A morphology-controllable molybdenum disulfide nanomaterial and its preparation method and application
By controlling the morphology of the zinc sulfide hard template through the cation exchange method, the morphology of molybdenum disulfide nanomaterials can be controlled and prepared, which solves the problems of high temperature pressure control and "three wastes" emissions in the existing technology, and realizes efficient and environmentally friendly industrial production. and widely used.
Patent Information
- Application Number
- CN202211137312.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-19
AI Technical Summary
When preparing molybdenum disulfide nanomaterials in the existing technology, the solvothermal method requires high temperature and pressure control, has a long reaction cycle and pollutes the environment, and the chemical vapor deposition method has a high reaction temperature and produces "three wastes", which is not suitable for industrial production.
The cation exchange method is used to control the morphology of the zinc sulfide hard template through the reaction of zinc sulfide and molybdenum salts, achieving controllable preparation of molybdenum disulfide morphology, adjustable calcination temperature and time, avoiding the emission of "three wastes", and low equipment requirements.
Efficient preparation of molybdenum disulfide nanomaterials with controllable morphology has been achieved, simplifying the process, reducing costs, and is suitable for large-scale industrial production. The material has a high specific surface area and multiple active sites, and is suitable for cocatalysts and n-type semiconductor materials, improving Improved photoelectric detection performance.
Smart Images

Figure CN115347083B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material synthesis, and specifically relates to a morphology-controllable molybdenum disulfide nano material and a preparation method and application thereof. Background Art
[0002] Molybdenum disulfide (MoS2), as a transition metal dichalcogenide (TMDCs), is a new type of two-dimensional direct bandgap semiconductor material with broad application prospects. Molybdenum disulfide is a hexagonal crystal with a direct bandgap of 1.2 to 1.8 eV and a S-Mo-S "sandwich" structure. MoS2 has significant properties such as direct bandgap, strong light-matter interaction and high carrier mobility, and has broad application prospects in transistors, integrated circuits and photodetectors. Studies have found that the morphology of the material has a certain degree of influence on its performance, and MoS2 exhibits different crystal forms due to differences in morphology. MoS2 nanomaterials with different morphologies have been developed one after another, and their application range is relatively wide.
[0003] At present, the main methods for preparing MoS2 nanomaterials include solvent thermal method, chemical vapor deposition method, etc., and the most common method for preparing molybdenum disulfide of different morphologies is to carry out solvent thermal treatment in a sulfur-containing compound solution (such as CN106379939 A). However, the solvent thermal method involves the regulation of temperature and pressure, has high requirements on equipment, has a long reaction period, and does not utilize industrial production. Chemical vapor deposition method is to place a molybdenum source and a sulfur source in an ark, and place the ark in the middle of a tubular furnace, and after vacuuming, prepare different morphologies of molybdenum disulfide at high temperature under argon protection (CN 110835747 B). However, the chemical vapor deposition method has a high reaction temperature, requires inert gas protection, and the reaction product pollutes the environment, damages human health, and brings difficulties to the treatment of three wastes. Summary of the invention
[0004] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a morphology-controllable molybdenum disulfide nanomaterial and its preparation method and application, which are simple to operate, mild reaction conditions, short reaction cycle, no "three wastes" are discharged during the preparation process, and are easy to be mass-produced industrially.
[0005] The present invention is achieved through the following technical solutions:
[0006] The invention discloses a method for preparing a morphology-controllable molybdenum disulfide nanomaterial, comprising the following steps:
[0007] Step 1: using a cation exchange method to react zinc sulfide of a specific morphology with a molybdenum salt to obtain a precursor;
[0008] Step 2: calcining the precursor obtained in step 1 to obtain a molybdenum disulfide nanomaterial having the same morphology as zinc sulfide.
[0009] Preferably, in step 1, the molar ratio of zinc sulfide to molybdenum salt is 1-10.
[0010] Preferably, in step 1, the zinc sulfide with a specific morphology is zinc sulfide nanoparticles, zinc sulfide nanorods, zinc sulfide nanospheres, zinc sulfide nanotubes or zinc sulfide nanobelts.
[0011] Preferably, in step 1, the molybdenum salt is one or more of ammonium molybdate, sodium molybdate, molybdenum trichloride and molybdenum pentachloride.
[0012] Preferably, step 1 is specifically as follows: adding zinc sulfide and molybdenum salt of specific morphology into ethylene glycol until they are completely immersed, stirring continuously for 6 to 24 hours, and then centrifuging, washing and drying to obtain a precursor.
[0013] Preferably, in step 2, the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 6 hours.
[0014] The invention also discloses a morphology-controllable molybdenum disulfide nanomaterial prepared by the preparation method. The molybdenum disulfide nanomaterial is molybdenum disulfide nanoparticles, molybdenum disulfide nanorods, molybdenum disulfide nanospheres, molybdenum disulfide nanotubes or molybdenum disulfide nanobelts.
[0015] The invention also discloses the application of the above-mentioned morphology-controllable molybdenum disulfide nanomaterial as a co-catalyst and an n-type semiconductor material.
[0016] Compared with the prior art, the present invention has the following beneficial technical effects:
[0017] The preparation method of the morphology-controllable molybdenum disulfide nanomaterial of the present invention utilizes a cation exchange method, and in the process of controlling the morphology reaction of a zinc sulfide hard template, the zinc sulfide hard template is used as a sacrificial template, and molybdenum disulfide grows from the inside to the outside along with the morphology of the hard template until the reaction is completed, thereby realizing precise control of the morphology of a two-dimensional MoS2 sample. The present invention has a simple process, simple operation, and low raw material production cost. Compared with the currently common solvothermal method and chemical vapor deposition method for preparing molybdenum disulfide nanomaterials, the present invention has low equipment requirements, short reaction cycle, no need to control temperature and pressure, and no "three wastes" are discharged during the preparation process. It is a green synthesis method that is easy to be industrialized on a large scale.
[0018] Furthermore, the molybdenum salts are ammonium molybdate, sodium molybdate, molybdenum trichloride, and molybdenum pentachloride, which have low toxicity, high specific surface area, multiple active sites, and high selectivity.
[0019] Furthermore, the calcination temperature is 200 to 1000° C. and the calcination time is 2 to 6 hours, which can make the prepared molybdenum disulfide nanomaterial crystal more stable.
[0020] The morphology-controllable molybdenum disulfide nanomaterial prepared by the preparation method disclosed in the present invention can flexibly select the use path of the material by adjusting the morphology of molybdenum disulfide.
[0021] The above-mentioned morphology-controllable molybdenum disulfide nanomaterial disclosed in the present invention is used as a co-catalyst and n-type semiconductor material. According to the different morphologies of the materials, it has different characteristics in application. The nanoparticles have high activity and selectivity in catalytic oxidation and reduction reactions. The nanorod and nanobelt structures have good structural stability, extend the diffusion path of photogenerated carriers, and suppress the recombination rate of photogenerated electron-hole pairs. The nanotube and nanosphere have a higher specific surface area, which can generate multiple reflections of photogenerated carriers in the cavity for the incident light, so that the light energy can be reused, thereby greatly enhancing the light collection ability and greatly improving the light energy utilization rate. Therefore, the morphology-controllable molybdenum disulfide nanomaterial has extremely wide applications in the field of catalysis, especially in the field of photoelectric detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The X-ray powder diffraction pattern (XRD) of the MoS2 nanorod powder prepared in Example 1 of the present invention;
[0023] Figure 2 This is a scanning electron microscope photo (SEM) of the MoS2 nanorod powder prepared in Example 1 of the present invention;
[0024] Figure 3 The X-ray powder diffraction pattern (XRD) of the MoS2 nanoparticle powder prepared in Example 2 of the present invention;
[0025] Figure 4 This is a scanning electron microscope photograph (SEM) of the MoS2 nanoparticle powder prepared in Example 2 of the present invention;
[0026] Figure 5 The X-ray powder diffraction pattern (XRD) of the MoS2 nanotube powder prepared in Example 3 of the present invention;
[0027] Figure 6 This is a scanning electron microscope photo (SEM) of the MoS2 nanotube powder prepared in Example 3 of the present invention;
[0028] Figure 7 The X-ray powder diffraction pattern (XRD) of the MoS2 nanosphere powder prepared in Example 4 of the present invention;
[0029] Figure 8 This is a scanning electron microscope photo (SEM) of the MoS2 nanosphere powder prepared in Example 4 of the present invention;
[0030] Fig. 9The X-ray powder diffraction pattern (XRD) of the MoS2 nanobelt powder prepared in Example 5 of the present invention;
[0031] Fig.10 This is a scanning electron microscope photograph (SEM) of the MoS2 nanobelt powder prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, which are intended to explain the present invention rather than to limit it.
[0033] Example 1
[0034] 0.5 mol of zinc sulfide nanorods and 0.5 mol of ammonium molybdate were added to 100 mL of ethylene glycol and stirred for 6 hours. After the reaction, the mixture was washed by centrifugation with anhydrous ethanol and deionized water, and dried to obtain a precursor powder. The precursor powder was calcined at 200 °C for 2 hours to obtain Figure 2 The morphology and structure shown are rod-shaped brown-black powders of molybdenum disulfide.
[0035] Example 2
[0036] 0.5 mol of zinc sulfide nanoparticles and 1.5 mol of sodium molybdate were added to 100 mL of ethylene glycol and stirred for 12 hours. After the reaction, the mixture was washed by centrifugation with anhydrous ethanol and deionized water, and dried to obtain a precursor powder. The precursor powder was calcined at 400 °C for 3 hours to obtain Figure 4 The morphology and structure shown are granular molybdenum disulfide brown-black powder.
[0037] Example 3
[0038] 0.5 mol of zinc sulfide nanotubes and 3.5 mol of molybdenum trichloride were added to 100 mL of ethylene glycol and stirred for 18 hours. After the reaction, the precursor powder was washed by centrifugation with anhydrous ethanol and deionized water, and dried to obtain a precursor powder. The precursor powder was calcined at 600 ° C for 4 hours to obtain Figure 6 The morphology shown is tubular molybdenum disulfide brown-black powder.
[0039] Example 4
[0040] 0.5 mol of zinc sulfide nanospheres and 5 mol of molybdenum pentachloride were added to 100 mL of ethylene glycol and stirred for 20 hours. After the reaction, the precursor powder was washed by centrifugation with anhydrous ethanol and deionized water, and dried to obtain a precursor powder. The precursor powder was calcined at 800 ° C for 5 hours to obtain Figure 8 The morphology and structure shown are spherical molybdenum disulfide brown-black powder.
[0041] Example 5
[0042] 0.5 mol of zinc sulfide nanobelt, 0.75 mol of ammonium molybdate and 0.75 mol of sodium molybdate were added to 100 mL of ethylene glycol and stirred for 24 hours. After the reaction, the precursor powder was washed by centrifugation with anhydrous ethanol and deionized water, and dried to obtain a precursor powder. The precursor powder was calcined at 1000 ° C for 6 hours to obtain Fig.10 The morphology shown is a ribbon-shaped brown-black powder of molybdenum disulfide.
[0043] Figure 1 , Figure 3 , Figure 5 , Figure 7 and Fig. 9 They are the XRD patterns of the product samples obtained in Examples 1 to 5, respectively. Each sample has diffraction peaks at around 14.1°, 33.5°, 39.6° and 59.1°, corresponding to the (002), (100), (101), (103) and (110) crystal planes of molybdenum disulfide, respectively, which are consistent with the standard spectrum of 2H-type MoS2 (PDF#37-1492), indicating that molybdenum disulfide has been successfully prepared.
[0044] Figure 2 , Figure 4 , Figure 6 , Figure 8 and Fig.10 The scanning electron microscope images of MoS2 samples prepared in Examples 1 to 5 correspond to the prepared molybdenum disulfide with different morphologies. Among them, the molybdenum disulfide powder prepared in Example 1 is rod-shaped, Example 2 is granular, Example 3 is tubular, Example 4 is powder, and Example 5 is ribbon-shaped, indicating that the preparation method of the present invention can accurately control the morphology of the molybdenum disulfide material.
[0045] It should be noted that the above is only a part of the implementation of the present invention, and equivalent changes made to the system described in the present invention are all included in the protection scope of the present invention. Those skilled in the art of the present invention can replace the specific examples described in a similar manner, as long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they all belong to the protection scope of the present invention.
Claims
1. A method for preparing a morphology-controllable molybdenum disulfide nanomaterial, characterized in that: The following steps are involved: Step 1: Using a cation exchange method, zinc sulfide and molybdenum salt with specific morphology are added to ethylene glycol until they are completely immersed, and stirred for 6 to 24 hours, and then centrifuged, washed and dried to obtain a precursor; Step 2: calcining the precursor obtained in step 1 at a temperature of 200-1000° C. for 2-6 hours to obtain a molybdenum disulfide nanomaterial having the same morphology as zinc sulfide; In step 1, the molar ratio of zinc sulfide to molybdenum salt is 1-10.
2. The method for preparing the morphology-controllable molybdenum disulfide nanomaterial according to claim 1, characterized in that: In step 1, the zinc sulfide with a specific morphology is zinc sulfide nanoparticles.
3. The method for preparing the morphology-controlled molybdenum disulfide nanomaterial according to claim 2, characterized in that: The zinc sulfide nanoparticles are zinc sulfide nanorods, zinc sulfide nanospheres, zinc sulfide nanotubes or zinc sulfide nanobelts.
4. The method for preparing the morphology-controllable molybdenum disulfide nanomaterial according to claim 1, characterized in that: In step 1, the molybdenum salt is one or more of ammonium molybdate, sodium molybdate, molybdenum trichloride and molybdenum pentachloride.
5. The morphology-controllable molybdenum disulfide nanomaterial obtained by the preparation method according to any one of claims 1 to 4, characterized in that: Molybdenum disulfide nanomaterial is molybdenum disulfide nanoparticles.
6. The morphology-controllable molybdenum disulfide nanomaterial prepared by the preparation method according to any one of claim 5, characterized in that: The molybdenum disulfide nanoparticles are molybdenum disulfide nanorods, molybdenum disulfide nanospheres, molybdenum disulfide nanotubes or molybdenum disulfide nanobelts.
7. Use of the morphology-controllable molybdenum disulfide nanomaterial according to claim 5 as a co-catalyst and n-type semiconductor material.
Citation Information
Patent Citations
Morphology-adjustable molybdenum disulfide preparation method
CN106379939A
A method for temperature-controlled morphology and defects of molybdenum disulfide
CN110835747B
Method for preparing non-crystal molybdemum sulfide nano powder
CN101024517A