Packaging sheet and preparation method thereof, photovoltaic device

By using special encapsulation sheets in photovoltaic devices, the problems of aesthetic adaptability and power attenuation of the encapsulation sheets are solved, the stability of the color layer and the reflectivity are improved, the service life of the photovoltaic devices is extended and the cost is reduced. Power attenuation.

CN115386125BActive Publication Date: 2024-10-29FOSTER (JIAXING) NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211209288.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-10-29
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing photovoltaic device packaging sheets have deficiencies in aesthetic adaptability and power attenuation. In particular, the color aging of colored photovoltaic backsheets after their service life increases, leading to appearance deterioration and power generation attenuation.

Method used

Provide an encapsulation sheet, including a support layer and a color layer on the surface. Through a specific lamination process and coating combination, the hardness, cross-linking degree and reflectivity of the color layer can be ensured to maintain 2000 under the conditions of 85℃ & 85% humidity. Hours of chromatic aberration stability, and the average reflectance in the 400-1200nm range is higher than 30%.

Benefits of technology

It achieves the appearance adaptability and color stability of photovoltaic devices, extends the service life, reduces power attenuation, and ensures excellent power generation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115386125B_ABST
    Figure CN115386125B_ABST
Patent Text Reader

Abstract

The present invention provides an encapsulation sheet material for encapsulation of photovoltaic devices, the encapsulation sheet material comprises a support layer, and a color layer arranged on at least one side surface of the support layer; the thickness of the color layer is 1-30 μm; the surface hardness of the color layer is not less than 2H; the encapsulation sheet material satisfies the following conditions: the encapsulation sheet material is stacked and laminated in the manner of encapsulation sheet material + EVA film + glass to obtain a laminated body, the laminated body is subjected to damp heat aging at 85°C & 85% humidity for 2000 hours, the color difference ΔE*ab of the laminated body before and after aging is tested, and the laminated body satisfies ΔE*ab not higher than 10. The encapsulation sheet material provided by the present invention is applied to photovoltaic devices for long-term use to ensure that the encapsulation sheet material still has good adaptability after aging, has long-term weather resistance, and has a certain gain effect on photovoltaic devices, reduces the power attenuation of photovoltaic devices, and ensures excellent power generation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell packaging, in particular to a packaging sheet and a preparation method thereof, and a photovoltaic device. Background Art

[0002] With the continuous changes in energy structure, the development of new energy has become a global proposition. In terms of application scenarios, solar cells have a clear trend of both centralized and distributed applications, and the prospects for diversified application areas and smart photovoltaics are broad. Industrial and commercial roofs, residential roofs, curtain walls, color steel plate factory roofs and other locations have received more and more attention because they can be used for both power generation and partial building materials.

[0003] The biggest difference between photovoltaic devices used in buildings and conventional ground power stations is the different requirements for customized appearance. Traditional photovoltaic devices, especially crystalline silicon photovoltaic devices, are relatively simple black and white, which is far from the pursuit of diverse aesthetics in architecture. For example, photovoltaic devices made of white backplane materials are white between the cell gaps, the frame and the cell, and the entire component will present alternating tones of white and blue. This color tone is applied to the roof or curtain wall, and the overall appearance is less beautiful and the client is less accepting. Therefore, it is a difficult problem for the photovoltaic industry to meet both component functions and aesthetic requirements.

[0004] In addition, as the years of use of photovoltaic devices increase, the power of photovoltaic devices will gradually decay. In order to solve the problem of photovoltaic device power decay, in addition to improving the performance of the cell itself, it is also crucial to improve the packaging sheet for photovoltaic devices. At present, the main solutions for improving the power decay of the module for the packaging sheet are focused on improving the water vapor barrier and reducing the migration of free metal ions to reduce the PID effect (Potential Induced Degradation) of the photovoltaic device, so as to reduce the power decay of the photovoltaic device, and the color stability of the packaging sheet also has an impact on the power decay of the photovoltaic device. Specifically, usually according to the appearance requirements, the photovoltaic backplane uses a colored sealing sheet. As the years of use of the photovoltaic device increase, the colored photovoltaic backplane begins to age first, and the color becomes lighter, causing the appearance of the module to deteriorate. At the same time, the colored photovoltaic backplane also bears the role of selectively reflecting the sunlight of each band. As the color of the photovoltaic backplane deteriorates, the reflectivity of each area of ​​the photovoltaic backplane deteriorates to varying degrees, affecting the power generation of the photovoltaic device and causing varying degrees of power decay. Photovoltaic encapsulation sheets with long-term color stability can delay the aging of photovoltaic devices and extend the service life of photovoltaic devices. They are an effective solution to reduce the power attenuation rate of components.

[0005] Therefore, it is necessary to develop a packaging sheet for use in photovoltaic devices that not only has long-term chromaticity stability, but can also meet the color matching problem between the packaging sheet and the battery cell in photovoltaic building applications to achieve an aesthetic effect, and also has the functional effects of extending weather resistance and reducing component attenuation power. Summary of the invention

[0006] The main purpose of the present invention is to provide a packaging sheet to solve the problems in the prior art that the packaging sheet is used in photovoltaic devices with low appearance adaptability and the photovoltaic device has serious power attenuation.

[0007] In order to achieve the above object, according to one aspect of the present invention, there is provided an encapsulation sheet material for encapsulation of a photovoltaic device, the encapsulation sheet material comprising a support layer, and a color layer disposed on at least one side surface of the support layer;

[0008] The thickness of the color layer is 1 to 30 μm;

[0009] The surface hardness of the color layer is not less than 2H;

[0010] The encapsulation sheet satisfies the following conditions: the encapsulation sheet is stacked and laminated in the manner of encapsulation sheet + EVA film + glass to obtain a laminate, the laminate is subjected to damp heat aging at 85°C & 85% humidity for 2000 hours, the color difference ΔE*ab of the laminate before and after aging is tested, and the laminate satisfies ΔE*ab not higher than 10.

[0011] Furthermore, the glass transition temperature of the color layer is 20-80°C.

[0012] Furthermore, the cross-linking degree of the color layer is not less than 75%.

[0013] Furthermore, the thickness of the support layer is 100-300 μm.

[0014] Furthermore, the average reflectivity of the surface of the color layer of the packaging sheet away from the support layer in the range of 400 to 1200 nm is higher than 30%.

[0015] Furthermore, the glossiness of the surface of the color layer away from the support layer is 25-85 GU.

[0016] Furthermore, the color layers are obtained by coating a coating on the surface of a support layer and then drying it, the coating comprising a resin, a pigment, an additive and a solvent, and the mass ratio of the resin to the pigment in the coating is 8 to 19:1.

[0017] Furthermore, the resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, phenolic resin, and terpene resin;

[0018] The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

[0019] A method for preparing an encapsulation sheet, the preparation method is used to manufacture the encapsulation sheet as described in claims 1-8, resin, additives, pigments and solvents are mixed evenly into a coating, coated on at least one side of a support layer by a coating process and dried at 60°C-200°C to obtain the encapsulation sheet.

[0020] A photovoltaic device comprises a photovoltaic front plate, a first photovoltaic adhesive film, a battery layer, a second photovoltaic adhesive film and a photovoltaic back plate, wherein the photovoltaic back plate is covered with the above-mentioned packaging sheet.

[0021] The encapsulation sheet provided by the present invention has good adaptability to the appearance of the battery layer in the photovoltaic device, and has good color stability. It can be used in photovoltaic devices for a long time to ensure that the encapsulation sheet can still have good adaptability after aging, has long-term weather resistance, and has a certain gain effect on the photovoltaic device, reducing the power attenuation of the photovoltaic device and ensuring excellent power generation performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 A structure of a packaging sheet is shown;

[0024] Figure 2 A structure of a photovoltaic device is shown.

[0025] The above drawings include the following reference numerals:

[0026] 1. Photovoltaic backplane; 11. Color layer; 12. Support layer; 2. Second photovoltaic film; 3. Cell layer; 4. First photovoltaic film; 5. Photovoltaic front panel. DETAILED DESCRIPTION

[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0028] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0029] A packaging sheet material is used for packaging a photovoltaic device, the packaging sheet material comprising a support layer and a color layer arranged on at least one side surface of the support layer;

[0030] The thickness of the color layer is 1 to 30 μm;

[0031] The hardness of the surface of the color layer away from the support layer is not less than 2H;

[0032] The encapsulation sheet satisfies the following conditions: the encapsulation sheet is stacked and laminated in the manner of encapsulation sheet + EVA film + glass to obtain a laminate, the laminate is subjected to damp heat aging at 85°C & 85% humidity for 2000 hours, the color difference ΔE*ab of the laminate before and after aging is tested, and the laminate satisfies ΔE*ab not higher than 10.

[0033] Specifically, the encapsulation sheet is used for encapsulation of photovoltaic devices, such as Figure 1 As shown, the encapsulation sheet includes at least one supporting layer and a color layer arranged on at least one side surface of the supporting layer, and the encapsulation sheet is adapted to the appearance of the photovoltaic device. The color layer needs to achieve a dark appearance and have a certain light transmittance so that the light in the visible-infrared band incident on the encapsulation sheet is partially reflected. From the perspective of light transmittance, the thickness of the color layer is 1 to 30 μm. When the thickness of the color layer is less than 1 μm, the thickness of the color layer is too thin, the visible light transmittance will also increase, and the covering effect will be significantly reduced, making it difficult to match the photovoltaic cell assembly and achieve a good appearance; when the thickness of the color layer is greater than 30 μm, the light transmittance of the visible-infrared light band decreases, the utilization rate of infrared rays is greatly reduced, and it is difficult to achieve the effect of power gain on the photovoltaic device.

[0034] The encapsulation sheet requires good appearance stability, especially when the encapsulation sheet is used in photovoltaic device encapsulation. In order to ensure that the encapsulation sheet has excellent appearance performance during use, the hardness of the surface of the color layer away from the support layer is not less than 2H.

[0035] Specifically, the color layer contains a pigment, and during the use of the photovoltaic device, the pigment will migrate from the color layer to the second photovoltaic film as the photovoltaic device ages. Due to the different migration rates of different pigments, the color layer and the second photovoltaic film have color areas of different depths. The increased hardness of the color layer means that the bond between the color layer resins is tighter, so that the pigment is difficult to migrate from the interface between the color layer and the second photovoltaic film, which can effectively slow down the color aging of the encapsulation sheet. In particular, when the hardness of the surface of the color layer away from the support layer is greater than 2H, the encapsulation sheet has extremely strong color stability. On the other hand, when the hardness of the surface of the color layer away from the support layer is too large, adverse effects such as cracking of the coating may occur during the use of the encapsulation sheet. Preferably, the hardness of the surface of the color layer away from the support layer is not less than 2H and not more than 4H.

[0036] In order to ensure that the encapsulation sheet has excellent appearance performance and stable power generation gain during use, the encapsulation sheet is adjusted through the color layer and the support layer so that the encapsulation sheet meets the following conditions: the encapsulation sheet is stacked and laminated in the manner of encapsulation sheet + EVA film + glass to obtain a laminate, the laminate is subjected to damp heat aging at 85°C and 85% humidity for 2000 hours, the color difference ΔE*ab of the laminate before and after aging is tested, and the laminate satisfies ΔE*ab not higher than 10, and the calculation formula is ΔE*ab=[(ΔL*)2+(Δa*)2+(Δb*)2]1 / 2.

[0037] Specifically, the laminate adopts a laminated structure of 3.2mm photovoltaic glass, 0.45mm F806PS (Foster) EVA film, and the encapsulation sheet, wherein the color layer is in direct contact with the EVA film layer, and is prepared after lamination at 145°C for 18 minutes. The laminate is measured according to the uniform color space and color difference formula of GB / T 7921-2008 to obtain the initial chromaticity L1, a1, b1, and then the laminate is subjected to damp heat aging at 85°C and 85% humidity for 2000 hours, and the aging chromaticity L2, a2, b2 of the laminate is tested and calculated according to the formula ΔE*ab=[(L1-L2)2+(a1-a2)2+(b1-b2)2]1 / 2.

[0038] The laminate satisfies ΔE*ab not higher than 10, and the encapsulation sheet has excellent appearance stability. When applied to photovoltaic devices, long-term stability can be guaranteed. In addition to excellent appearance, the encapsulation sheet also ensures the gain effect of the photovoltaic device. Preferably, the laminate satisfies ΔE*ab not higher than 8.

[0039] Preferably, the LAB value range of the laminate before aging is L1: 10-55, a1: -20-50, b1: -40-50, and the LAB value range after aging is L2: 10-65, a2: -25-55, b2: -45-85.

[0040] When the encapsulation sheet has long-term chromaticity stability, the encapsulation sheet is used for the encapsulation of photovoltaic devices to ensure that pigment migration does not occur during long-term use. At this time, not only can the appearance of the photovoltaic device remain stable for a long time, but the reflectivity of the encapsulation sheet of the photovoltaic device is also maintained in a stable range, and there will be no difference in reflectivity in different areas due to uneven color migration, resulting in different power generation of cells in different areas, thereby ensuring uniform and stable power generation in various areas of the photovoltaic device, thereby reducing the reduction in light utilization due to reflectivity changes caused by color aging of the encapsulation sheet, reducing the power attenuation of the photovoltaic device, and helping to extend the service life of the photovoltaic device.

[0041] Furthermore, the glass transition temperature of the color layer is 20-80°C.

[0042] Specifically, in order to ensure that the pigment in the color layer does not easily migrate to the second photovoltaic adhesive film, the glass transition temperature of the color layer should be higher than 20°C to prevent the color layer from cracking during use. Preferably, the glass transition temperature of the color layer is 20-80°C.

[0043] Furthermore, the cross-linking degree of the color layer is not less than 75%.

[0044] Specifically, the degree of crosslinking of the color layer has a great influence on the long-term color stability of the encapsulation sheet. Usually, as the degree of crosslinking of the color layer increases, the resins in the color layer are more tightly connected, and the pigments in the color layer are more easily fixed in the grid formed by the crosslinking of the resins, making it difficult to migrate from the color layer to the second photovoltaic adhesive film, thereby greatly slowing down the color aging of the encapsulation sheet. Preferably, the degree of crosslinking of the color layer is not less than 75%, at which time the encapsulation sheet has excellent and long-lasting color stability. When the degree of crosslinking of the color layer is less than 75%, the pigments in the color layer are easy to migrate during the use of the component, and the encapsulation sheet is very easy to fade, and the color stability of the encapsulation sheet is poor.

[0045] Furthermore, the thickness of the support layer is 100-300 μm.

[0046] From the perspective of manufacturing process and stability of the encapsulation sheet, the thickness of the support layer is 100-300μm. If the thickness of the support layer is less than 100μm, the reflectivity of the encapsulation sheet in the visible-infrared band will be reduced, and it will be difficult to ensure the power gain effect of the photovoltaic device. At the same time, the thickness of the overall encapsulation sheet is relatively small, and the color difference of the color layer will further increase after aging treatment, making it difficult to ensure the stability of the appearance. If the thickness of the support layer is greater than 300μm, it will be difficult to produce with conventional double-pulling equipment, the thickness uniformity will be difficult to control, the mechanical property uniformity will be difficult to control, and the cost of the encapsulation sheet will be greatly increased.

[0047] Furthermore, the average reflectivity of the surface of the color layer of the packaging sheet away from the support layer in the range of 400 to 1200 nm is higher than 30%.

[0048] Specifically, the encapsulation sheet has a certain degree of selective permeability and selective reflectivity for light of each band. The support layer selectively reflects visible-infrared band light, which is used to improve the utilization rate of light by the cells in the photovoltaic device and improve the power generation of the photovoltaic device. At the same time, it can reduce the absorption of infrared band light by other parts of the photovoltaic device and improve the power generation of the photovoltaic device. The color layer is used to selectively transmit visible-infrared band light to achieve a dark appearance and reduce the transmission of ultraviolet band light, thereby extending the service life of the photovoltaic device. Specifically, the average reflectivity of the surface of the color layer of the encapsulation sheet away from the support layer in the range of 400 to 1200nm is higher than 30%. It should be noted here that the reflectivity of the surface of the color layer of the encapsulation sheet away from the support layer is higher than 30%, which does not refer to the reflectivity of the color layer itself, but the reflectivity of the encapsulation sheet itself combined with the support layer and the color layer.

[0049] The glossiness of the surface of the color layer away from the support layer is 25-85 GU.

[0050] The color layer is obtained by curing the coating after being coated on the surface of the support layer. Compared with the surface of the support layer, the surface of the color layer is more prone to scratches, creases and other marks. Although it does not affect the actual performance after lamination in the photovoltaic device, the defects in appearance can easily affect product sales. Therefore, in order to solve the problem of product appearance, it is necessary to control the glossiness of one side of the color layer of the encapsulation sheet to be less than 85GU. When the surface glossiness of one side of the color layer of the encapsulation sheet is less than 85GU, even if scratches and creases appear on the surface of the color layer, they are not obvious to the naked eye and do not affect the appearance of the encapsulation sheet. Preferably, the glossiness of the surface of one side of the color layer of the encapsulation sheet is 25-85GU. At this time, the encapsulation sheet presents a certain matte effect, excellent appearance, and does not lose too much light, thereby improving the power generation of the photovoltaic device.

[0051] The color layer is prepared by coating a coating on the surface of a support layer and then drying the coating. The coating contains resin, pigment, auxiliary agent and solvent. The mass ratio of the resin to the pigment in the coating is 8 to 19:1.

[0052] Specifically, the color layer is obtained by coating a coating on one side of the support layer and then drying it. The color layer is a composition comprising a mixture of resin, pigment, additive and solvent, and the mass ratio of the resin: additive: pigment is preferably 8-19:0.5-5:1. If the mass ratio of the pigment is too low, the color coverage is poor, and the ultraviolet and visible light transmittance is high; if the mass ratio of the pigment is too high, the dispersion uniformity is poor, and the occurrence of agglomeration will reduce the transmittance in the infrared range.

[0053] Furthermore, the resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, phenolic resin, and terpene resin;

[0054] From the perspective of improving the color stability of the encapsulation sheet, it is preferred that the acid value of the resin is less than 10 mgKOH / g and the hydroxyl value is greater than 40 mgKOH / g. When the acid value of the resin in the coating exceeds 10 mgKOH / g, there are more carboxyl groups in the coating, and the reaction between the carboxyl groups in the coating resin and the curing agent is slow, resulting in a reduction in cross-linking sites, which further leads to a decrease in the weather resistance and color stability of the color layer to varying degrees. However, if the hydroxyl value of the resin in the coating is too small and the content of cross-linkable active groups is low, it is difficult to achieve sufficient cross-linking degree in the production process, resulting in insufficient surface hardness of the coating, which further leads to the migration of the pigment, making it difficult to ensure the color stability of the encapsulation sheet.

[0055] The auxiliary agent is selected from one or more of a curing agent, a stabilizing agent, a catalyst, and a diluent;

[0056] The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

[0057] Specifically, the pigment can be selected from benzimidazolone, copper phthalocyanine, aluminum phthalocyanine, zinc phthalocyanine, tetrafluoroisoindolinone, 3,4,9,10-tetracarboxamide diimide, quinacridone, 2,9-dimethyl-anthraquino[2,1,9-DEF:6,5,10-D'E'F']diisoquinoline-1,3,8,10(2H,9H)-tetraone, 5,12-dihydro-quinolino[2,3-B]acridine-7,14-dione, N-[4-(aminocarbonyl)phenyl]-4-[[1-[[(2,3-dihydro -2-oxo-1H-benzimidazol-5-yl)-amino]carbonyl]-2-oxopropyl]azo]aniline, N,N-bis(4-methoxybenzyl)perylene-3,4,9,10-dicarboximide, 8,18-dichloro-5,15-diethyl-5,15-dihydrocarbazo[3',2':5,6][1,4]oxazine[2,3-b]indol[2,3-i]phenoxazine, 3,6-bis(4-chlorophenyl)-2,5-dihydro-pyrrolo[3,4-c]pyrrole-1,4-dione, etc.

[0058] Further, from the perspective of improving the crosslinking degree of the color layer, the curing agent is selected from one or more of hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated xylylene isocyanate trimer, hydrogenated xylylene isocyanate prepolymer, toluene diisocyanate trimer, toluene diisocyanate prepolymer, methylated polymethylol melamine resin, butylated polymethylol melamine resin, mixed etherified polymethylol melamine resin, polyamide, polymethylene diamine, diethylene triamine, pentamethyl diethylene triamine, triethylene tetramine, diethylene triamine, triethylene tetramine, (2,3-dimethyl) dibutylene triamine;

[0059] Preferably, the curing agent content is preferably an isocyanate curing agent, and the curing agent is preferably one or more of hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated xylene diisocyanate trimer, hydrogenated xylene diisocyanate prepolymer, toluene diisocyanate trimer, and toluene diisocyanate prepolymer.

[0060] The stabilizing agent is selected from one or more of acrylic block copolymers, silicon-containing copolymers, acidic group-containing copolymers, polyether siloxane copolymers, acrylate copolymers, calcium carbonate, silicon dioxide, and zinc oxide;

[0061] The catalyst is selected from one or more of pentamethyldiethylenetriamine, bis(dimethylaminoethyl)ether, stannous octoate, dioctyltin dilaurate, monobutyltin oxide, monobutyltin triisooctoate, dibutyltin dilaurate, acetic acid, p-toluenesulfonic acid, phthalic acid, lauric acid, and isooctanoic acid; the diluent is selected from one or more of alcohols, benzenes, esters, and ketones.

[0062] Furthermore, the support layer is selected from any one of polyethylene terephthalate film, polyethylene naphthalate film, polyolefin film, polycarbonate film, polyethylene-acrylate film, polyethylene-methacrylate film, polyester film, polyurethane film, styrene-methyl methacrylate copolymer film, methyl methacrylate-butadiene-styrene copolymer film, preferably any one of polyethylene terephthalate film, polyethylene naphthalate film, and polyolefin film.

[0063] Specifically, the support layer is preferably one of a polyethylene terephthalate film, a polyethylene naphthalate film, and a polyolefin film.

[0064] Furthermore, the encapsulation sheet is applied to a photovoltaic back panel, and the color layer is obtained by uniformly mixing resin, additives, and pigments, coating the mixture on a support layer using a coating process, and then drying the mixture at 60° C.-200° C. and rolling the mixture up.

[0065] A photovoltaic device, such as Figure 2 As shown, the photovoltaic device includes a photovoltaic front panel, a first photovoltaic film, a battery layer, a second photovoltaic film and a photovoltaic back panel, the photovoltaic back panel includes the encapsulation sheet, the photovoltaic front panel is photovoltaic glass, the first photovoltaic film and the second photovoltaic film are commonly used EVA films, POE films, or EPE and other photovoltaic films.

[0066] Furthermore, the encapsulation sheet is applied to a photovoltaic back panel, and the side of the encapsulation sheet support layer away from the color layer may be a polyester film, a fluorine film, or other coatings.

[0067] The encapsulation sheet provided by the present invention has good adaptability to the appearance of the battery cells in the photovoltaic device, and has good color stability. It can be used in photovoltaic devices for a long time to ensure that the encapsulation sheet can still have good adaptability after aging, has long-term weather resistance, and has a certain gain effect on the photovoltaic device, reducing the power attenuation of the photovoltaic device and ensuring excellent power generation performance.

[0068] The beneficial effects of the present application are further illustrated below in combination with embodiments and comparative examples.

[0069] Preparation of coating composition: The color layer is prepared by coating the coating on the surface of the support layer and then drying it. The components and addition amounts of the coating composition are shown in Table 1.

[0070] Table 1

[0071]

[0072]

[0073] The specific components in Table 1 are as follows:

[0074] Resin

[0075] A1 fluorocarbon resin 41011 (Changxing Chemical), acid value 1 mgKOH / g, hydroxyl value 56 mgKOH / g

[0076] A2 acrylic resin BS965 (Jiangsu Sanmu Chemical Co., Ltd.), acid value 7mgKOH / g, hydroxyl value 56mgKOH / g

[0077] A3 acrylic resin ACR6458 (Gaoming Tongde Chemical Co., Ltd.), acid value 1mgKOH / g, hydroxyl value 40mgKOH / g

[0078] A4 acrylic resin AC3267 (Nengda Chemical Co., Ltd.), acid value 6mgKOH / g, hydroxyl value 99mgKOH / g

[0079] A5 alkyd resin 3222 (Hebei Deda New Materials Co., Ltd.), acid value is 4mgKOH / g, hydroxyl value is 150mgKOH / g

[0080] A6 polyester resin 220# (Toyobo), acid value is 2mgKOH / g, hydroxyl value is 50mgKOH / g

[0081] A7 acrylic resin AC166 (Shanghai Qizhan New Material Technology Co., Ltd.), acid value is 15mgKOH / g, hydroxyl value is 100mgKOH / g

[0082] A8 acrylic resin PR-870 (Shanghai Qizhan New Material Technology Co., Ltd.), acid value 5mgKOH / g, hydroxyl value 17mgKOH / g

[0083] pigment

[0084] B1 N,N-bis(4-methoxybenzyl)perylene-3,4,9,10-dicarboximide (Xin Hongli Chemical Co., Ltd.)

[0085] B2 Copper Phthalocyanine G (Longsheng Dye Chemical Co., Ltd.)

[0086] B3 Tetracarboxylic Acid Diimide (Handafei Biotechnology Co., Ltd.)

[0087] B4 3,6-bis(4-chlorophenyl)-2,5-dihydro-pyrrolo[3,4-c]pyrrole-1,4-dione (Handafei Biotechnology Co., Ltd.)

[0088] B5 N-[4-(Aminocarbonyl)phenyl]-4-[[1-[[(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)-amino]carbonyl]-2-oxopropyl]azo]aniline (Nona Technology Co., Ltd.)

[0089] B6 Zinc Phthalocyanine (Wonder Chemical Co., Ltd.)

[0090] Curing agent

[0091] C1 Hexamethylene diisocyanate trimer TPA-90SB (Asahi Chemical)

[0092] C2 butylated polymethylol melamine resin XT-1 (Moore Chemical Co., Ltd.)

[0093] Other additives

[0094] D1 acrylic block copolymer A122 (Juncai Material Technology Co., Ltd.)

[0095] D2 Bis(dimethylaminoethyl)ether BDMAEE (Guangsiyuan Polyurethane Materials Co., Ltd.)

[0096] D3 Acidic group copolymer BYK110 (BYK, Germany)

[0097] D4 p-Toluenesulfonic acid (Yinglang Chemical Co., Ltd.)

[0098] D5 Silicon-containing copolymer NXH-308 (Xuanhao New Materials Co., Ltd.)

[0099] D6 calcium carbonate (Jiangxi Bairui Calcium Carbonate Co., Ltd.)

[0100] D7 Silica (Rui Chuangxin Materials Technology Co., Ltd.)

[0101] D8 zinc oxide (Haishun New Materials Co., Ltd.)

[0102] D9 Stannous Octoate (Hui An Chemical Co., Ltd.)

[0103] The preparation method of the encapsulation sheet is to apply the above coating to the support layer by a coating process, and then dry at 60°C-200°C and roll up to obtain the encapsulation sheet S1-17 and the encapsulation sheet T1-2. The thickness setting method of the support layer and the color layer of the encapsulation sheet S1-17 and the encapsulation sheet T1-2 is shown in Table 2:

[0104] Table 2

[0105]

[0106]

[0107] The support layer is a DS11 series PET film customized by Dongcai Technology Group Co., Ltd. The reflectivity of the support layer is shown in Table 3:

[0108] Table 3

[0109] 400-1200nm Reflectivity E1 60.2% E2 78.4% E3 29.8%

[0110] Test items and test methods

[0111] It should be noted that the above performance indicators are measured by the following methods:

[0112] 1. Transmittance and reflectivity

[0113] The test method refers to the standard GB / T 29848 "Ethylene-vinyl acetate copolymer (EVA) film for photovoltaic module encapsulation"

[0114] There is a spectrophotometer method with an integrating sphere.

[0115] Testing instrument: UV-visible spectrophotometer.

[0116] Test conditions: 200nm~2500nm.

[0117] 2. Surface gloss

[0118] Test method: Use a gloss meter with a measuring angle of 60°, place it on the horizontal coating surface, and read the gloss.

[0119] 3. Adhesion

[0120] The test method refers to the standard GB / T 31034 "Insulating backsheet for crystalline silicon solar cell modules";

[0121] Sample size: 200mm*200mm;

[0122] Test conditions: +25℃, 50%RH.

[0123] 4. Constant resistance to moisture and heat aging

[0124] The test method refers to the standard GBT31034-2014 "Insulating backsheet for crystalline silicon solar cell modules".

[0125] Test conditions: +85℃, relative humidity 85%.

[0126] 5. UV resistance

[0127] The test method refers to the standard GBT31034-2014 "Insulating backsheet for crystalline silicon solar cell modules".

[0128] Test conditions: +60℃, 320-400nm.

[0129] 6. Photovoltaic device power attenuation

[0130] The power test method refers to the standard IEC61215 "Terrestrial crystalline silicon photovoltaic modules - Design identification and finalization".

[0131] Sample size: bifacial cells, 72 modules.

[0132] Test conditions: AM 1.5, irradiance 1000W / m2, +25℃, 50%RH.

[0133] Power attenuation rate = (initial power - power after aging) / initial power * 100%.

[0134] 7. Surface hardness test

[0135] The test method refers to the standard GB / T6739-1996 "Coating Hardness Pencil Test Method".

[0136] 8. Dark crosslinking test

[0137] The test was conducted by heating and extracting with butanone. The ratio of the mass not dissolved by butanone to the initial mass was the crosslinking degree. The arithmetic mean of the three samples was taken in %.

[0138] 9. Glass transition temperature test

[0139] The test method refers to the standard GB / T 19466.2-2004 Plastics Differential Scanning Calorimetry (DSC) Part 2: Determination of glass transition temperature.

[0140] The test results of the performance parameters of the encapsulation sheets S1-17 and T1-2 are shown in Tables 4 and 5.

[0141] Table 4

[0142]

[0143] Table 5

[0144]

[0145]

[0146] Preparation of photovoltaic devices:

[0147] The encapsulation sheet S1-13 and the encapsulation sheet T1-2 are arranged and laminated as follows to prepare a photovoltaic device: the component adopts a 3.2mm photovoltaic glass / 0.45mm F406PS (Foster) / 182P-per half-cell / 0.45mm F806PS (Foster) / the encapsulation sheet laminated structure, and is prepared after lamination at 145°C for 18 minutes. The relevant properties of the photovoltaic device are shown in Table 6:

[0148] Table 6

[0149] Example Component power attenuation S1 3.2% S2 5.8% S3 6.0% S4 2.8% S5 2.1% S6 1.2% S7 1.8% S8 4.8% S9 2.9% S10 4.2% S11 5.8% S12 3.4% S13 3.8% S14 3.2% S15 2.9% S16 5.5% S17 7.7% T1 9.3% T2 8.2%

[0150] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0151] It can be seen from Table 1-6 that the performance of encapsulation sheet S1-17 is substantially better than that of encapsulation sheet T1-2. In particular, when the encapsulation sheet is used for a photovoltaic backplane and for encapsulation of photovoltaic devices, it can effectively reduce the power attenuation of photovoltaic devices.

[0152] Specifically, according to the performance parameters between T1 and S1, S9-11, and S16, it can be intuitively seen that the coating thickness of the color layer has a certain influence on the power attenuation of the photovoltaic device. It basically shows that as the thickness of the color layer increases, the power attenuation effect of the photovoltaic device increases, especially when the thickness of the color layer exceeds 30μm, the power of the photovoltaic device significantly decays. The increase in the thickness of the color layer causes the defect of color stability of the encapsulation sheet. It can be intuitively seen that as the thickness of the color layer increases, the ΔE*ab of the encapsulation sheet has increased significantly. In addition to the deterioration of the appearance performance, considering the difference in reflectivity caused by the migration of pigments in the color layer and the deterioration of the internal environment of the component, the power attenuation of the photovoltaic device increases. As the thickness of the color layer increases, the overall reflectivity of the packaging sheet shows a decreasing trend. The increase in the thickness of the color layer will reduce the transmittance of the color layer to light of each band. Therefore, as the thickness of the color layer increases, the resistance to UV yellowing is improved to a certain extent. The thickness of the color layer in the packaging sheet T2 reaches 50μm. At this time, the peel strength and adhesion of the packaging sheet are significantly reduced. Considering that the thickness of the color layer is too large, the color layer inside cannot withstand the stress and starts to tear from the inside of the color layer; the color layer thickness of the packaging sheet S17 is 1μm, which is relatively high in production cost and difficult in process. In addition, if the thickness of the color layer is too low, the adhesion between the color layer and the support layer and the peel strength between the packaging sheet and the film will both decrease.

[0153] Specifically, it can be seen intuitively from the performance parameters of the encapsulation sheets S1-7, S17 and T2 that the coating formula of the color layer has a significant impact on the performance of the final encapsulation sheet. It can be seen from S1-7, S17 and T2 that the hydroxyl value of the resin type used in T2 is too low, less than 40mgKOH / g, and the hardness of the color layer is only 1. Considering the low degree of crosslinking inside the color layer, the pigment in the color layer is very easy to migrate, resulting in a significant increase in the ΔE*ab of the encapsulation sheet, which in turn causes an increase in the power attenuation of the photovoltaic device.

[0154] The performance parameters of encapsulation sheet S1 and encapsulation sheets S12 and 13 can be seen intuitively. Generally, the performance of encapsulation sheets changes with the type and thickness of the support layer. In particular, the support layer thickness of encapsulation sheet S13 reaches 300μm. Although the light reflectivity is excellent and there is a certain gain in the power generation of photovoltaic devices, the heat dissipation of PET itself is poor. As the thickness of the PET support layer increases, the internal working environment of the component is poor, and the power attenuation of the photovoltaic device will increase.

[0155] It can be seen from the encapsulation sheets S3, S5, and S7 that the inorganic filler in the color layer coating has a great influence on the glossiness of the color layer. The color layer needs to maintain a certain amount of inorganic filler. As the content of inorganic filler increases, the glossiness of one side of the color layer of the encapsulation sheet decreases, that is, the better the appearance performance, the less likely it is to have obvious scratches and other defects.

[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A packaging sheet for packaging photovoltaic devices, characterized in that: The encapsulation sheet comprises a support layer and a color layer arranged on at least one side surface of the support layer; The thickness of the color layer is 1-30 μm; The surface hardness of the color layer is not less than 2H; The encapsulation sheet satisfies the following conditions: the encapsulation sheet is stacked and laminated in the manner of encapsulation sheet + EVA film + glass to obtain a laminate, the laminate is subjected to damp heat aging at 85°C & 85% humidity for 2000 hours, the color difference ΔE*ab of the laminate before and after aging is tested, and the laminate satisfies ΔE*ab not higher than 10, and the hydroxyl value of the resin in the color layer is greater than 40 mg KOH / g; the color layer is coated with a coating, the coating contains a resin, a pigment, an additive and a solvent, and the mass ratio of the resin to the pigment in the coating is 8~19:

1.

2. The encapsulation sheet according to claim 1, characterized in that: The glass transition temperature of the color layer is 20-80°C.

3. The encapsulation sheet according to claim 1, characterized in that: The degree of crosslinking of the color layer is not less than 75%.

4. The encapsulation sheet according to claim 1, characterized in that: The thickness of the support layer is 100-300 μm.

5. The encapsulation sheet according to claim 1, characterized in that: The average reflectivity of the surface of the color layer of the packaging sheet away from the support layer in the range of 400-1200nm is higher than 30%.

6. The encapsulation sheet according to claim 1, characterized in that: The glossiness of the surface of the color layer away from the support layer is 25-85 GU.

7. The encapsulation sheet according to claim 1, characterized in that: The resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, and phenolic resin; The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

8. A method for preparing a packaging sheet, characterized in that: The preparation method is used to manufacture the encapsulation sheet as described in any one of claims 1 to 7, wherein the resin, additives, pigments and solvents are evenly mixed into a coating, which is applied to at least one side of the support layer using a coating process and dried at 60°C-200°C to obtain the encapsulation sheet.

9. A photovoltaic device, characterized in that: The photovoltaic device comprises a photovoltaic front panel, a first photovoltaic adhesive film, a battery layer, a second photovoltaic adhesive film and a photovoltaic back panel, and the photovoltaic back panel comprises the encapsulation sheet according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Polyolefin photovoltaic backsheet comprising a stabilized polypropylene layer

    CN106661289A

  • Weather-resistant paint, weather-resistant coating, photovoltaic backboard and preparation method thereof

    CN111440528A