conveyor belt with the hydrogel article 5 arranged between the two original sheets, and are supplied to the first film joint section 20. The loss tangent (1 Hz) of the hydrogel in the hydrogel article 5 at this time is equal to or greater than the above value. The two original sheets 11 and 12 are conveyed in a state where the positions of the two side edges thereof are overlapped and pass through the first film joint section 20, whereby the joining parts of the two original sheets 11 and 12, that is, the two side parts, are continuously joined along the conveying direction MD to form the first joining parts 15 and 15. After the two original sheets 11 and 12 pass through the first film joint section 20, the hydrogel article 5 is conveyed together with the original sheets in a state where it is located between the first joining parts 15 and 15 formed at the two side parts of the two original sheets 11 and 12 in the direction CD (hereinafter also referred to as the "width direction CD") orthogonal to the conveying direction MD. The joining method in the first film joint section 20 can be, for example, heat sealing. From the viewpoint of efficiently joining the films, as shown in the figure, it is preferable to arrange the pair of first film-joining parts 20 outward from both side edges of the hydrogel article 5 in the width direction CD.

[0060] The nozzle portion 30 is a portion for supplying the gas containing carbon dioxide gas sealed in the package. The nozzle portion 30 is a hollow member through which gas can flow, and has: one end of the nozzle portion 30 located at a position closer to the upstream side of the conveying direction MD than the first film joint portion 20, and an open end 31 as the other end of the nozzle portion 30. The nozzle portion 30 can continuously or intermittently supply the gas containing carbon dioxide gas supplied from a gas source (not shown) connected to one end thereof to the outside from the open end 31 as the other end of the nozzle portion 30. The open end 31 of the nozzle portion 30 is located at a position closer to the downstream side of the conveying direction MD than the first film joint portion 20, and is located at a position closer to the inner side of the CD direction than the first joint portion 15. Figure 1 The nozzle unit 30 shown in the figure has a pair of nozzle extensions 32 arranged in a manner extending along the conveying direction MD between the two original sheets 11 and 12, thereby supplying a gas flow along the conveying direction MD of the two original sheets 11 and 12. The nozzle extensions 32 are arranged to be substantially parallel to each other. In addition, the nozzle extensions 32 of the nozzle unit 30 are located at a position closer to the inside than the first film joint 20 in the width direction CD, and are arranged at a position closer to the outside than the two end edges of the water-containing gel article 5 to be conveyed. The nozzle unit 30 shown in the figure has a portion bent from the outside of the two side portions of the original sheets 11 and 12 to the inside at a position closer to the upstream side of the first film joint 20 in the conveying direction, thereby, the nozzle extension 32 is arranged between the two original sheets 11 and 12.

[0061] By supplying the gas containing carbon dioxide through the nozzle portion 30, more than 90% by volume of the atmosphere in the space defined by the two original sheets 11 and 12 can be replaced with the gas containing carbon dioxide. Therefore, when the gas containing carbon dioxide is carbon dioxide itself, the gas concentration in the space defined by the two original sheets 11 and 12 can be set to approximately 100% by volume of carbon dioxide.

[0062] A second film joining section 40 is arranged downstream in the conveying direction MD of the arrangement position of the nozzle section 30. The second film joining section 40 is a device for joining the two original sheets 11 and 12 whose both sides are joined to each other by the first film joining section 20 in a direction intersecting the conveying direction MD. The second film joining section 40 shown in the figure is in the form of a heating roller. In a state where the hydrogel article 5 is located between the two heating rollers constituting the second film joining section 40, the two original sheets 11 and 12 are joined at a predetermined interval in a direction intersecting the conveying direction MD, thereby forming a continuous package body 1A in which the two original sheets 11 and 12 are joined at the periphery of the hydrogel article 5. For example, heat sealing or the like can be used as a joining method in the second film joining section 40.

[0063] The second film joining section 40 joins the two original sheets 11 and 12 whose both sides are joined by the first film joining section 20 in a direction intersecting the conveying direction MD to form second joining locations 16 and 16 extending over the entire area in the width direction CD. Figure 1 The second film joint part 40 shown is in the form of a heating roller. Before the second joint part 16 is formed, the second film joint part 40 is arranged so that the parts of the two original sheets 11 and 12 other than the first joint part 15 are separated. Preferably, the second film joint part 40 is separated from the two original sheets 11 and 12. When the hydrogel article 5 is located between the second film joint parts 40 arranged along the conveying direction MD, the second film joint part 40 is pressed against the two original sheets 11 and 12 by a control mechanism (not shown) that moves the second film joint part 40 so that the two original sheets 11 and 12 abut against each other, and the two original sheets 11 and 12 are joined in a direction intersecting the conveying direction MD. Thus, the two original sheets 11 and 12 located outside the periphery of the hydrogel article 5 are joined to each other through a pair of first joint parts 15 and 15 and a pair of second joint parts 16 and 16. Thus, a continuous package body 1A in which the hydrogel article 5 and the gas containing carbon dioxide are sealed in a sealed state in the two joint parts 15 and 16 can be formed.

[0064] A cutting unit 50 is arranged at a position downstream of the second film joint unit 40 in the conveying direction MD. The cutting unit 50 has a cutting blade extending in a direction intersecting the conveying direction MD, and can cut the two original sheets 11 and 12 at the second joint portion 16 of the package continuous body 1A to separate the two packages 1. Figure 1 The cutting unit 50 shown is in the form of a cutting roller whose axial direction is consistent with the width direction CD, and has: a first cutting blade 50a arranged on the circumference of the roller and extending in the axial direction of the roller, and a second cutting blade 50b extending along the circumferential direction of the roller. By the rotation of the cutting roller, the first cutting blade 50a cuts the package body continuum 1A in the direction intersecting the conveying direction MD at the position of the second joint portion 16. At the same time, since a pair of second cutting blades 50b are arranged on both end sides of the package body continuum 1A in the width direction CD, the package body continuum 1A is cut in the conveying direction MD at the position of the first joint portion 15. In this way, a package body 1 in which a gas containing carbon dioxide gas and a hydrogel article are sealed can be formed.

[0065] According to the apparatus having the above structure, the nozzle portion 30 is located inwardly of the first film-joining portion 20 in the width direction CD, and the opening end 31 of the nozzle portion 30 is located downstream of the first film-joining portion 20 in the conveying direction. Therefore, the nozzle portion 30 functions as a guide for defining the joining position of the two original sheets 11 and 12, and the two original sheets 11 and 12 can be joined to each other at a desired position along the conveying direction. In addition, when the films are joined to each other, since the movement of the hydrogel article 5 is restricted by the nozzle portion 30, the hydrogel article 5 can be prevented from being accidentally caught in or bitten by the first film-joining portion 20. As a result, the package 1 can be stably and continuously manufactured without damaging the hydrogel article 5. In addition, since the nozzle portion 30 is configured along the conveying direction MD and extends downstream of the conveying direction of the first film joining portion 20, compared with the case where the nozzle portion 30 is inserted in a direction intersecting the conveying direction MD, the advantage of being able to efficiently replace the atmosphere in the two original sheets 11 and 12 with a gas containing carbon dioxide is also achieved.

[0066] Thus, according to the apparatus having the above structure, the following steps can be continuously performed: a first joining step of joining the two sides of the two sheets conveyed in one direction along the conveying direction while the hydrogel article is arranged between the first non-air-permeable sheet and the second non-air-permeable sheet and the gas containing carbon dioxide is supplied between the two sheets; a second joining step of joining the two sheets in a direction intersecting the conveying direction at a position where the hydrogel article is not present to form a continuous package body enclosed with the hydrogel article and the gas containing carbon dioxide; and a cutting step of cutting the continuous package body in a direction intersecting the conveying direction at the portion joined by the second joining step to form a package body. As a result, not only can the carbon dioxide be absorbed when the cross-linking degree of the water-soluble polymer is low, but also the desired hydrogel article containing carbon dioxide can be manufactured with better productivity.

[0067] (3) Cross-linking process of hydrogel

[0068] Through the above-mentioned step (2), the hydrogel article is sealed in a package together with the gas containing carbon dioxide. In this sealed state, the carbon dioxide is absorbed by the hydrogel. The absorption of carbon dioxide by the hydrogel occurs spontaneously. Therefore, no special operation such as heating the package is required. That is, the absorption of carbon dioxide by the hydrogel can be performed at room temperature. In addition, in the case where it is desired to increase the production speed, in this step, from the viewpoint of promoting the cross-linking of the water-soluble polymer described below, for example, the package can also be heated.

[0069] When bubbles exist in the hydrogel, carbon dioxide is dissolved in the hydrogel due to the osmotic pressure (concentration gradient) in the sealed package, and further diffuses into the bubbles. That is, carbon dioxide is not only absorbed by the hydrogel itself, but also absorbed into the bubbles when bubbles exist in the hydrogel. As carbon dioxide is absorbed, the concentration of carbon dioxide in the package gradually decreases, but this does not become a problem.

[0070] While the hydrogel absorbs carbon dioxide, the water-soluble polymer contained in the hydrogel is cross-linked. As a result, the loss tangent of the hydrogel is continuously reduced. From the viewpoint of making it easy for the hydrogel to contain carbon dioxide, the water-soluble polymer is cross-linked until the loss tangent (1 Hz) is less than 0.46, preferably less than 0.40, more preferably less than 0.38, and further preferably less than 0.35. When cross-linking is performed at room temperature, the time for cross-linking to be performed until the loss tangent is less than 0.46 is preferably from 24 hours to 366 hours after the hydrogel article is sealed, and more preferably from 24 hours to 240 hours.

[0071] In addition, from the viewpoint of making it easy for the hydrogel to contain carbon dioxide and improving the adhesiveness of the obtained hydrogel article, the crosslinking of the water-soluble polymer is preferably carried out until the loss tangent (1 Hz) is greater than 0.20 and less than 0.45, more preferably until the loss tangent (1 Hz) is greater than 0.35 and less than 0.45, and further preferably until the loss tangent (1 Hz) is greater than 0.40 and less than 0.45.

[0072] The crosslinking of the water-soluble polymer improves the shape retention of the hydrogel. When the crosslinking is completed, the concentration of carbon dioxide gas contained in the hydrogel is usually 10 ppm to 20,000 ppm, but this depends on the type of the water-soluble polymer or the water content of the hydrogel.

[0073] The so-called "carbon dioxide concentration" refers to a value obtained by placing a hydrogel article containing carbon dioxide in a covered container filled with an alkaline solution and immersing it for 12 hours, capturing carbon dioxide in the aqueous solution in the form of carbonate, and then restoring the acidity using an acidic buffer solution, and measuring the carbon dioxide concentration of the solution at room temperature 25°C using a carbon dioxide electrode. Thereafter, the obtained carbon dioxide concentration, the mass of the article, and the volume of the solution are converted into the content of carbon dioxide in the hydrogel article containing carbon dioxide.

[0074] In the prior art, when manufacturing such articles containing carbon dioxide, a long time is spent on aging in order to allow the hydrogel to absorb carbon dioxide. Therefore, in order to absorb carbon dioxide, it is necessary to ensure a space for temporarily preserving the articles. In contrast, according to the present manufacturing method, aging as performed in the prior art is performed at the end of the manufacturing process, so there is no need to ensure a space for temporarily preserving the articles. More specifically, the following advantages can be listed, etc.: After the completion of step (3), the articles can be immediately packed into a shipping box such as a cardboard box without taking up extra space.

[0075] In this way, a hydrogel article containing carbon dioxide can be obtained in which the hydrogel fully absorbs carbon dioxide. The article is preferably used as a body adhesive article for bonding the hydrogel to the body. By bonding the hydrogel article containing carbon dioxide to the body, the carbon dioxide contained in the hydrogel is released and acts on the skin, which can promote the blood circulation of the user. As the bonding site, it is preferably the body other than the scalp, for example, the feet, arms, shoulders, waist, etc. can be listed. There is no particular restriction on the time of bonding application, preferably more than 15 minutes, more preferably more than 30 minutes. For example, using the adhesive force of the hydrogel, it is attached before going to bed and used as a body adhesive article that is continuously applied throughout the whole sleeping process. In addition, the hydrogel article containing carbon dioxide in the present invention is not necessarily a sheet-like hydrogel article in which the hydrogel is supported on a support such as a non-woven fabric, but can also be a form in which the hydrogel is directly applied to the body.

[0076] The water-soluble polymer used in the above production method is not particularly limited in type as long as it can stably retain water. From the viewpoint of moldability, for example, anionic polymers are preferred.

[0077] As anionic polymers, for example, polymers having carboxyl groups, sulfate groups, or phosphoric acid groups can be cited. Specifically, poly(meth)acrylic acid and salts thereof; carboxyvinyl polymers and salts thereof; anionic cellulose derivatives such as carboxymethyl cellulose and carboxyethyl cellulose and salts thereof; carrageenan, alginic acid, and salts thereof; anionic starch derivatives, etc. Among them, from the perspective of obtaining a hydrogel that satisfies a particularly high water retention capacity and sufficient gel strength and flexibility that can follow unevenness or movement, it is preferred to use at least one selected from carboxymethyl cellulose and its salts, and poly(meth)acrylic acid and its salts, and more preferably, sodium carboxymethyl cellulose is used.

[0078] As the crosslinking agent for the water-soluble polymer, a crosslinking agent corresponding to the type of the water-soluble polymer is appropriately selected. When the water-soluble polymer is, for example, the anionic polymer described above, as the crosslinking agent, for example, metal ion compounds, cationic polymers, multifunctional epoxy compounds, etc. can be used.

[0079] Examples of the metal ion compound include oxides or hydroxides, salts, etc. containing aluminum, magnesium, calcium, potassium, etc. For example, one or more selected from aluminum hydroxide, potassium aluminum sulfate, aluminum sulfate, aluminum oxide, aluminum glycinate, aluminum acetate, aluminum lactate, aluminum stearate, hydrated aluminum silicate, aluminum metasilicate, magnesium aluminometasilicate, magnesium chloride, magnesium stearate, calcium carbonate, calcium hydroxide, kaolin, synthetic aluminum carbonate, and potassium hydroxide can be used.

[0080] When an anionic polymer that can be cross-linked by the action of aluminum, such as carboxymethyl cellulose or its salt, is used as the water-soluble polymer, a cross-linking agent that can supply aluminum to the water-soluble polymer, that is, an aluminum ion supplying cross-linking agent, is preferably used as the cross-linking agent because it has high solubility and good dispersibility in the hydrogel. As such a cross-linking agent, for example, aluminum ion compounds such as magnesium aluminum silicate or aluminum hydroxide are preferably used. In particular, magnesium aluminum silicate not only has high solubility and good dispersibility in the hydrogel, but also easily undergoes a cross-linking reaction even at room temperature, so it can give sufficient elasticity to the hydrogel.

[0081] When magnesium aluminum silicate is used as a crosslinking agent, it can be used alone or in combination with other crosslinking agents. When magnesium aluminum silicate is used with other crosslinking agents, from the viewpoint of being able to fully crosslink the water-soluble polymer, the ratio of magnesium aluminum silicate in the crosslinking agent is preferably set to 30 mass % or more and 100 mass % or less, and more preferably set to 70 mass % or more and 100 mass % or less.

[0082] From the viewpoint of increasing the daily production volume, it is preferred that the crosslinking agent be contained in the step (1) so that the content of the crosslinking agent is 0.01% by mass or more and 10% by mass or less in the hydrogel. From the viewpoint of further increasing the daily production volume, the amount of the crosslinking agent added is more preferably 0.03% by mass or more, further preferably 0.05% by mass or more, and further preferably 0.1% by mass or more in the hydrogel. From the viewpoint of making it easier to contain carbon dioxide gas in the hydrogel, it is more preferably 5% by mass or less, and further preferably 2% by mass or less.

[0083] Regarding the hydrogel article containing carbon dioxide obtained by the present production method, from the viewpoint of making it easy for the hydrogel to contain carbon dioxide, it is preferred that the hydrogel contain 10% or more of bubbles containing carbon dioxide in terms of bubble ratio, and more preferably contain 20% or more of bubbles containing carbon dioxide in terms of bubble ratio.

[0084] On the other hand, the hydrogel article containing carbon dioxide gas obtained by the present production method preferably contains 40% or less of bubbles containing carbon dioxide gas in terms of bubble ratio in the hydrogel, and more preferably contains 35% or less of bubbles containing carbon dioxide gas in terms of bubble ratio, from the viewpoint of making it difficult to peel off from the attached surface and having excellent followability to the attached surface. Here, the bubble ratio refers to a value measured and calculated by the following method.

[0085] The hydrogel article containing carbon dioxide obtained by the present manufacturing method is a product sealed in a gas-impermeable container, so the value measured within 5 minutes after the container is opened and the sheet is taken out is taken as the bubble rate. Specifically, the specific gravity of the part without bubbles is assumed to be 1, the taken out sheet is cut into a rectangular shape, and the volume A (mL) of the sheet is calculated based on the vertical, horizontal and high dimensions, and the mass B (g) is further measured. Then, these are substituted into the following formula (1) to calculate the bubble rate.

[0086] Bubble rate (%) = (A-B) / A×100 (1)

[0087] In addition, when the hydrogel article containing carbon dioxide gas is further supported on a support layer or a peeling layer, from the perspective of ease of operation, the measurement can be performed without removing or peeling these layers, and then the total mass of these support layers or peeling layers can be subtracted to calculate the bubble ratio.

[0088] In the hydrogel article containing carbon dioxide obtained by the present production method, the total area occupied by bubbles with a virtual diameter of 5 mm or more is preferably 10% or less of the surface area of ​​the hydrogel of 100%. In this way, by controlling the size of the bubbles, the carbon dioxide in the article can be efficiently supplied to the skin. In addition, the mixing of useless coarsened bubbles can be avoided, thereby improving the smoothness of the surface of the hydrogel, so that the adhesiveness of the article can be enhanced, and the adhesion to the body can be effectively improved.

[0089] In the hydrogel article containing carbon dioxide obtained by the present production method, the bubbles existing on the surface of the hydrogel are bubbles measured within 5 minutes after the hydrogel article containing carbon dioxide as the sealed content is taken out from the gas-impermeable container described below under the conditions of room temperature 25°C and relative humidity 50%. Here, since the bubbles may be indefinite ellipses, the bubbles are regarded as virtual circles whose diameter is the value obtained by adding the major axis and the minor axis and dividing by 2, and the diameter of the virtual circle is defined as the "virtual diameter of the bubbles". Therefore, the "total area occupied by bubbles with a virtual diameter of 5 mm or more" means the sum of the areas of the virtual circles calculated based on the virtual diameters of all bubbles with a virtual diameter of 5 mm or more defined in this way and existing on the surface of the skin contact side of the article. Then, the value of the total area is divided by the surface area of ​​the hydrogel taken as 100%, and the value is taken as the value of "the total area (%) occupied by bubbles with a virtual diameter of 5 mm or more in the surface area of ​​the hydrogel 100%".

[0090] In addition, regarding the hydrogel article containing carbon dioxide obtained by the present production method, when such fine bubbles exist in the entire region of the hydrogel layer, the bubbles exist not only on the surface of the hydrogel but also inside the hydrogel. Therefore, in a cross section of the hydrogel, regarding the bubbles existing in the cross section, "the value of the total area (%) occupied by bubbles with a virtual diameter of 5 mm or more in 100% of the area of ​​the cross section" also represents the same value as "the total area (%) occupied by bubbles with a virtual diameter of 5 mm or more in 100% of the surface area of ​​the hydrogel".

[0091] From the viewpoint of making the hydrogel article containing carbon dioxide gas obtained by the present production method difficult to peel off from the attached surface and having excellent followability to the attached surface, the total area occupied by bubbles with a virtual diameter of 5 mm or more in 100% of the surface area of ​​the hydrogel is, as described above, preferably 10% or less, more preferably 5% or less, and further preferably the hydrogel does not contain bubbles with a virtual diameter of 5 mm or more in 100% of the surface area of ​​the hydrogel.

[0092] As components that can be used arbitrarily when preparing the water-containing gel, there are listed components commonly used in cosmetics or pharmaceuticals, such as oily components, water-soluble polymers, alcohols, sugars, blood circulation promoters, skin nutrients, vitamins, antioxidants, antioxidant aids, preservatives, pigments, fragrances, etc.

[0093] As a support for coating the hydrogel, sheet substrates such as woven fabrics, nonwoven fabrics, knitted fabrics, films of synthetic resins, and water-resistant paper can be used. A laminate formed by stacking these layers can also be used. Specifically, woven fabrics or nonwoven fabrics formed by synthetic fibers such as polyamide, polypropylene, polyester, polyethylene, polystyrene, polyurethane, and polyolefins, and natural fibers such as silk, cotton, linen, rayon, and collagen can be used; sheets of polyamide, polypropylene, polyester, polyethylene, polyurethane, etc.; film sheets of pullulan or starch, etc., etc. Among them, from the viewpoint of suppressing the size of bubbles and ensuring good adhesion to the body, it is preferred to use woven fabrics or nonwoven fabrics, and more preferably nonwoven fabrics.

[0094] The thickness of the support is about 0.05 mm to 2.0 mm. The surface of the support coated with the hydrogel may be subjected to a hydrophilic treatment or a hydrophobic treatment.

[0095] As the non-air-permeable material constituting the packaging body, for example, a film on which a metal such as aluminum is vapor-deposited, or a laminated film in which two or more layers of films of different materials are laminated, etc. can be used. Figure 1 In the case of devices other than those shown, glass containers or plastic containers may also be used.

[0096] The package body must be airtight, and in particular, must be impermeable to carbon dioxide. “Impermeable to carbon dioxide” means that the carbon dioxide permeability is 50cc / (m 2 ·day·atm)(ASTMD-1434) or less, and non-permeable is further preferred. Preferred materials for the packaging body include materials with heat-sealing properties, specifically, laminated films laminated with aluminum foil, laminated films with aluminum vapor-deposited layers, polyvinylidene chloride films, laminated films containing polyvinylidene chloride layers, and the like. The form of the packaging body is preferably a flat bag or a self-supporting bag, etc. If necessary, in order to maintain a composition consisting only of the hydrogel, the following method may be used, etc.: using a tray made of polyethylene terephthalate, etc., filling the tray with the hydrogel, and storing it in a packaging body such as the bag described above.

[0097] Furthermore, from the viewpoint of suppressing expansion of the package due to temperature changes or the like, the package preferably maintains a volume with a filling ratio of 0.5 to 35% relative to its volume.

[0098] The present invention has been described above based on its preferred embodiments, but the present invention is not limited to the above embodiments. For example, the above steps (1) to (3) are preferably carried out at room temperature, and more preferably at room temperature and atmospheric pressure, but cooling, heating, decompression, pressurization and the like may be adopted in any one or more of the steps (1) to (3) as required. In particular, from the viewpoint of obtaining the target object efficiently and productively, it is preferred that all the steps (1) to (3) are carried out at room temperature and atmospheric pressure.

[0099] In relation to the above-mentioned embodiment, the present invention further discloses a method for producing a water-containing gel article containing carbon dioxide gas as described below.

[0100] <1>

[0101] A method for producing a hydrogel article containing carbon dioxide, comprising the following steps (1) to (3):

[0102] (1) preparing an article containing a hydrogel, the hydrogel containing (A) a water-soluble polymer, (B) a cross-linking agent for the water-soluble polymer, and (C) water, wherein the loss tangent of the hydrogel at 1 Hz in a dynamic viscoelasticity measurement is 0.46 or more;

[0103] (2) when the loss tangent of the hydrogel in the hydrogel-containing article at 1 Hz in a dynamic viscoelasticity measurement is 0.46 or more, adjusting the composition of the surrounding gas atmosphere of the hydrogel-containing article so that the concentration of carbon dioxide gas in the surrounding gas atmosphere becomes 10% by volume or more, and sealing the hydrogel-containing article in a package;

[0104] (3) The hydrogel is cross-linked until the loss tangent of the hydrogel in the hydrogel-containing article at 1 Hz in a dynamic viscoelasticity measurement is less than 0.46, thereby obtaining a hydrogel article containing carbon dioxide gas sealed in the package.

[0105] <2>

[0106] The production method as described in the above <1>, wherein the step (2) is performed at room temperature and atmospheric pressure.

[0107] <3>

[0108] The production method as described in <1> or <2> above, wherein:

[0109] The water-soluble polymer contains an anionic polymer.

[0110] The crosslinking agent contains aluminum ions to supply the crosslinking agent.

[0111] <4>

[0112] The production method as described in any one of <1> to <3> above, wherein step (2) comprises:

[0113] A first joining step is to place the hydrogel-containing article between a first air-impermeable sheet and a second air-impermeable sheet and to supply a gas containing carbon dioxide between the two sheets, and then join the two sides of the two sheets along the conveying direction.

[0114] A second joining step of joining the two original sheets in a direction intersecting the conveying direction at a position where the hydrogel article is not present, to form a continuous package body enclosing the hydrogel article and the gas containing carbon dioxide; and

[0115] The cutting step is to cut the continuous package body in a direction intersecting the conveying direction at the portion joined in the second joining step to form the package body.

[0116] <5>

[0117] A manufacturing method as described in any one of the above <1> to <4>, wherein in step (2), when the loss tangent is preferably greater than 0.48, more preferably greater than 0.50, further preferably greater than 0.55, and preferably less than 0.90, more preferably less than 0.80, further preferably less than 0.65, further more preferably less than 0.64, the composition of the surrounding gas atmosphere is adjusted in such a manner that the concentration of carbon dioxide gas in the surrounding gas atmosphere of the above-mentioned article containing the hydrogel becomes greater than 10 volume %.

[0118] <6>

[0119] The production method as described in the above <1> or <5>, wherein the step (1) includes the step of mixing the water-soluble polymer, the crosslinking agent and the water under atmospheric pressure to prepare the water-containing gel containing bubbles.

[0120] <7>

[0121] A manufacturing method as described in any one of the above <1> to <6>, wherein in step (2), when the loss tangent is greater than 0.46, the composition of the surrounding gas atmosphere is adjusted in such a manner that the concentration of carbon dioxide gas in the surrounding gas atmosphere of the above-mentioned article containing the hydrogel becomes greater than 10 volume %, preferably greater than 30 volume %, more preferably greater than 60 mass %, and further preferably greater than 80 volume %.

[0122] <8>

[0123] A manufacturing method as described in any one of the above <1> to <7>, wherein step (2) is carried out as follows: the operation of housing the above-mentioned article containing the hydrogel in the above-mentioned package and the operation of supplying the gas containing carbon dioxide into the above-mentioned package are carried out in this order, in the reverse order, or simultaneously, and then the package is sealed.

[0124] <9>

[0125] A production method as described in any one of the above <1> to <8>, wherein in step (3), the above-mentioned hydrogel is cross-linked until the above-mentioned loss tangent is preferably less than 0.40, more preferably less than 0.38, and further preferably less than 0.35, thereby obtaining a hydrogel article containing carbon dioxide gas sealed in the above-mentioned package.

[0126] <10>

[0127] The production method as described in any one of <1> to <9> above, wherein step (3) is carried out at room temperature, and in step (3), the time until the loss tangent becomes less than 0.46 is preferably from 24 hours to 366 hours after sealing the water-containing gel article, and more preferably from 24 hours to 240 hours.

[0128] <11>

[0129] A manufacturing method as described in any one of the above <1> to <10>, wherein in step (3), the crosslinking of the above-mentioned water-containing gel is preferably carried out until the above-mentioned loss tangent becomes greater than 0.20 and less than 0.45, more preferably carried out until the above-mentioned loss tangent becomes greater than 0.35 and less than 0.45, and further preferably carried out until the above-mentioned loss tangent becomes greater than 0.40 and less than 0.45.

[0130] <12>

[0131] The production method as described in any one of <1> to <11> above, wherein step (1) comprises the step of applying the obtained hydrogel onto a support to form an article containing the hydrogel on the support.

[0132] <13>

[0133] The manufacturing method as described in <12> above, wherein, in the step of forming the above-mentioned article containing the hydrogel on the above-mentioned support, the hydrogel is applied in such a manner that the thickness of the hydrogel in the above-mentioned hydrogel article containing carbon dioxide gas is preferably 0.5 mm to 5 mm, more preferably 0.7 mm to 3 mm, and even more preferably 1 mm to 2 mm.

[0134] <14>

[0135] The production method as described in any one of <1> to <13>, wherein in step (1), the time for mixing the water-soluble polymer, the crosslinking agent and the water is preferably from 1 minute to 60 minutes, and more preferably from 5 minutes to 30 minutes.

[0136] <15>

[0137] A production method as described in any one of the above <1> to the above <14>, wherein in step (1), the stirring speed when mixing the above-mentioned water-soluble polymer, the above-mentioned cross-linking agent and the above-mentioned water is preferably from 10 rpm to 80 rpm, more preferably from 20 rpm to 70 rpm, and further preferably from 30 rpm to 65 rpm.

[0138] <16>

[0139] The production method according to any one of <1> to <15>, wherein the water-soluble polymer is an anionic polymer.

[0140] <17>

[0141] The production method as described in the above <16>, wherein the anionic polymer is a carboxyl group, a sulfate group, or a phosphoric acid group.

[0142] <18>

[0143] A production method as described in <17> above, wherein the anionic polymer is at least one selected from poly(meth)acrylic acid and its salts, carboxyvinyl polymers and their salts, anionic cellulose derivatives such as carboxymethyl cellulose and carboxyethyl cellulose and their salts, carrageenan, alginic acid, and their salts, and anionic starch derivatives.

[0144] <19>

[0145] The production method according to any one of <1> to <18>, wherein the crosslinking agent is a metal ion compound, a cationic polymer, or a polyfunctional epoxy compound.

[0146] <20>

[0147] The production method as described in <19> above, wherein

[0148] The above cross-linking agent is a metal ion compound,

[0149] The metal ion compound is an oxide or hydroxide or a salt containing aluminum, magnesium, calcium, potassium, etc.

[0150] <21>

[0151] A production method as described in the above <20>, wherein the above-mentioned metal ion compound is one or more selected from aluminum hydroxide, potassium aluminum sulfate, aluminum sulfate, aluminum oxide, aluminum glycinate, aluminum acetate, aluminum lactate, aluminum stearate, hydrated aluminum silicate, aluminum metasilicate, magnesium aluminum silicate, magnesium chloride, magnesium stearate, calcium carbonate, calcium hydroxide, kaolin, synthetic aluminum magnesium carbonate, and potassium hydroxide.

[0152] <22>

[0153] The production method as described in the above <21>, wherein the metal ion compound is magnesium aluminum silicate.

[0154] <23>

[0155] The production method as described in the above <22>, wherein the ratio of magnesium aluminum silicate to the crosslinking agent is preferably 30 mass % to 100 mass %, more preferably 70 mass % to 100 mass %.

[0156] <24>

[0157] The production method as described in any one of the above <1> to <23>, wherein the amount of the cross-linking agent added to the above-mentioned hydrogel is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, further preferably 0.05% by mass or more, further more preferably 0.1% by mass or more, and is 10% by mass or less, more preferably 5% by mass or less, further preferably 2% by mass or less.

[0158] <25>

[0159] The production method as described in any one of the above <1> to the above <24>, wherein the amount of the water added to the above-mentioned water-containing gel is preferably 20 mass % to 95 mass %, more preferably 30 mass % to 92 mass %, further preferably 40 mass % to 88 mass %, and even more preferably 70 mass % to 88 mass %.

[0160] [Example]

[0161] Hereinafter, the present invention will be further described in detail by way of examples, but the scope of the present invention is not limited to the examples.

[0162] [Example 1]

[0163] <Process (1)>

[0164] The components shown in Table 1 were used in the amounts shown in the table. Under atmospheric pressure and 25° C., an aqueous solution prepared by dissolving 5 g of succinic acid and 50.0 g of polyvinyl alcohol in 764 g of water was added to a wet mixing kneader, and 28.0 g of sodium carboxymethylcellulose, 0.5 g of aluminum magnesium silicate, 100.0 g of glycerol, 50.0 g of propylene glycol and 2.5 g of methyl paraben were further added, and these were mixed at a stirring speed of 60 rpm for 40 minutes to prepare a water-containing gel containing bubbles.

[0165] [Step of forming an article containing a hydrogel]

[0166] The hydrogel obtained in step (1) was sandwiched between a polypropylene film and a nonwoven fabric under atmospheric pressure and 25°C, and stretched by a two-roll coater to form a hydrogel layer with a thickness of 2 mm. 2 , water-containing gel coating weight 1250g / m 2 ) in a rectangular size. Thus, a hydrogel article having a hydrogel layer containing bubbles formed on a support body comprising a nonwoven fabric was obtained.

[0167] <Process (2)>

[0168] In this process, use Figure 1 When the loss tangent (1 Hz) of the hydrogel in the hydrogel article obtained in the above process is 0.50 (4 hours after the completion of process (1)), two punched hydrogel articles are placed between two rectangular aluminum vapor-deposited films, carbon dioxide gas is supplied between the two films, and the four sides of the two vapor-deposited films are airtightly joined and sealed in a package containing the vapor-deposited films. The inner surface area of ​​the package containing the aluminum vapor-deposited film at this time is 300 cm 2 The volume of the package is 354cm 3 This step was performed at 25° C. and atmospheric pressure. Furthermore, the calculation method of the concentration of carbon dioxide gas in the surrounding atmosphere when the package body was sealed was as follows.

[0169] [Calculation method of carbon dioxide gas concentration in the surrounding gas atmosphere when the package is sealed]

[0170] Carbon dioxide is filled into a gas-impermeable container, and the oxygen concentration in the container is measured for the packaged hydrogel article. The carbon dioxide concentration in the container is calculated based on the value obtained. Specifically, the oxygen concentration (F%) in the container is measured using a zirconium oxide oxygen concentration meter LS-450F (manufactured by Toray Engineering Co., Ltd.). Since the oxygen concentration in the air is 20.6%, the ratio of air in the container (G%) is calculated using the formula: (F / 20.6)×100. Assuming that the gas other than the air is carbon dioxide, the carbon dioxide concentration (H%) in the container is defined as the formula: 100-G.

[0171] [Calculation method of the volume inside the package based on the surface area inside the package]

[0172] In this specification, the volume calculated based on the inner surface area of ​​the package body means that the volume of the cube obtained based on the inner surface area is defined as its volume. That is, the surface area S of the cube is 6 times the square of X when one side is X cm, and the volume is the cube of X. Therefore, assuming that the volume = the volume, the volume is calculated by (S / 6) to the power of 3 / 2.

[0173] <Step (3)>

[0174] The hydrogel article sealed in the package was left in an environment of 25° C. for 120 hours to crosslink the hydrogel until the loss tangent of the hydrogel reached 0.30. In this way, the intended hydrogel article containing carbon dioxide was obtained.

[0175] [Example 2]

[0176] In step (1), 1.5 g of aluminum hydroxide was used as a crosslinking agent, and in step (3), crosslinking was performed at 50° C. Except for this, the same operation as in Example 1 was performed to obtain a water-containing gel article containing carbon dioxide gas.

[0177] [Example 3]

[0178] In step (1), 10.0 g of tartaric acid was used instead of succinic acid, 50.0 g of glycerol was used, 30.0 g of sodium carboxymethylcellulose, 30.0 g of polyacrylic acid, and 20.0 g of sodium polyacrylate were used as water-soluble polymers, and polyvinyl alcohol was not contained.

[0179] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0180] [Example 4]

[0181] In step (2), the concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article is sealed is set to 61%. In step (3), the hydrogel is crosslinked until the loss tangent of the hydrogel reaches 0.29.

[0182] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0183] [Example 5]

[0184] In step (2), the concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article is sealed is set to 31%. In step (3), the hydrogel is crosslinked until the loss tangent of the hydrogel becomes 0.28.

[0185] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0186] [Example 6]

[0187] In step (2), the concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article is sealed is set to 15%. In step (3), the hydrogel is cross-linked until the loss tangent of the hydrogel reaches 0.28.

[0188] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0189] [Example 7]

[0190] In step (1), 0.4 g of magnesium aluminum silicate and 0.1 g of aluminum hydroxide were used as crosslinking agents. In step (2), when the loss tangent (1 Hz) of the hydrogel in the hydrogel article was 0.58, two punched hydrogel articles were sealed in a package. In step (3), the hydrogel was crosslinked until the loss tangent of the hydrogel became 0.31.

[0191] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0192] [Example 8]

[0193] In step (1), 0.4 g of magnesium aluminum silicate and 0.01 g of aluminum hydroxide were used as crosslinking agents.

[0194] Except for these, the same operation as in Example 7 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0195] [Example 9]

[0196] In step (1), 0.3 g of magnesium aluminum silicate and 0.1 g of aluminum hydroxide were used as crosslinking agents. In step (2), when the loss tangent (1 Hz) of the hydrogel in the hydrogel article reached 0.62, two punched hydrogel articles were sealed in a package. In step (3), the hydrogel was crosslinked until the loss tangent of the hydrogel reached 0.43.

[0197] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0198] [Example 10]

[0199] In step (2), when the loss tangent (1 Hz) of the hydrogel in the hydrogel article reaches 0.49, the two punched hydrogel articles are sealed in a package. In step (3), the hydrogel is crosslinked until the loss tangent of the hydrogel reaches 0.42.

[0200] Except for these, the same operation as in Example 9 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0201] [Comparative Example 1]

[0202] In step (2), the concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article is sealed is set to 6%. In step (3), the hydrogel is cross-linked until the loss tangent of the hydrogel reaches 0.28.

[0203] Except for these, the same operation as in Example 1 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0204] [Comparative Example 2]

[0205] In step (1), 1.5 g of aluminum hydroxide was used as a crosslinking agent, and the mixture was aged at 50° C. for 2 days until the loss tangent of the hydrogel reached 0.26, and then carbon dioxide gas was added. Therefore, step (3) was not performed in this comparative example. Except for these, the same operation as in Example 1 was performed to obtain a hydrogel article containing carbon dioxide gas.

[0206] [Comparative Example 3]

[0207] In step (1), 0.5 g of magnesium aluminum silicate was used as a crosslinking agent, and the hydrogel was aged at 50°C for 2 days until the loss tangent of the hydrogel reached 0.31, and then filled with carbon dioxide gas. The concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article was sealed was set to 61%.

[0208] Except for these, the same operation as in Comparative Example 2 was carried out to obtain a water-containing gel article containing carbon dioxide gas.

[0209] [Comparative Example 4]

[0210] The concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article was sealed was set to 31%. The same operation as in Comparative Example 2 was performed except for this, to obtain a hydrogel article containing carbon dioxide gas.

[0211] [Comparative Example 5]

[0212] The concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article was sealed was set to 15%. The same operation as in Comparative Example 2 was performed except for this, to obtain a hydrogel article containing carbon dioxide gas.

[0213] [Comparative Example 6]

[0214] The concentration of carbon dioxide gas in the surrounding atmosphere when the hydrogel article was sealed was set to 6%. The same operation as in Comparative Example 2 was performed except for this, thereby obtaining a hydrogel article containing carbon dioxide gas.

[0215] [evaluate]

[0216] For the hydrogel articles containing carbon dioxide obtained in the examples and comparative examples, the carbon dioxide concentration in the hydrogel was measured by the following method. In addition, the daily output of the hydrogel articles containing carbon dioxide in the examples and comparative examples was measured. There is no particular limitation on the supply amount of the hydrogel, and in this evaluation, the total supply amount of the gel in each example is fixed at 3000 kg. In addition, for the hydrogel articles containing carbon dioxide obtained in the examples and comparative examples, the bubble rate and the ratio of the total area occupied by bubbles with a hypothetical diameter of 5 mm or more to 100% of the surface area of ​​the hydrogel articles containing carbon dioxide were measured. In addition, for the hydrogel articles containing carbon dioxide obtained in the examples and comparative examples, the adhesiveness of the articles was measured and evaluated by the following method. These results are shown in the following Tables 1 and 2.

[0217] In addition, when the daily production of the hydrogel article containing carbon dioxide is 15,000 or more, it can be determined that the hydrogel article containing carbon dioxide can be produced sufficiently efficiently. In addition, when the concentration of carbon dioxide in the hydrogel is 250 ppm or more, it can be determined that the hydrogel article containing carbon dioxide has a blood circulation promoting effect.

[0218] [Measurement of Carbon Dioxide Concentration]

[0219] The concentration of carbon dioxide in the hydrogel article containing carbon dioxide is measured immediately after the package is opened. Specifically, first, the hydrogel article containing carbon dioxide is immersed in a covered bottle filled with an alkaline solution to dissolve the gel and convert the carbon dioxide into carbonate. Next, the acidic state is restored using an acidic buffer solution (pH 4.5), and the concentration of the generated carbon dioxide is measured using a carbon dioxide electrode (CE-2041; manufactured by DKK East Asia Co., Ltd.). Based on the obtained carbon dioxide concentration, the concentration of carbon dioxide in the hydrogel article containing carbon dioxide is calculated. The value of the carbon dioxide concentration can be used as an evaluation index of the carbon dioxide retention of the obtained hydrogel article containing carbon dioxide.

[0220] [Evaluation of Adhesiveness of Hydrogel Articles Containing Carbon Dioxide]

[0221] The package containing the hydrogel article containing carbon dioxide was opened, the article was taken out, and then the article was quickly attached to the calf of a professional functional tester, who performed plantar flexion and dorsiflexion exercises 10 times.

[0222] Next, the area of ​​the portion of the hydrogel article containing carbon dioxide gas attached to the calf that bulges out from the calf, that is, the area of ​​the portion that has peeled off from the calf, is measured. Then, the ratio (%) of the area of ​​the peeled off portion to the total area of ​​the hydrogel article containing carbon dioxide gas is calculated. The obtained ratio is evaluated according to the following criteria as an evaluation index of the adhesion of the hydrogel article containing carbon dioxide gas. In addition, the higher the evaluation value, the better the adhesion. When the adhesion is excellent, it can be said that the adhesion and tracking properties are also excellent.

[0223] <Evaluation criteria for adhesiveness>

[0224] 6: The area ratio of the peeled portion is more than 0% and is 10% or less.

[0225] 5: The area ratio of the peeled portion is more than 10% and less than 20%.

[0226] 4: The area ratio of the peeled portion is more than 20% and less than 30%.

[0227] 3: The area ratio of the peeled portion is more than 30% and not more than 40%.

[0228] 2: The area ratio of the peeled portion is more than 40% and less than 50%.

[0229] 1: The area ratio of the peeled portion exceeds 50%.

[0230]

[0231] [Table 2]

[0232]

[0233] From the results shown in Tables 1 and 2, it can be seen that the target object can be produced with good productivity by adopting the present production method as compared with the method of the comparative example.

[0234] Furthermore, it was found that, by adopting the present production method, a target product having a higher carbon dioxide gas retention property can be obtained compared with the comparative example.

[0235] [Industrial Applicability]

[0236] According to the present invention, a hydrogel article having high carbon dioxide gas retention capacity in the hydrogel can be produced with good productivity.

Claims

1. A method for producing a hydrogel article containing carbon dioxide, wherein: The process comprises the following steps (1) to (3): (1) a step of preparing an article containing a hydrogel, wherein the hydrogel contains (A) a water-soluble polymer, (B) a cross-linking agent for the water-soluble polymer, and (C) water, and wherein the loss tangent of the hydrogel at 1 Hz in a dynamic viscoelasticity measurement is 0.46 or more; (2) when the loss tangent of the hydrogel in the hydrogel-containing article at 1 Hz in a dynamic viscoelasticity measurement is 0.46 or more, the composition of the surrounding gas atmosphere of the hydrogel-containing article is adjusted so that the concentration of carbon dioxide gas in the surrounding gas atmosphere becomes 10% by volume or more, and the hydrogel-containing article is sealed in a package; (3) cross-linking the hydrogel until the loss tangent of the hydrogel in the hydrogel-containing article at 1 Hz in a dynamic viscoelasticity measurement is less than 0.46, thereby obtaining a hydrogel article containing carbon dioxide sealed in the package. The water-soluble polymer is an anionic polymer. The crosslinking agent is a metal ion compound, a cationic polymer or a multifunctional epoxy compound.

2. The manufacturing method according to claim 1, wherein: The step (2) is carried out at room temperature and atmospheric pressure.

3. The manufacturing method according to claim 1, wherein: The crosslinking agent contains aluminum ions to supply the crosslinking agent.

4. The production method according to any one of claims 1 to 3, wherein: Step (2) comprises: A first joining step of placing the hydrogel-containing article between a first air-impermeable sheet and a second air-impermeable sheet and supplying a gas containing carbon dioxide between the two sheets, and joining both sides of the two sheets along a conveying direction; A second joining step of joining the two original sheets in a direction intersecting the conveying direction at a position where the hydrogel article is not present, to form a continuous package body enclosing the hydrogel article and the gas containing carbon dioxide; and The cutting step is to cut the package body continuous body in a direction intersecting the conveying direction at the portion joined in the second joining step to form the package body.

5. The production method according to any one of claims 1 to 3, wherein: In step (2), when the loss tangent is 0.48 or more and 0.90 or less, the composition of the surrounding atmosphere is adjusted so that the concentration of carbon dioxide gas in the surrounding atmosphere of the article containing the hydrogel becomes 10% by volume or more.

6. The production method according to any one of claims 1 to 3, wherein: The step (1) includes a step of mixing the water-soluble polymer, the crosslinking agent, and the water under atmospheric pressure to prepare the water-containing gel containing bubbles.

7. The production method according to any one of claims 1 to 3, wherein: In step (2), when the loss tangent is 0.46 or more, the composition of the surrounding atmosphere is adjusted so that the concentration of carbon dioxide gas in the surrounding atmosphere of the article containing the hydrogel becomes 30% by volume or more.

8. The production method according to any one of claims 1 to 3, wherein: Step (2) is performed by placing the article containing the hydrogel in the package and supplying the gas containing carbon dioxide into the package in this order, in the reverse order, or simultaneously, and then sealing the package.

9. The production method according to any one of claims 1 to 3, wherein: In step (3), the hydrogel is cross-linked until the loss tangent is less than 0.40, thereby obtaining a hydrogel article containing carbon dioxide gas sealed in the package.

10. The production method according to any one of claims 1 to 3, wherein: The step (3) is carried out at room temperature. In step (3), the time until the loss tangent becomes less than 0.46 is 24 hours to 366 hours from the time the water-containing gel article is sealed.

11. The production method according to any one of claims 1 to 3, wherein: In step (3), crosslinking of the hydrogel is performed until the loss tangent becomes 0.20 or more and 0.45 or less.

12. The production method according to any one of claims 1 to 3, wherein: Step (1) comprises the step of applying the obtained hydrogel onto a support to form an article containing the hydrogel on the support.

13. The manufacturing method according to claim 12, wherein: In the step of forming the hydrogel-containing article on the support, the hydrogel is applied so that the thickness of the hydrogel in the hydrogel-containing carbon dioxide gas article is 0.5 mm to 5 mm.

14. The production method according to any one of claims 1 to 3, wherein: In the step (1), the time for mixing the water-soluble polymer, the crosslinking agent, and the water is from 1 minute to 60 minutes.

15. The production method according to any one of claims 1 to 3, wherein: In the step (1), the stirring speed when the water-soluble polymer, the cross-linking agent, and the water are mixed is 10 rpm to 80 rpm.

16. The manufacturing method according to claim 1, wherein: The anionic polymer is a polymer having a carboxyl group, a sulfate group, or a phosphoric acid group.

17. The manufacturing method according to claim 1, wherein: The anionic polymer is one or more selected from poly(meth)acrylic acid and salts thereof, carboxyvinyl polymer and salts thereof, anionic cellulose derivatives and salts thereof, carrageenan, alginic acid and salts thereof, and anionic starch derivatives.

18. The manufacturing method according to claim 1, wherein: The cross-linking agent is a metal ion compound, The metal ion compound is an oxide, a hydroxide, or a salt containing aluminum, magnesium, calcium, or potassium.

19. The manufacturing method according to claim 18, wherein: The metal ion compound is one or more selected from aluminum hydroxide, potassium aluminum sulfate, aluminum sulfate, aluminum oxide, aluminum glycinate, aluminum acetate, aluminum lactate, aluminum stearate, hydrated aluminum silicate, aluminum metasilicate, magnesium aluminum silicate, magnesium chloride, magnesium stearate, calcium carbonate, calcium hydroxide, kaolin, synthetic aluminum carbonate, and potassium hydroxide.

20. The manufacturing method according to claim 19, wherein: The metal ion compound is magnesium aluminum silicate.

21. The manufacturing method according to claim 20, wherein: The ratio of aluminum magnesium silicate in the cross-linking agent is 30 mass % or more and 100 mass % or less.

22. The production method according to any one of claims 1 to 3, wherein: The amount of the cross-linking agent added to the hydrogel is 0.01% by mass or more and 10% by mass or less.

23. The production method according to any one of claims 1 to 3, wherein: The amount of water added to the water-containing gel is 20 mass % or more and 95 mass % or less.

Citation Information

Patent Citations

  • Coating composition and coating product using the coating composition

    JP2014062087A

  • Body cosmetic

    US20200100991A1

  • Sheet preparation to be applied to the human body

    CN101903019A

  • Hydrogel composition

    CN107106418A