A method for removing sulfate and chloride impurities from rare earth oxides using a two-stage anion exchange resin
Through the two-stage anion exchange resin and oxalic acid precipitation process, sulfate and chloride ions in rare earth oxides were successfully removed, solving the problem of difficult removal of impurities and difficult to meet the purity standards in the prior art, and achieving efficient and low-cost rare earth oxide purification .
Patent Information
- Application Number
- CN202210936648.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-08-05
AI Technical Summary
The prior art is difficult to effectively remove sulfate and chloride ion impurities in rare earth oxides, making it difficult for the purity of rare earth products to meet high standards, and new impurities are easily introduced during the treatment process, increasing production costs and waste liquid volume.
Using two-stage anion exchange resin, firstly use polystyrene-based large-pore strong alkali anion exchange resin to remove sulfate, then use polyacrylic gel weak alkali anion exchange resin to remove chloride ions, through multi-step ion exchange and oxalic acid precipitation, etc. Process, the content of sulfate and chloride ions in rare earth oxides is lower than the national standard detection limit.
It significantly reduces production costs, improves rare earth recovery rate, avoids resource waste, ensures high purity of rare earth oxides, overcomes the long cycle and high cost problems of pure oxalate precipitation method, and meets the needs of high-purity rare earth products. .
Smart Images

Figure CN115367783B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth material purification, and particularly relates to a method for removing sulfate and chloride ion impurities in rare earth oxides by using a two-stage anion exchange resin. Background Art
[0002] Rare earth materials are key raw materials that are indispensable for the development of high-tech and cutting-edge defense technologies. They are known as "industrial MSG", "industrial vitamins" and "the mother of new materials" and are precious strategic metal resources. Due to their great effects and small usage, rare earths have become an important element for improving product structure, increasing scientific and technological content and promoting technological progress in the industry. They are widely used in metallurgy, military, petrochemicals, glass ceramics, agriculture and new materials. At the same time, with the application needs of magnetic materials, luminescent materials, catalysis, hydrogen storage, ceramic materials, and especially the development of high-end applications such as optical functional crystals, electronic ceramics, and high-purity rare earth coating materials, the demand for high-purity rare earths will increase. High performance, high purity and the development of new applications are the development trends of rare earth materials.
[0003] With the development of science and technology, new rare earth materials emerge in an endless stream, and higher requirements are put forward for the relevant detection indicators of rare earths. The current product standards of 15 types of rare earth oxides clearly stipulate the content of chlorine, among which the current product standards of 6 kinds of rare earth oxides: "GB / T 4154-2015 Lanthanum Oxide", "GB / T 4155-2015 Cerium Oxide", "GB / T5239-2015 Praseodymium Oxide", "GB / T5240-2015 Neodymium Oxide", "GB / T13558-2019 Dysprosium Oxide", "XB / T201-2016 Holmium Oxide" also require the content of sulfate.
[0004] When the sulfate content in rare earth products is high, cyclohexane acid is generally used to extract rare earths to separate them from sulfates, or barium chloride precipitation is used to remove sulfates. In this process, new impurity elements are easily introduced. In order to control the chlorine content in rare earth products and produce rare earth oxides of higher purity, oxalic acid precipitation is generally used to convert them into rare earth oxalates in neutral or weakly acidic solutions, and then the insolubility of rare earth oxalates is used to separate them from soluble chloride ions. This treatment method is completed through dissolution, precipitation, washing, sedimentation, calcination and other operating steps. During the treatment process, large pieces of rare earth oxalate precipitates are prone to entrain chloride ions, and it cannot be guaranteed that the chloride ions in the final calcined rare earth are completely removed. For this reason, it is necessary to continue to study the removal methods and equipment of sulfate and chloride ions in rare earth oxides to improve the quality of rare earth products and meet actual production needs. Summary of the invention
[0005] The object of the present invention is to provide a method for removing sulfate and chloride impurities in rare earth oxides by a two-stage anion exchange resin. The specific technical scheme is as follows:
[0006] A method for removing sulfate and chloride impurities in rare earth oxides by using two-stage anion exchange resins comprises the steps of sequentially treating rare earth oxide ion exchange stock solution with polystyrene macroporous strong base anion exchange resin and polyacrylic acid gel weak base anion exchange resin, wherein the mass percentage of sulfate ions in the treated rare earth oxides is less than 0.025%, and the mass percentage of chloride ions is less than 0.005%.
[0007] Furthermore, the polystyrene-based macroporous strong-base anion exchange resin and the polyacrylic acid-based gel weak-base anion exchange resin are both loaded into two ion exchange columns connected end to end;
[0008] And / or, the particle size of the polystyrene-based macroporous strong base anion exchange resin is 0.560-0.780 mm, and the ion exchange capacity is >1.0 eq / L; the particle size of the polyacrylic acid-based gel weak base anion exchange resin is 0.540-0.730 mm, and the ion exchange capacity is >1.6 eq / L.
[0009] Furthermore, the polystyrene-based macroporous strong base anion exchange resin is converted into an OH-type ion exchange resin after pretreatment and then loaded into the first ion exchange column and the second ion exchange column connected end to end, respectively; the polyacrylic acid-based gel weak base anion exchange resin is converted into an acetate-type ion exchange resin after pretreatment and then loaded into the third ion exchange column and the fourth ion exchange column connected end to end; the first ion exchange column and the third ion exchange column are placed at 20 to 65° C., preferably 40 to 60° C.; the second ion exchange column and the fourth ion exchange column are placed at room temperature, such as 20 to 30° C.
[0010] Furthermore, the polystyrene-based macroporous strong base anion exchange resin is converted into an OH-type ion exchange resin after water washing, alkali washing, acid washing, and alkali washing, and the polyacrylic acid-based gel weak base anion exchange resin is converted into an acetate-type ion exchange resin after water washing and acid washing.
[0011] Furthermore, the rare earth oxide ion filtrate treated with the polystyrene macroporous strong base anion exchange resin is detected by barium chloride turbidimetry until sulfate cannot be detected, and then the filtrate is treated with the polyacrylic acid gel weak base anion exchange resin.
[0012] Furthermore, the first ion exchange column and the third ion exchange column have a column length of 35 to 45 cm, a diameter to column length ratio of 1:20 to 1:30, and are filled with more than 30 mL of wet resin; the second ion exchange column and the fourth ion exchange column have a column length of 15 to 25 cm, a diameter to column length ratio of 1:20 to 1:30, and are filled with more than 15 mL of wet resin.
[0013] Furthermore, the volume ratio of the rare earth oxide ion exchange stock solution to the resin is 10:1 to 100:1.
[0014] Furthermore, the rare earth oxide ion exchange stock solution is a rare earth oxide nitric acid solution obtained by dissolving rare earth oxide in nitric acid, the rare earth ion concentration in the rare earth oxide ion exchange stock solution is 20-50 mg / mL, the volume concentration of nitric acid is 5%-20%, and the volume concentration of nitric acid is preferably 5%-10%.
[0015] Furthermore, the mass percentage of sulfate in the rare earth oxide is ≤2%, and the mass percentage of chloride ion is ≤1%;
[0016] And / or, the rare earth oxide includes one or more of lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, scandium oxide, yttrium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide.
[0017] Furthermore, the method also includes a step of treating with oxalic acid; further, after treating the rare earth oxide ion exchange stock solution with two-stage anion exchange resin, oxalic acid is used for precipitation, filtration, drying and calcination to obtain rare earth oxides with a sulfate ion mass percentage of less than 0.025% and a chloride ion mass percentage of less than 0.005%.
[0018] Furthermore, the first ion exchange column or the third ion exchange column is placed in a liquid heat device for heating, the inlet of the first ion exchange column is connected to a liquid inlet pipe located outside the liquid heat device, the outlet of the first ion exchange column is connected to a liquid outlet pipe located outside the liquid heat device, and the liquid outlet pipe is connected to the second ion exchange column;
[0019] The inlet of the third ion exchange column is connected to the liquid inlet pipe outside the liquid thermal device, the outlet of the third ion exchange column is connected to one end of the liquid outlet pipe outside the liquid thermal device, and the other end of the liquid outlet pipe is connected to the fourth ion exchange column.
[0020] Furthermore, the liquid thermal device comprises a heating container, the heating container contains liquid, a heating rod, a thermocouple and an ion exchange column, the heating container has an external temperature acquirer and a heating controller, and the ion exchange column is a first ion exchange column or a third ion exchange column.
[0021] Furthermore, an insulation layer is provided outside the heating container; a thermocouple is connected to a temperature acquirer for measuring the temperature of the liquid; a heating rod is connected to a heating controller for controlling the heating temperature of the liquid; and / or the ion exchange column is fixed by an ion exchange column bracket.
[0022] The beneficial effects of the present invention are:
[0023] (1) The method of the present invention has simple operation steps, high yield, small amount of reagents used, and small amount of experimental waste liquid generated, which can significantly reduce production costs, is economical and efficient, and is easy to promote industrially; the rare earth recovery rate after treatment by the method of the present invention is high, and the resin product can be recycled, which can effectively avoid waste of resources.
[0024] (2) The mass percentage of sulfate in the rare earth oxide treated by the method of the present invention is less than 0.025%, and the mass percentage of chloride ion is less than 0.005%, both of which are lower than the detection limit of the current national standard method; the problem that sulfate in rare earth products is easily introduced into other impurity ions by the extraction process or precipitation process is overcome, and the problem that the simple oxalate precipitation rare earth dechlorination method has a long cycle, a large amount of waste liquid to be treated, a high cost, and a low yield is solved.
[0025] (3) The liquid thermal device provided by the present invention fully considers the applicability of the device and can perform heating treatment on preparative chromatographic columns of different sizes. The device has low energy consumption, reduces the actual operation cost, and the device can meet the accuracy requirements for temperature control. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the ion exchange treatment equipment of the present invention;
[0027] Figure 2 It is a schematic diagram of the composition of the liquid heat device in the ion exchange treatment equipment of the present invention.
[0028] Explanation of reference numerals: 1-high-pressure constant-current sampling pump; 2-liquid inlet pipe; 3-first waterproof fixed joint; 4-liquid heating device; 5-fixed joint; 6-second ion exchange column; 40-heating container; 41-outer insulation layer; 42-first heating rod; 43-ion exchange column bracket; 44-first thermocouple; 45-elastic sealing plug; 46-liquid outlet pipe; 47-second waterproof fixed joint; 48-second heating rod; 49-first ion exchange column; 410-first flexible claw; 411-second flexible claw; 412-claw fastening bolt; 413-claw connecting bracket; 414-temperature acquisition device; 415-heating controller; 416-second thermocouple; 417-liquid level. DETAILED DESCRIPTION
[0029] The present invention provides a method for removing sulfate and chloride impurities in rare earth oxides by using a two-stage anion exchange resin. The present invention is further described below in conjunction with embodiments.
[0030] The present invention discloses a method for removing sulfate and chloride impurities in rare earth oxide by using two-stage anion exchange resin. In a specific embodiment of the present invention, the method comprises the steps of preparing ion exchange stock solution, preparing ion exchange column, primary ion exchange, secondary ion exchange, rare earth ion precipitation separation and the like. The two-stage anion exchange column is used to perform ion exchange on sulfate and chloride impurities in a rare earth solution. The sulfate in the rare earth solution is exchanged by using a primary large-capacity strong base anion resin to reduce the sulfate concentration in the rare earth solution to below 2 μg / mL. The chloride in the solution is then exchanged by using a secondary weak base anion resin to reduce the chloride concentration in the rare earth solution to below 0.8 μg / mL. Finally, the method is completed by using the steps of oxalic acid precipitation, calcination and the like. The mass percentage of sulfate and chloride in the treated rare earth oxide can be controlled to be lower than the detection limit of the detection method.
[0031] In some specific embodiments, the method for removing sulfate and chloride impurities in rare earth oxides using a two-stage anion exchange resin provided by the present invention comprises the following steps:
[0032] (1) Preparation of ion exchange stock solution: Weigh a certain amount of rare earth oxide and heat it with a certain amount of nitric acid on an electric furnace to dissolve it into a rare earth solution, which is the rare earth oxide ion exchange stock solution;
[0033] Among them, the rare earth oxides include one or more of lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, scandium oxide, yttrium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide; the mass percentage of sulfate in the rare earth oxides is ≤2%, and the mass percentage of chloride ions is ≤1%.
[0034] The rare earth ion concentration in the obtained rare earth oxide ion exchange stock solution is 20-50 mg / mL, the volume concentration of nitric acid is 5%-20%, and the volume concentration of nitric acid is preferably 5%-10%.
[0035] (2) Preparation of ion exchange columns: Select a polystyrene-based macroporous strong base anion exchange resin such as FPA91 macroporous strong base anion exchange resin, convert it into an OH-type anion exchange resin after pretreatment with water washing-alkali washing-acid washing-alkali washing, and wet-load it into the first ion exchange column and the second ion exchange column. The first ion exchange column is labeled as column A, and the second ion exchange column is labeled as column B. Select a polyacrylic acid-based gel weak base anion exchange resin such as IRA67 gel weak base anion exchange resin, convert it into an acetate-type ion exchange resin after pretreatment with water washing-acid washing, and wet-load it into the third ion exchange column and the fourth ion exchange column. The third ion exchange column is labeled as column C, and the fourth ion exchange column is labeled as column D.
[0036] Among them, the diameter of the first ion exchange column and the third ion exchange column is larger than that of the second ion exchange column and the fourth ion exchange column. The column length of the first ion exchange column and the third ion exchange column is 35 to 45 cm, the length ratio of the diameter to the column length is 1:20 to 1:30, and more than 30 mL of wet resin needs to be filled. The column length of the second ion exchange column and the fourth ion exchange column is 15 to 25 cm, the length ratio of the diameter to the column length is 1:20 to 1:30, and more than 15 mL of wet resin needs to be filled.
[0037] The volume ratio of rare earth oxide ion exchange stock solution to resin is 10:1 to 100:1.
[0038] Among them, the particle size of the polystyrene macroporous strong base anion exchange resin is 0.560-0.780 mm, and the ion exchange capacity is >1.0 eq / L. There is no limit to the pretreatment of the polystyrene macroporous strong base anion exchange resin. For example, the specific treatment steps of the FPA91 macroporous strong base anion exchange resin for water washing-alkali washing-acid washing-alkali washing pretreatment include: ① Water washing: The new resin is soaked in 50°C hot water. When the soaking starts, the water is changed every 15 minutes. Stir from time to time during the soaking. After changing the water 4 to 5 times, the water is changed every 30 minutes. The total water change is 7 to 8 times until the soaking water has no color and there is little foam. ② Alkaline washing: The washed resin is loaded into a simple chromatography column, and 1 mol / L NaOH is slowly passed through the resin, and the amount used is about 2 times the volume of the resin. ③ Acid washing: rinse with water, the pH of the water is about 9, and slowly flow 1mol / L hydrochloric acid through the resin, the amount of which is about 2 times the volume of the resin. ④ Alkali washing: rinse with water, the pH of the water is about 5, and use 1mol / L NaOH to convert the resin into OH type, the amount of which is about 4 times the volume of the resin. After the alkali solution flows out, rinse with water until the pH of the water is below 8, and then it can be put into use.
[0039] Among them, the particle size of the polyacrylic acid gel weak base anion exchange resin is 0.540-0.730 mm, and the ion exchange capacity is >1.6eq / L. The specific treatment steps for water washing-acid washing pretreatment of IRA67 gel weak base anion exchange resin include: ① Water washing: The new resin is soaked in 50℃ hot water. When the soaking starts, the water is changed every 15 minutes. Stir from time to time during the soaking. After changing the water 4-5 times, the water is changed every 30 minutes. A total of 7-8 times of water change is required until the soaking water has no color and very little foam. ② Acid washing: The washed resin is loaded into a simple chromatography column, and a 10mol / L acetic acid solution is slowly passed through the resin. The amount is about 5 times the volume of the resin. After the acid solution flows out, it is rinsed with water until the pH value of the outlet water is above 6, and then it can be put into use.
[0040] (3) Primary ion exchange: Column A is operated at a high temperature such as 20-65°C, preferably 40-60°C, and a pressure of 1-10 MPa is applied. The rare earth oxide ion exchange stock solution is added from the top of column A at a rate of 15 mL / min. Column A and column B are connected end to end through a PEEK capillary pressure-resistant tube. Column B is operated at room temperature. When there is filtrate at the bottom of column B, a saturated oxalic acid solution is used to detect whether rare earth ions flow out. The filtrate before the rare earth ions come out is discarded, and the filtrate containing the rare earth ions is retained. The barium chloride turbidimetry method is used to detect whether sulfate can be detected in the filtrate. If it can be detected, the filtrate is led back to the top of column A for exchange again. After repeating 2-3 times, columns A and B exchange sulfate ions to reach saturation. If sulfate can still be detected, an ion exchange column B' needs to be added. The size of ion exchange column B' is the same as column B until sulfate cannot be detected.
[0041] (4) Secondary ion exchange: Column C is operated at a high temperature such as 20-65°C, preferably 40-60°C, and a pressure of 1-10 MPa is applied. The filtrate obtained by the primary ion exchange in step (3) is added from the top of column C, and the addition rate of the exchange liquid is controlled to be 10 mL / min. Column C and column D are connected end to end through a PEEK capillary pressure-resistant tube. Column D is operated at room temperature. When there is filtrate at the bottom of column D, a saturated oxalic acid solution is used to detect whether rare earth ions flow out. The filtrate before the rare earth ions come out is discarded, and the filtrate containing the rare earth ions is retained. The filtrate is tested by silver nitrate turbidimetry to see whether chloride ions can be detected in the filtrate. If they can be detected, the filtrate is led back to the top of column C for exchange again. After repeating 2-3 times, column C and column D exchange chloride ions to a saturated state. If chloride ions can still be detected, an ion exchange column D' needs to be added. The size of the ion exchange column D' is the same as that of column D.
[0042] (5) The filtrate containing the rare earth ion portion obtained by the secondary ion exchange in step (4) is concentrated, and then precipitated with a saturated oxalic acid solution to obtain an oxalate rare earth precipitate, which is filtered to obtain a filter cake, which is then dried and calcined to obtain a rare earth oxide, wherein the mass percentage of sulfate in the powder is lower than the detection limit of 0.025% of the national standard turbidimetric method, and the mass percentage of chloride ion is lower than the detection limit of 0.005% of the national standard turbidimetric method.
[0043] After use, each ion exchange column is regenerated and transformed for recycling: the strong base anion exchange resin is regenerated with a saline solution of 0.2% NaOH + 10% NaCl, and after water washing-alkali washing-acid washing-alkali washing pretreatment, it is converted to OH type for use. The weak base anion exchange resin can be regenerated with 2% ammonia water, and after water washing-acid washing pretreatment, it is converted to acetate type for use.
[0044] The two-stage ion exchange in steps (3) and (4) of the above method of the present invention is achieved by using the following device: The high temperature environment of column A and column C in steps (3) and (4) is achieved by using a liquid heating device.
[0045] Taking step (3) as an example, the equipment for implementing the primary ion exchange in step (3) is described in detail as follows: Figure 1 and Figure 2 As shown, the processing equipment for ion exchange includes a high-pressure constant-current sample injection pump 1, a liquid inlet pipe 2, a first waterproof fixed joint 3, a liquid thermal device 4, a fixed joint 5 and a second ion exchange column 6; wherein the liquid thermal device 4 includes a first ion exchange column 49, a second waterproof fixed joint 47 and a liquid outlet pipe 46.
[0046] Among them, the high-pressure constant-current injection pump 1 is the power source of the entire device, which can generally control the output pressure and flow rate. It needs to be installed and fixed on a firm horizontal platform, located in the A power source area. The inlet pipe 2 and the outlet pipe 46 are made of PEEK capillary pressure-resistant tubes. One end of the inlet pipe 2 is connected to the high-pressure constant-current injection pump 1, and the other end is connected to the inlet of the first ion exchange column 49 through the first waterproof fixed joint 3. One end of the outlet pipe 46 is connected to the second ion exchange column 6 through the fixed joint 5, and the other end is connected to the outlet of the first ion exchange column 49 through the second waterproof fixed joint 47. This part is located in area C. One end of the first waterproof fixed joint 3 is an external thread structure, which is used to cooperate with the internal thread hole at the inlet end of the first ion exchange column 49. The other end of the first waterproof fixed joint 3 is a tapered structure, which forms an interference fit when connected to the inlet pipe 2, and the connection is firm. The second waterproof fixed joint 47 has the same structure as the first waterproof fixed joint 3.
[0047] The liquid heating device 4 is a device for heating the first ion exchange column 49 by liquid, and is located in the B heating zone. Generally, a certain height difference is set between the A zone and the B zone (the A zone is higher than the B zone, and the B zone is higher than the C zone), mainly to reduce the internal pressure of the liquid inlet pipe 2 and reduce the internal liquid flow resistance. Figure 2 As shown, the liquid thermal device 4 includes a heating container 40, an outer insulation layer 41, a first heating rod 42, an ion exchange column bracket 43, a first thermocouple 44, an elastic sealing plug 45, a liquid outlet pipe 46, a second waterproof fixed joint 47, a second heating rod 48, a first ion exchange column 49, a temperature acquisition device 414, a heating controller 415, a second thermocouple 416, and a liquid level 417.
[0048] The heating container 40 is preferably made of steel, and its shape is not limited to a cube. It is hollow inside and can hold liquid. The outer insulation layer 41 is a single-sided adhesive PU foam material with a thickness of 3 to 5 mm, which is pasted on the outer surface of the heating container 40. The first ion exchange column 49 is a standard laboratory instrument made of steel. The outlet end of the first ion exchange column 49 is connected to one end of the liquid outlet pipe 46 through the second waterproof fixed joint 47.
[0049] Among them, the ion exchange column bracket 43 is used to fix the first ion exchange column 49, and is made of steel, including a first flexible claw 410, a second flexible claw 411 and a claw connecting bracket 413, wherein the first flexible claw 410 and the second flexible claw 411 together form a flexible annular structure, and in a free state, its annular inner diameter is slightly smaller than the outer diameter of the middle part of the first ion exchange column 49, and the first flexible claw 410 and the second flexible claw 411 open under the action of an external force under non-destructive conditions, and its annular inner diameter can be larger than the maximum outer diameter of the first ion exchange column 49. The first flexible claw 410 and the second flexible claw 411 have a through hole at the corresponding position, and the first flexible claw 410 and the second flexible claw 411 are fastened by the claw fastening bolt 412.
[0050] The first heating rod 42 and the second heating rod 48 are used for heating the liquid and are preferably located at two diagonal positions of the heating container 40 . Lead wires from the first heating rod 42 and the second heating rod 48 are respectively connected to the heating controller 415 .
[0051] Among them, the first thermocouple 44 and the second thermocouple 416 are used to measure the liquid temperature in real time. The two thermocouples are located in the diagonal direction of the body different from the position of the heating rod. The first thermocouple 44 is arranged in the bottom area of the liquid, and the second thermocouple 416 is arranged in the internal area of the liquid close to the liquid level 417. The leads of the first thermocouple 44 and the second thermocouple 416 are connected to the temperature acquisition device 414; the heating controller 415 controls the heating power of the heating rod according to the set liquid temperature, and controls the heating power of the heating rod by reading the real-time temperature from the temperature acquisition device 414, so as to keep the liquid temperature in the set temperature range in real time.
[0052] Among them, the elastic sealing plug 45 is fixed to the bottom inside the heating container 40. The elastic sealing plug 45 and the heating container 40 are fixed by high-temperature resistant strong adhesive glue. The elastic sealing plug 45 is hollow inside, and the inner diameter is smaller than the outer diameter of the liquid outlet pipe 46. The liquid outlet pipe 46 needs to pass through the elastic sealing plug 45, and the two are interference fit. When the liquid outlet pipe 46 passes through the inner diameter of the elastic sealing plug 45, it is generally necessary to apply lubricating oil on the inner diameter of the elastic sealing plug 45 and the outer diameter of the liquid outlet pipe 46.
[0053] The device for implementing the secondary ion exchange in step (4) is the same as the equipment for the primary ion exchange in step (3).
[0054] Example 1
[0055] A method for removing sulfate and chloride impurities in thulium oxide by a two-stage anion exchange resin comprises the following steps:
[0056] (1) Preparation of ion exchange stock solution: Weigh 5.71 g of thulium oxide sample containing 1.3% sulfate and 0.78% chloride, heat with 20 mL nitric acid on an electric furnace to dissolve into a rare earth solution, and dilute to about 250 mL after cooling. This solution is the ion exchange stock solution. The rare earth ion concentration in the ion exchange stock solution is about 20 mg / mL, and the volume concentration of nitric acid is 8%.
[0057] (2) Preparation of ion exchange columns: select macroporous strong base anion exchange resin FPA91, the resin particle size is 0.560-0.780 mm, the ion exchange capacity is >1.0 eq / L, the resin is converted to OH type after water washing-alkali washing-acid washing-alkali washing pretreatment, and wet-loaded into columns A and B, wherein column A is 40 cm long and 2 cm in diameter, and column B is 20 cm long and 1 cm in diameter; select polyacrylic acid gel weak base anion exchange resin IRA67, the resin particle size is 0.540-0.730 mm, the ion exchange capacity is >1.6 eq / L, the resin is converted to acetate type after water washing-acid washing pretreatment, and wet-loaded into columns C and D, wherein column C is 40 cm long and 2 cm in diameter, and column D is 20 cm long and 1 cm in diameter.
[0058] (3) Primary ion exchange: Fix column A in the liquid heating device 4, connect the pipeline and waterproof fixed joint, input the temperature of the heating controller end to 60°C, use the high-pressure constant current injection pump 1 to output 8MPa pressure, add the ion exchange stock solution from the top of column A at a rate of 15mL / min, and connect column A and column B end to end through the PEEK capillary pressure-resistant tube. Column B can work at room temperature, and no heating device and injection pump are required. When there is filtrate at the bottom of column B, use saturated oxalic acid solution to detect whether there is rare earth ion outflow, discard the filtrate before the rare earth ions come out, and retain the filtrate containing the rare earth ions. No sulfate was detected in the filtrate by barium chloride turbidimetry.
[0059] (4) Secondary ion exchange: Fix column C in the liquid heating device 4, connect the pipeline and waterproof fixed joint, heat the controller end input temperature to 50°C, use the high-pressure constant current injection pump 1 to output 6MPa pressure, add the filtrate obtained by the primary ion exchange in step (3) from the top of column C, control the addition rate of the exchange liquid to be 10mL / min, and connect column C and column D end to end through a PEEK capillary pressure-resistant tube. Column D can work at room temperature, and no heating device and injection pump are required. When there is filtrate at the bottom of column D, use a saturated oxalic acid solution to detect whether there is rare earth ion outflow, discard the filtrate before the rare earth ions come out, and retain the filtrate containing the rare earth ions. No chloride ions were detected in the filtrate by silver nitrate turbidimetry.
[0060] (5) Precipitation and separation of rare earth ions: The filtrate containing the rare earth ions obtained by the secondary ion exchange in step (4) is concentrated and precipitated with a saturated oxalic acid solution to obtain an oxalate rare earth precipitate, which is filtered to obtain a filter cake, which is then dried and calcined to obtain a rare earth oxide. The mass percentage of sulfate in the powder is lower than the detection limit of 0.025% of the national standard turbidimetric method, and the mass percentage of chloride ions is lower than the detection limit of 0.005% of the national standard turbidimetric method. Finally, each ion exchange column is regenerated, transformed, and recycled.
[0061] Example 2
[0062] A method for removing sulfate and chloride impurities in lanthanum oxide using a two-stage anion exchange resin comprises the following steps:
[0063] (1) Preparation of ion exchange stock solution: Weigh 14.66 g of lanthanum oxide sample containing 1.9% sulfate and 0.34% chloride, heat with 25 mL nitric acid on an electric furnace to dissolve into a rare earth solution, and dilute to about 250 mL after cooling. This solution is the ion exchange stock solution. The rare earth ion concentration in the ion exchange stock solution is about 50 mg / mL, and the volume concentration of nitric acid is 10%;
[0064] (2) Preparation of ion exchange columns: select macroporous strong base anion exchange resin FPA91, the resin particle size is 0.560-0.780 mm, the ion exchange capacity is>1.0 eq / L, the resin is converted to OH type after water washing-alkali washing-acid washing-alkali washing pretreatment, and wet-loaded into columns A and B, wherein column A is 40 cm long and 2 cm in diameter, and column B is 20 cm long and 1 cm in diameter; select polyacrylic acid gel weak base anion exchange resin IRA67, the resin particle size is 0.540-0.730 mm, the ion exchange capacity is>1.6 eq / L, the resin is converted to acetate type after water washing-acid washing pretreatment, and wet-loaded into columns C and D, wherein column C is 40 cm long and 2 cm in diameter, and column D is 20 cm long and 1 cm in diameter;
[0065] (3) Primary ion exchange: Fix column A in the liquid heating device 4, connect the pipeline and waterproof fixed joints, input the temperature of the heating controller end to 50°C, use the high-pressure constant-current injection pump 1 to output a pressure of 8MPa, and add the ion exchange stock solution from the top of column A at a rate of 15mL / min. Column A and column B are connected end to end through a PEEK capillary pressure-resistant tube. Column B can work at room temperature and does not require a separate heating device and injection pump. When there is filtrate at the bottom of column B, use a saturated oxalic acid solution to detect whether there is rare earth ion outflow. The filtrate before the rare earth ions come out is discarded, and the filtrate containing the rare earth ions is retained. The concentration of sulfate in the filtrate is detected by barium chloride turbidimetry to be 50μg / mL. The filtrate is led back to the top of column A for exchange again. After repeating twice, no sulfate is detected in the filtrate;
[0066] (4) Secondary ion exchange: Fix column C in the liquid heating device 4, connect the pipeline and the waterproof fixed joint, input the temperature of the heating controller end to 50°C, use the high-pressure constant-current injection pump 1 to output a pressure of 6MPa, add the filtrate obtained by the primary ion exchange in step (3) from the top of column C, and control the addition rate of the exchange liquid to 10mL / min. Column C and column D are connected end to end through a PEEK capillary pressure-resistant tube. Column D can work at room temperature, and no heating device and injection pump are required. When there is filtrate at the bottom of column D, use a saturated oxalic acid solution to detect whether there is rare earth ions flowing out. The filtrate before the rare earth ions come out is discarded, and the filtrate containing the rare earth ions is retained. No chloride ions were detected in the filtrate using the silver nitrate turbidimetric method;
[0067] (5) Precipitation and separation of rare earth ions: The filtrate containing the rare earth ions obtained by the secondary ion exchange in step (4) is concentrated and precipitated with a saturated oxalic acid solution to obtain an oxalate rare earth precipitate, which is filtered to obtain a filter cake, which is then dried and calcined to obtain a rare earth oxide. The mass percentage of sulfate in the powder is lower than the detection limit of 0.025% of the national standard turbidimetric method, and the mass percentage of chloride ions is lower than the detection limit of 0.005% of the national standard turbidimetric method. Finally, each ion exchange column is regenerated, transformed, and recycled.
[0068] The invention adopts two-stage anion exchange resin to remove sulfate and chloride ions in rare earth oxides. The method comprises the steps of preparing ion exchange stock solution, preparing ion exchange column, primary ion exchange, secondary ion exchange, rare earth ion precipitation separation and the like. Under high temperature and high pressure conditions, two-stage anion exchange column is used to carry out ion exchange on impurities in rare earth solution. Sulfate in rare earth solution is exchanged by primary large-capacity strong base anion resin, and chloride ions in solution are exchanged by secondary weak base anion resin. The filtrate containing rare earth ions is precipitated by saturated oxalic acid solution, and then dried and calcined. The mass percentage of sulfate in the obtained rare earth oxide is lower than 0.025%, and the mass percentage of chloride ions is lower than 0.005%. The method overcomes the problem that other impurity ions are easily introduced in the sulfate removal of rare earth products by extraction process or precipitation process, and also solves the problems of long cycle, large amount of waste liquid to be treated, high cost and low yield of simple oxalate precipitation rare earth dechlorination method. The contents of sulfate and chloride ions in rare earth oxide can be controlled to be lower than the detection limit of the current national standard method. The product quality is very good and has good production benefits.
[0069] Comparative Example 1
[0070] The method for removing sulfate and chloride impurities in lutetium oxide by using a primary anion exchange resin comprises the following steps:
[0071] (1) Preparation of ion exchange stock solution: Weigh 8.53 g of lutetium oxide sample containing 1.1% sulfate and 0.53% chloride, heat with 20 mL nitric acid on an electric furnace to dissolve into a rare earth solution, and dilute to about 250 mL after cooling. This solution is the ion exchange stock solution. The rare earth ion concentration in the ion exchange stock solution is about 30 mg / mL, and the volume concentration of nitric acid is 8%;
[0072] (2) Preparation of ion exchange columns: Select polyacrylic acid gel weak base anion exchange resin IRA67 that has been pre-treated by water washing, and wet-load it into columns A and B, where column A is 40 cm long and 2 cm in diameter, and column B is 20 cm long and 1 cm in diameter;
[0073] (3) Ion exchange: Column A and column B are fixed on the preparative chromatographic column holder, the pipeline and the fixed joint are connected, and the ion exchange stock solution is added from the top of column A at a speed of 15 mL / min using an injection pump. Column A and column B are connected end to end through a PEEK capillary pressure-resistant tube. Column A and column B are both operated at room temperature. When there is filtrate at the bottom of column B, a saturated oxalic acid solution is used to detect whether rare earth ions flow out. The filtrate before the rare earth ions come out is discarded, and the filtrate containing the rare earth ions is retained. The concentration of sulfate in the filtrate detected by turbidimetry is 290 μg / mL, and the concentration of chloride ions is 140 μg / mL. The filtrate is led back to the top of column A for exchange again. After repeating 3 times, the sulfate in the filtrate is still 280 μg / mL, and the concentration of chloride ions is 125 μg / mL. Compared with Examples 1 and 2, the removal effect of impurity ions cannot meet the national standard.
Claims
1. A method for removing sulfate and chloride impurities from rare earth oxides using a two-stage anion exchange resin, characterized in that: The method comprises the steps of sequentially treating rare earth oxide ion exchange stock solution with polystyrene macroporous strong base anion exchange resin and polyacrylic acid gel weak base anion exchange resin; and further comprises the step of treating with oxalic acid: after the rare earth oxide ion exchange stock solution is treated with two-stage anion exchange resins, oxalic acid is used for precipitation, filtration, drying and burning to obtain rare earth oxide with a sulfate ion mass percentage of less than 0.025% and a chloride ion mass percentage of less than 0.005%; The polystyrene-based macroporous strong-base anion exchange resin is converted into an OH-type ion exchange resin after pretreatment and then respectively loaded into a first ion exchange column and a second ion exchange column connected end to end; the polyacrylic acid-based gel weak-base anion exchange resin is converted into an acetate-type ion exchange resin after pretreatment and then respectively loaded into a third ion exchange column and a fourth ion exchange column connected end to end; the first ion exchange column and the third ion exchange column are placed at 20-65° C.; the second ion exchange column and the fourth ion exchange column are placed at room temperature; The polystyrene-based macroporous strong base anion exchange resin is converted into an OH-type ion exchange resin after water washing, alkali washing, acid washing, and alkaline washing, and the polyacrylic acid-based gel weak base anion exchange resin is converted into an acetate-type ion exchange resin after water washing and acid washing; The rare earth oxide ion exchange stock solution is a rare earth oxide nitric acid solution obtained by dissolving rare earth oxide in nitric acid.
2. The method according to claim 1, characterized in that The particle size of the polystyrene-based macroporous strong base anion exchange resin is 0.560~0.780 mm, and the ion exchange capacity is >1.0 eq / L; the particle size of the polyacrylic acid-based gel weak base anion exchange resin is 0.540~0.730 mm, and the ion exchange capacity is >1.6 eq / L.
3. The method according to claim 1, characterized in that: The first ion exchange column and the third ion exchange column have a column length of 35 to 45 cm, a diameter to column length ratio of 1:20 to 1:30, and are filled with more than 30 mL of wet resin; the second ion exchange column and the fourth ion exchange column have a column length of 15 to 25 cm, a diameter to column length ratio of 1:20 to 1:30, and are filled with more than 15 mL of wet resin.
4. The method according to any one of claims 1 to 3, characterized in that The rare earth oxide ion filtrate treated with polystyrene macroporous strong base anion exchange resin is detected by barium chloride turbidimetry until sulfate radicals cannot be detected, and then the filtrate is treated with polyacrylic acid gel weak base anion exchange resin; The loading volume of rare earth oxide ion exchange stock solution and resin is 10:1~100:
1.
5. The method according to claim 4, characterized in that The rare earth ion concentration in the rare earth oxide ion exchange stock solution is 20-50 mg / mL, and the volume concentration of nitric acid is 5%-20%.
6. The method according to claim 5, characterized in that The mass percentage of sulfate in the rare earth oxide is ≤2%, and the mass percentage of chloride ion is ≤1%; And / or, the rare earth oxide includes one or more of lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, scandium oxide, yttrium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide.
7. The method according to claim 1, characterized in that The first ion exchange column or the third ion exchange column is placed in a liquid heat device for heating, the inlet of the first ion exchange column is connected to a liquid inlet pipe located outside the liquid heat device, the outlet of the first ion exchange column is connected to one end of a liquid outlet pipe located outside the liquid heat device, and the other end of the liquid outlet pipe is connected to the second ion exchange column; The inlet of the third ion exchange column is communicated with the liquid inlet pipe located outside the liquid thermal device, the outlet of the third ion exchange column is communicated with the liquid outlet pipe located outside the liquid thermal device, and the liquid outlet pipe is communicated with the fourth ion exchange column.
8. The method according to claim 7, characterized in that The liquid thermal device comprises a heating container, wherein the heating container has liquid, a heating rod, a thermocouple and an ion exchange column inside, the heating container is externally provided with a temperature acquirer and a heating controller, and the ion exchange column is a first ion exchange column or a third ion exchange column; And / or, a heat preservation layer is also arranged outside the heating container; a thermocouple is connected to a temperature acquirer for measuring the temperature of the liquid; a heating rod is connected to a heating controller for controlling the heating temperature of the liquid; and / or, the ion exchange column is fixed by an ion exchange column bracket.