Method for comprehensively utilizing sulfuric acid process titanium dioxide waste acid
By using oxidation, extraction, and back-extraction processes, ferrous iron in the waste acid from the sulfuric acid process for titanium dioxide is converted into ferric iron, producing potassium sulfate and ferric phosphate. This solves the problem of low utilization efficiency of waste acid and realizes efficient recycling of resources and maximizes economic benefits.
Patent Information
- Application Number
- CN202410848677.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
AI Technical Summary
In existing technologies, waste acid from the sulfuric acid process for titanium dioxide production cannot be effectively utilized, resulting in low economic efficiency. Furthermore, the resulting ferrous heptahydrate product has a high impurity content, making it difficult to meet the requirements of lithium iron phosphate batteries.
The ferrous iron in the waste acid is oxidized to ferric iron using an oxidant. Potassium chloride is added to generate potassium sulfate and ferric chloride. The ferric phosphate precursor and potassium sulfate are separated by an organic extractant and back-extracted with phosphoric acid or phosphate.
This technology enables the efficient recovery of waste acid and the recycling of resources, producing high-value potassium sulfate fertilizer and lithium iron phosphate precursors, thereby improving economic benefits.
Smart Images

Figure BDA0004916304110000051 
Figure BDA0004916304110000061 
Figure BDA0004916304110000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste acid treatment, and specifically relates to a method for comprehensive utilization of waste acid of titanium dioxide produced by a sulfuric acid process. Background Art
[0002] The sulfuric acid process of titanium dioxide produces a certain amount of waste acid during the production process. The commonly used method in the past was to neutralize and discharge it, but this method cannot achieve the economic benefits. Even if the ferrous heptahydrate product is made and sold, the impurity content is still very high, and further purification is still required when used by downstream industries.
[0003] On the other hand, the production process of iron phosphate requires a large amount of iron source, and the commonly used raw material is ferrous sulfate heptahydrate produced in the production process of titanium dioxide. The lithium battery industry has a very low tolerance for impurity elements in the precursor iron phosphate, and the commercially available ferrous sulfate heptahydrate must be deeply purified, otherwise it cannot be used in the production of iron phosphate. Among new energy sources, lithium iron phosphate batteries have far exceeded the three major lithium batteries. They are safe, environmentally friendly, low-priced, and have good recyclability. The rapid development of battery cars has also pushed forward the large expansion of lithium iron phosphate and precursor industries, so the demand for iron phosphate raw materials has also increased sharply. Summary of the invention
[0004] The purpose of the present invention is to provide a method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process in order to solve the deficiencies of the prior art.
[0005] The purpose of the present invention is achieved by the following technical solutions:
[0006] A method for comprehensive utilization of waste sulfuric acid titanium dioxide acid, comprising the following steps:
[0007] S1. using an oxidant to oxidize the divalent iron in the sulfuric acid titanium dioxide waste acid into trivalent iron;
[0008] S2. adding potassium chloride to the oxidized waste acid to react with sulfate and ferric iron in the waste acid to generate potassium sulfate and ferric chloride;
[0009] S3. extracting the solution obtained in step S2 with an organic extractant to obtain an organic phase extract containing ferric chloride and a raffinate containing potassium sulfate;
[0010] S4. The organic phase extract is stripped with phosphoric acid or phosphate to obtain a stripping raffinate containing a ferric phosphate precursor and an organic phase stripping solution.
[0011] Preferably, the iron ion content in the sulfuric acid process titanium dioxide waste acid in step S1 is 10-100 g / L, and the acidity is 100-300 g / L, and the acidity content is calculated in terms of sulfuric acid.
[0012] Preferably, the oxidant in step S1 is one or more selected from chlorine, air, O2, O3, H2O2, and sodium persulfate, and the amount of the oxidant is based on completely oxidizing the ferrous ions in the waste acid into ferric ions.
[0013] Preferably, the molar ratio of the amount of potassium chloride used in step S2 to the sulfate in the waste acid is (2-3):1.
[0014] Preferably, the organic extractant in step S3 is an N235 extraction system or a TOC extraction system;
[0015] The N235 extraction system or TOC extraction system consists of N235 or TOC, TBP and sulfonated kerosene. The volume fraction of N235 or TOC in the extraction system is 10-35%, the volume fraction of TBP is 10-20%, and the rest is sulfonated kerosene.
[0016] Preferably, the extraction O / A volume ratio in step S3 is 2:(0.5-2).
[0017] Preferably, the phosphate in step S4 is one or more combinations selected from the following compounds: ammonium phosphate, ammonium dihydrogen phosphate, diamine hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, and the stripping O / A volume ratio is 2:(0.5-1).
[0018] Preferably, the raffinate containing potassium sulfate in step S3 is concentrated by MVR, cooled, crystallized, and centrifuged to obtain potassium sulfate solid and mother liquor, and the mother liquor is returned to the MVR concentration front end; the potassium sulfate content in the potassium sulfate solid is ≥70%, and the Cl ion content is ≤1.5%.
[0019] Preferably, in step S4, the organic phase reverse extraction liquid is returned to the front end for extraction.
[0020] This application couples the treatment of waste acid from titanium dioxide produced by sulfuric acid, the production of potassium sulfate fertilizer, and the production of iron phosphate, a precursor of lithium iron phosphate, to fully realize the expansion of economic benefits and achieve the goal of circular economy. While efficiently recovering iron ions in waste acid, it converts low-priced KCL into higher-priced and more widely used K2SO4, opening up a new way and new solution for the recycling of waste acid from titanium dioxide produced by sulfuric acid. DETAILED DESCRIPTION
[0021] The sulfuric acid method titanium dioxide will produce a certain amount of waste acid during the production process. In the prior art, a typical waste acid has an iron ion content of about 10-100 g / L and an acidity of about 100-300 g / L, and the acidity content is calculated in terms of sulfuric acid. In addition, it also contains a certain amount of impurities, such as chloride ions, aluminum ions, magnesium ions, etc. Specifically, the chloride ion content is about 0.1-10 g / L, the aluminum ion content is about 1-5 g / L, the titanium ion content is about 0.1-3 g / L, the magnesium ion content is about 0.1-3 g / L, and the manganese ion content is about 0.1-3 g / L.
[0022] The present application provides a method for comprehensive utilization of waste sulfuric acid titanium dioxide, comprising the following steps:
[0023] S1. Use an oxidant to oxidize the divalent iron in the waste acid of sulfuric acid titanium dioxide into trivalent iron; preferably, the oxidant is one or more selected from chlorine, air, O2, O3, H2O2, and sodium persulfate, and the amount of the oxidant is based on completely oxidizing the ferrous ions in the waste acid into trivalent iron ions.
[0024] S2. adding potassium chloride to the oxidized waste acid to react with sulfate and ferric iron in the waste acid to generate potassium sulfate and ferric chloride;
[0025] Potassium chloride is added in this step to react with sulfate and iron ions in the waste acid to generate potassium sulfate and ferric chloride, that is, potassium chloride and ferric sulfate are replaced by ferric chloride and potassium sulfate. On the one hand, ferric chloride has a strong coordination with ferric sulfate and is more easily extracted by a commonly used iron removal composite extraction system such as N235, and is separated from other impurity ions (chloride ions combine with iron ions to form FeCl4 - In the form of FeCl4 - It is easier to be extracted by commonly used iron removal extractants such as N235, thereby achieving the extraction of iron and separation of potassium sulfate). On the other hand, potassium sulfate is more expensive and has a wider range of uses than potassium chloride. It is a commonly used agricultural fertilizer, which improves the utilization value of potassium ions.
[0026] If potassium chloride replacement is not used and an organic extraction system such as N235 is used directly to extract iron sulfate from waste acid, and there is no chloride ion involved in the extraction system, the extraction efficiency will be low.
[0027] Preferably, the molar ratio of potassium chloride to sulfate in the waste acid is 2 to 3:1. The sulfate ions in the waste acid are present in the form of sulfuric acid and ferrous sulfate, so the sulfate is in excess relative to the iron ions. When the molar ratio of potassium chloride to sulfate is 2 to 3:1, Cl:Fe 3+ The molar ratio is ≧4:1, the iron ions are completely converted into ferric chloride, and the amount of chloride ions is limited, which can ensure that the chloride ion content in the potassium sulfate product meets the requirements.
[0028] S3. extracting the solution obtained in step S2 with an organic extractant to obtain an organic phase extract containing ferric chloride and a raffinate containing potassium sulfate;
[0029] The organic extractant can be a commonly used iron removal composite extraction system such as N235 (trioctyl tertiary amine) or TOC (trioctylamine), which can selectively extract ferric chloride from the waste acid iron system and separate it from other impurity ions. Preferably, the N235 or TOC extraction system is composed of N235 or TOC, TBP and sulfonated kerosene. The volume fraction of N235 or TOC in the extraction system is 10-35%, the volume fraction of TBP is 10-20%, and the rest is sulfonated kerosene. The extraction O / A volume ratio is 2: (0.5-2), the extraction temperature is room temperature, and the extraction level depends on the Fe content in the raffinate. 3+ The raffinate containing potassium sulfate is concentrated, cooled, crystallized and centrifuged by MVR to obtain potassium sulfate solid and mother liquor. The potassium sulfate content in the potassium sulfate solid is ≥70%, and the Cl ion content is ≤1.5%. The mother liquor is returned to the MVR concentration front end for reprocessing. The potassium sulfate solid can be used to produce potassium sulfate fertilizer.
[0030] S4. Re-extracting the organic phase extract with phosphoric acid or phosphate to obtain a stripping raffinate containing the iron phosphate precursor and an organic reverse extract.
[0031] After extraction with N235 or TOC, the ferric chloride needs to be stripped out of the organic phase. Phosphoric acid or phosphate is used. Phosphate can coordinate with iron ions to form dihydrate ferric phosphate and re-enter the aqueous phase. After washing and calcination, it can be used to produce battery-grade ferric phosphate. The organic reverse extraction liquid is returned to the front end for extraction and can be recycled.
[0032] Preferably, phosphate is used for stripping, as phosphate has better stripping effect than phosphoric acid.
[0033] The phosphate is preferably one or more combinations selected from the following compounds: ammonium phosphate, ammonium dihydrogen phosphate, diamine hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, the stripping O / A volume ratio is 2: (0.5-1), and the stripping temperature is room temperature.
[0034] Therefore, this application couples the treatment of waste acid from titanium dioxide produced by sulfuric acid process, the production of potassium sulfate fertilizer, and the production of iron phosphate, a precursor of lithium iron phosphate, to fully realize the expansion of economic benefits and achieve the goal of circular economy. While efficiently recovering iron ions in waste acid, the low-priced KCL is converted into K2SO4 with a higher price and wider application, opening up a new way and new solution for the recycling of waste acid from titanium dioxide produced by sulfuric acid process.
[0035] Example 1
[0036] 1. Passing O2 gas into the waste acid of titanium dioxide produced by sulfuric acid process at room temperature, with the end point being that the ferrous ions therein are completely oxidized to trivalent ferrous ions, wherein the ferrous ion content in the waste acid of titanium dioxide produced by sulfuric acid process is 22.9 g / L, the chloride ion content is 0.2 g / L, and the acidity is 280.5 g / L (calculated as sulfuric acid);
[0037] 2. Add potassium chloride solid to the oxidized waste acid, with the molar ratio of potassium chloride to sulfate content being 2.4:1;
[0038] 3. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, N235 as a main extractant, and TBP as a phase modifier, wherein N235 accounted for 20% by volume, TBP accounted for 15% by volume, and the rest was diluted sulfonated kerosene. During extraction, the extraction phase O / A volume ratio was 2:1, the extraction time was 5 minutes, the extraction temperature was room temperature, and the extraction rate was 98.7%;
[0039] 4. Sodium dihydrogen phosphate is used for stripping, the stripping O / A volume ratio is 2:1, the stripping temperature is room temperature, the stripping rate is 99.3%, the organic reverse extraction liquid is returned to the front end for extraction, and the stripping raffinate is used as a raw material for the production of iron phosphate. After washing and calcination, the corresponding indicators of the produced iron phosphate are shown in Table 1:
[0040] Table 1
[0041]
[0042] 5. The raffinate in step S3 is concentrated, cooled, crystallized and centrifuged by MVR to obtain potassium sulfate solid, which is used to produce potassium sulfate fertilizer, and the mother liquor is returned to the front end of MVR.
[0043] Example 2
[0044] 1. Passing O2 gas into the waste acid of titanium dioxide produced by sulfuric acid process at room temperature, with the end point being that the ferrous ions therein are completely oxidized to ferric ions, wherein the ferrous ion content in the waste acid of titanium dioxide produced by sulfuric acid process is 23.6 g / L, the chloride ion content is 2.0 g / L, and the acidity is 278.5 g / L (calculated as sulfuric acid);
[0045] 2. Add potassium chloride solid to the oxidized waste acid, with the molar ratio of potassium chloride to sulfate content being 2.8:1;
[0046] 3. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, TOA as a main extractant, and TBP as a phase modifier, wherein TOC accounted for 30% by volume, TBP accounted for 20% by volume, and the rest was diluted sulfonated kerosene. During extraction, the volume ratio of the extracting phase to O / A was 1:1, the extraction time was 5 minutes, the extraction temperature was room temperature, and the extraction rate was 99.2%;
[0047] 4. Use ammonium dihydrogen phosphate for stripping, the stripping O / A volume ratio is 2:1, the stripping temperature is room temperature, the stripping rate is 99.3%, the organic reverse extraction liquid is returned to the front end for extraction, and the stripping raffinate is used as a raw material for the production of iron phosphate. After washing and calcination, the corresponding indicators of the produced iron phosphate are shown in Table 2:
[0048] Table 2
[0049]
[0050] 5. The raffinate in step S3 is concentrated, cooled, crystallized and centrifuged by MVR to obtain potassium sulfate solid, which is used to produce potassium sulfate fertilizer, and the mother liquor is returned to the front end of MVR.
[0051] Example 3
[0052] 1. Passing O2 gas into the waste acid of titanium dioxide produced by the sulfuric acid process at room temperature, with the end point being that the ferrous ions therein are completely oxidized to trivalent ferrous ions, wherein the ferrous ion content in the waste acid of titanium dioxide produced by the sulfuric acid process is 24.7 g / L, the chloride ion content is 1.8 g / L, and the acidity is 267.8 g / L (calculated as sulfuric acid);
[0053] 2. Add potassium chloride solid to the oxidized waste acid, with the molar ratio of potassium chloride to sulfate content being 3.0:1;
[0054] 3. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, TOA as a main extractant, and TBP as a phase modifier, wherein TOC accounted for 30% by volume, TBP accounted for 20% by volume, and the rest was diluted sulfonated kerosene. During extraction, the extraction phase O / A volume ratio was 1:1, the extraction time was 5 minutes, the extraction temperature was room temperature, and the extraction rate was 99.4%;
[0055] 4. Use ammonium dihydrogen phosphate for stripping, the stripping O / A volume ratio is 2:1, the stripping temperature is room temperature, the stripping rate is 99.4%, the organic reverse extraction liquid is returned to the front end for extraction, and the stripping raffinate is used as a raw material for the production of iron phosphate. After washing and calcination, the corresponding indicators of the produced iron phosphate are shown in Table 3:
[0056] Table 3
[0057]
[0058] 5. The raffinate in step S3 is concentrated, cooled, crystallized and centrifuged by MVR to obtain potassium sulfate solid, which is used to produce potassium sulfate fertilizer, and the mother liquor is returned to the front end of MVR.
[0059] Example 4
[0060] 1. Passing O2 gas into the waste acid of titanium dioxide produced by sulfuric acid process at room temperature, to completely oxidize the ferrous ions therein into ferric ions, wherein the waste acid of titanium dioxide produced by sulfuric acid process is the same as that in Example 3;
[0061] 2. Add potassium chloride solid to the oxidized waste acid, with the molar ratio of potassium chloride to sulfate content being 2.0:1;
[0062] 3. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, TOA as a main extractant, and TBP as a phase modifier, wherein TOC accounted for 15% by volume, TBP accounted for 15% by volume, and the rest was diluted sulfonated kerosene. During extraction, the extraction phase O / A volume ratio was 2:0.5, the extraction time was 5 minutes, and the extraction temperature was room temperature;
[0063] 4. Use phosphoric acid for stripping, the stripping O / A volume ratio is 2:0.5, the stripping temperature is room temperature, the organic reverse extraction liquid is returned to the front end for extraction, and the stripping raffinate is used as a raw material for iron phosphate production;
[0064] 5. The raffinate in step S3 is concentrated, cooled, crystallized and centrifuged by MVR to obtain potassium sulfate solid, which is used to produce potassium sulfate fertilizer, and the mother liquor is returned to the front end of MVR.
[0065] Comparative Example 1
[0066] 1. Passing O2 gas into the waste acid of titanium dioxide produced by sulfuric acid process at room temperature, with the end point being that the ferrous ions therein are completely oxidized to trivalent ferrous ions, wherein the ferrous ion content in the waste acid of titanium dioxide produced by sulfuric acid process is 22.9 g / L, the chloride ion content is 0.2 g / L, and the acidity is 280.5 g / L (calculated as sulfuric acid);
[0067] 2. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, N235 as a main extractant, and TBP as a phase modifier, wherein N235 accounted for 20% by volume, TBP accounted for 15% by volume, and the rest was diluted sulfonated kerosene. During extraction, the extraction phase O / A volume ratio was 2:1, the extraction time was 5 minutes, and the extraction temperature was room temperature;
[0068] 3. The extraction is finished, and the extraction rate is low, only 13%;
[0069] 4. Use diammonium phosphate for stripping, the stripping O / A volume ratio is 2:1, the stripping temperature is room temperature, the stripping rate is 99.4%, and the stripping solution is used as a raw material for the production of iron phosphate. After washing and calcination, the corresponding indicators of the produced iron phosphate are shown in Table 4:
[0070] Table 4
[0071]
[0072] Comparative Example 2
[0073] 1. Passing O2 gas into the waste acid of titanium dioxide produced by the sulfuric acid process at room temperature, with the end point being that the ferrous ions therein are completely oxidized to trivalent ferrous ions, wherein the ferrous ion content in the waste acid of titanium dioxide produced by the sulfuric acid process is 24.7 g / L, the chloride ion content is 1.8 g / L, and the acidity is 267.8 g / L (calculated as sulfuric acid);
[0074] 2. Extraction was performed using a composite extractant consisting of sulfonated kerosene as a diluent, N235 as a main extractant, and TBP as a phase modifier, wherein N235 accounted for 15% by volume, TBP accounted for 15% by volume, and the rest was diluted sulfonated kerosene. During extraction, the extracting phase O / A volume ratio was 2:1, the extraction time was 5 minutes, and the extraction temperature was room temperature;
[0075] 3. The extraction is finished, and the extraction rate is low, only 11%;
[0076] 4. Use diammonium phosphate for stripping, the stripping O / A volume ratio is 2:1, the stripping temperature is room temperature, the stripping rate is 99.3%, and the stripping solution is used as a raw material for the production of iron phosphate. After washing and calcination, the corresponding indicators of the produced iron phosphate are shown in Table 5:
[0077] Table 5
[0078]
[0079] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process, characterized in that: The following steps are involved: S1. using an oxidant to oxidize the divalent iron in the sulfuric acid titanium dioxide waste acid into trivalent iron; S2. adding potassium chloride to the oxidized waste acid to react with sulfate and ferric iron in the waste acid to generate potassium sulfate and ferric chloride; S3. extracting the solution obtained in step S2 with an organic extractant to obtain an organic phase extract containing ferric chloride and a raffinate containing potassium sulfate; S4. The organic phase extract is stripped with phosphoric acid or phosphate to obtain a stripping raffinate containing a ferric phosphate precursor and an organic phase stripping solution.
2. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process as claimed in claim 1, characterized in that: In step S1, the iron ion content in the sulfuric acid process titanium dioxide waste acid is 10-100 g / L, and the acidity is 100-300 g / L, and the acidity content is calculated in terms of sulfuric acid.
3. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process as claimed in claim 1, characterized in that: The oxidant in step S1 is one or more selected from chlorine, air, O2, O3, H2O2, and sodium persulfate, and the amount of the oxidant used is based on completely oxidizing the ferrous ions in the waste acid into ferric ions.
4. The method for comprehensive utilization of waste acid from sulfuric acid process titanium dioxide according to claim 1, characterized in that: The molar ratio of the amount of potassium chloride used in step S2 to the sulfate in the waste acid is (2-3):
1.
5. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process as claimed in claim 1, characterized in that: The organic extractant in step S3 is an N235 extraction system or a TOC extraction system; The N235 extraction system or TOC extraction system consists of N235 or TOC, TBP and sulfonated kerosene. The volume fraction of N235 or TOC in the extraction system is 10-35%, the volume fraction of TBP is 10-20%, and the rest is sulfonated kerosene.
6. The method for comprehensive utilization of waste sulfuric acid titanium dioxide according to claim 5, characterized in that: The extraction O / A volume ratio in step S3 is 2:(0.5-2).
7. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process as claimed in claim 1, characterized in that: The phosphate in step S4 is one or more combinations selected from the following compounds: ammonium phosphate, ammonium dihydrogen phosphate, diamine hydrogen phosphate, sodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, and the stripping O / A volume ratio is 2:(0.5-1).
8. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process as claimed in claim 1, characterized in that: In step S3, the raffinate containing potassium sulfate is concentrated, cooled, crystallized, and centrifuged by MVR to obtain potassium sulfate solid and mother liquor, and the mother liquor is returned to the MVR concentration front end; The potassium sulfate content in the potassium sulfate solid is ≥70%, and the Cl ion content is ≤1.5%.
9. The method for comprehensive utilization of waste acid from titanium dioxide produced by sulfuric acid process according to claim 1, characterized in that: In step S4, the organic phase extract is returned to the front end for extraction.
Citation Information
Patent Citations
Method for recovering titanium
EP0298763A2
Cited By
Battery-grade lithium iron phosphate, preparation method thereof, positive pole piece and secondary battery
CN118993008A
Method for treating washing wastewater in production process of 2-chloro-5-chloromethylpyridine