Highly exposed platinum nanocluster HER electrocatalyst and its preparation method and application
The preparation of highly exposed ligand-free platinum nanocluster HER electrocatalysts through electrochemical reduction-assisted photodecomposition method, solving the sintering and agglomeration problems caused by calcination of platinum nanoclusters at high temperature in the prior art, and realizing the acidic environment The high activity and low overpotential have industrial application value.
Patent Information
- Application Number
- CN202211008916.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-08-22
AI Technical Summary
The prior art When preparing platinum nanocluster HER electrocatalysts with high exposure without ligands, it is prone to sintering and cluster agglomeration due to high temperature calcination, which limits the stability and activity of the catalyst, and the high cost and scarcity of precious metal platinum. Limits its application.
Using electrochemical reduction-assisted photodecomposition method, irradiation of platinum precursor solution by ultraviolet lamp, combined with carbon support and nafion solution, ultrasonic and electrochemical reduction treatment were performed to prepare a highly exposed platinum nanocluster HER electrocatalyst with no ligand .
Ultra-low overpotential and high-quality activity in acidic environments and lower operating voltages in PEMWE devices, showing excellent stability and industrial application prospects.
Smart Images

Figure CN115386897B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of hydrogen energy, and in particular relates to a high-exposed platinum nanocluster HER electrocatalyst and a preparation method and application thereof. Background Art
[0002] As the cleanest fuel, hydrogen is considered one of the most promising energy sources in the 21st century. However, most of the hydrogen currently produced comes from steam methane reforming, which comes from fossil reserves and produces a large amount of carbon dioxide. Electrocatalytic hydrogen production (HER) is a promising alternative method that can replace the current fossil fuel-based energy system that emits carbon dioxide, while achieving efficient energy conversion and storage of intermittent energy sources (such as wind power, solar energy). However, in an acidic environment, precious metal platinum is still widely used as HER catalyst due to the limitations of reaction kinetics and stability. But the high cost and scarcity of precious metal platinum severely limit its commercial application. Therefore, it is crucial to develop low-platinum HER catalysts and reduce catalyst loading while maintaining high activity.
[0003] Platinum cluster catalysts take into account the characteristics of high reactivity and high atomic utilization, and are a new type of catalyst with development prospects. However, so far, obtaining high-exposure, ligand-free stable platinum nanoclusters is still a challenging topic. In terms of methodology, platinum nanoclusters are generally synthesized by solvothermal method, which is a method of preparing metal nanoclusters protected by end-capping agents by mixing metal precursors with a solution containing end-capping agents and adding a reducing agent (J.Am.Chem.Soc., 2014, 136, 1782). However, the end-capping agents introduced during the synthesis process often cover the active surface and even poison the catalyst. In order not to affect the catalytic activity, the obtained metal nanoclusters are generally roasted at high temperature for several hours to remove the end-capping agent. And the removal of ligands by high-temperature roasting often causes sintering, resulting in cluster agglomeration (Adv.Mater.2020, 32, 1901349). Therefore, the development of a simple high-exposure platinum nanocluster HER electrocatalyst is of great significance for the development of hydrogen production reactions. Summary of the invention
[0004] The purpose of the present invention is to provide a highly exposed platinum nanocluster HER electrocatalyst and its preparation method and application, and to prepare a highly exposed and surface ligand-free platinum nanocluster HER electrocatalyst by electrochemical reduction-assisted photolysis, which effectively solves the shortcomings of the existing preparation process. In the acidic HER test, it shows ultra-low overpotential and ultra-high mass activity, and has excellent stability. In the PEMWE device demonstration, it has a lower operating voltage than commercial Pt / C, and is a new type of HER catalyst with industrial application prospects.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a method for preparing a high-exposed platinum nanocluster HER electrocatalyst, comprising the following steps:
[0007] (1) When the platinum-containing precursor solution is irradiated with an ultraviolet lamp, the color of the solution deepens and the Tyndall phenomenon occurs;
[0008] (2) mixing the solution obtained in step (1) with the carbon support, stirring for adsorption, filtering and drying to obtain a black powder;
[0009] (3) The black powder described in step (2) is mixed with a nafion solution, subjected to ultrasound, and the resulting slurry is drop-coated on a glassy carbon electrode and subjected to electrochemical reduction to obtain a high-exposed platinum nanocluster HER electrocatalyst.
[0010] Furthermore, the platinum-containing precursor in step (1) is one or more of H2PtCl6, Na2PtCl6, and K2PtCl6.
[0011] Furthermore, the platinum-containing precursor solution in step (1) is a 3-5 mg / mL H2PtCl6 solution.
[0012] Furthermore, the platinum-containing precursor solution in step (1) is a 3-5 mg / mL H2PtCl6 aqueous solution.
[0013] Furthermore, the wavelength of the emitted light of the ultraviolet lamp in step (1) is in the range of 240 nm to 285 nm, and the power density is in the range of 1 to 3 mW cm -2 ; The ultraviolet lamp irradiation time in step (1) is 20 to 60 minutes.
[0014] Furthermore, the power density of the UV lamp in step (1) is 1 mW cm -2 ; The ultraviolet light irradiation time in step (1) is 20 minutes.
[0015] Furthermore, the entire operation process of step (2) is carried out in the dark.
[0016] Furthermore, the stirring and adsorption time in step (2) is 1 to 4 hours.
[0017] Furthermore, the stirring and adsorption time in step (2) is 1 to 3 hours.
[0018] Furthermore, the stirring adsorption time in step (2) is 2 hours; the drying in step (2) is freeze-drying, and the drying time in step (2) is 24 to 48 hours.
[0019] Furthermore, the drying time in step (2) is 24 hours.
[0020] Furthermore, the carbon carrier in step (2) is Cabot carbon black Vulcan XC-72 or carbon nanotubes CNT; and the mass ratio of platinum to carbon carrier is 1:30 to 1:150.
[0021] Furthermore, the mass of the carbon carrier in step (2) is 50 to 250 mg.
[0022] Furthermore, the carbon carrier in step (2) is 50 to 100 mg of Cabot carbon black Vulcan XC-72.
[0023] Furthermore, the nafion solution in step (3) is a 0.5wt.% to 1.5wt.% nafion ethanol mixed solution, and the preparation step includes: mixing a commercial nafion solution with an ethanol solution, stirring evenly, to obtain a 0.5wt.% to 1.5wt.% nafion ethanol mixed solution.
[0024] Furthermore, the nafion solution in step (3) is a 0.84wt.% nafion ethanol mixed solution, and the preparation steps include: taking 20g of commercial 5.0% nafion solution and mixing it with 100g of anhydrous ethanol solution, stirring evenly to obtain a 0.84wt.% nafion ethanol mixed solution.
[0025] Furthermore, the ratio of the mass of the black powder in step (3) to the volume of the nafion solution is 1:100 to 1:50 mg / μL; and the ultrasonic time in step (3) is 30 to 60 min.
[0026] Furthermore, the ratio of the mass of the black powder in step (3) to the volume of the nafion solution is 1:50 mg / μL; and the ultrasonic time in step (3) is 30 min.
[0027] Furthermore, the volume of the nafion solution in step (3) is 250 to 500 μL.
[0028] Furthermore, in step (3), the diameter of the glassy carbon electrode is 5.0 mm and the electrode area is 0.2 cm 2 .
[0029] Furthermore, the electrochemical reduction operation in step (3) comprises the following steps: applying the slurry in step (3) dropwise onto a glassy carbon electrode with a diameter of 5.0 mm, allowing it to dry naturally, and then irradiating it with an infrared lamp for 3 to 5 minutes to allow the solid to be firmly adsorbed on the electrode surface. A saturated calomel electrode (SCE) and a gold wire are used as a reference electrode and a counter electrode, respectively. The electrolyte solution is a 0.05 to 0.5 MH2SO4 aqueous solution. Within a voltage range of 0 to -0.4 V relative to the saturated calomel electrode, the reaction mixture is heated to 50 mV s -1Scan 10 to 50 times.
[0030] The present invention provides a highly exposed platinum nanocluster HER electrocatalyst prepared by the above-mentioned preparation method. The photodecomposition characteristics of chloroplatinic acid are utilized to prepare a platinum nanocluster HER electrocatalyst with a particle size of 1.1 nm, high exposure and no ligand protection by using an electrochemical reduction-assisted photodecomposition method.
[0031] The present invention provides an application of a highly exposed platinum nanocluster electrocatalyst in electrocatalytic hydrogen production (HER). Under acidic conditions, at a current density of 10 mA cm -2 The PEMWE device assembled as the cathode exhibited an excellent voltage advantage at 1A cm -2 At a hydrogen production current density of 1.74 V, only an external voltage of 1.74 V is required. It is a new type of HER electrocatalyst with industrial application prospects.
[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0033] (1) The present invention provides a method for preparing a highly exposed platinum nanocluster HER electrocatalyst. This method is a new electrochemical reduction-assisted photodecomposition method for preparing highly exposed platinum nanoclusters. The preparation process is all in an aqueous environment, without the involvement of organic solvents, and is green and environmentally friendly. The method has simple steps, easy operation, and controllable product morphology. It has broad applicability and application prospects.
[0034] (2) The preparation method of the high-exposed platinum nanocluster HER electrocatalyst provided by the present invention does not involve the addition of surfactants or capping agents during the preparation process. The obtained high-exposed platinum nanocluster HER electrocatalyst has no ligand protection, and the active sites can be fully utilized.
[0035] (3) The high-exposed platinum nanocluster HER electrocatalyst provided by the present invention has ultra-high mass activity and high atomic utilization.
[0036] (4) The high-exposed platinum nanocluster HER electrocatalyst provided by the present invention is used in acidic electrocatalytic hydrogen production. It utilizes the characteristics of high exposure and high intrinsic activity of its active sites to have excellent electrocatalytic activity and ultra-high mass activity for acidic HER reactions. As a cathode in a PEMWE device, it has a lower operating voltage than commercial 20wt.% Pt / C.
[0037] (5) The preparation process of the present invention is simple and convenient, and has broad application prospects in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters / HADDF-STEM image of XC-72.
[0039] Figure 2 The catalyst H-HE-Pt prepared in Example 1 clusters / X-ray photoelectron spectrum of XC-72.
[0040] Figure 3 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters Linear sweep voltammograms of Cabot Carbon Black Vulcan XC-72 and commercial 20wt.% Pt / C.
[0041] Figure 4 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters Mass activity curves of Pt / XC-72 and commercial 20wt.% Pt / C.
[0042] Figure 5 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters / XC-72 and commercial 20wt.% Pt / C water electrolysis curves. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with the accompanying drawings and specific preferred embodiments, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0044] Example 1
[0045] H-HE-Pt clusters / The preparation of XC-72 comprises the following steps:
[0046] (1) Preparation of H-Pt-Cl cluster solution: 0.5 mL of 3.0 mg / mL H2PtCl6 aqueous solution and 20 mL of deionized water were added to a 100 mL beaker and irradiated with a UV lamp for 20 min. The UV lamp had an emission wavelength of 250 nm and a power density of 1 mW cm -2 , the color of the solution deepened, and when irradiated with laser light, the Tyndall phenomenon occurred, and the resulting solution was named H-Pt-Clclusters solution;
[0047] (2) Preparation of H-Pt-Cl clusters / XC-72: Weigh 21.4 mg of Cabot Vulcan XC-72, with a mass ratio of platinum to Cabot Vulcan XC-72 of 1:30, and add the mixture to the H-Pt-Cl clusters solution obtained in step (1). Stir the mixture magnetically for 1 h to ensure that the H-Pt-Cl clusters are adsorbed on the Cabot Vulcan XC-72. Filter the mixture under reduced pressure and freeze-dry it for 24 h to obtain a black powder. The entire step is performed in the dark and protected from light. The obtained black powder is named H-Pt-Cl clusters / XC-72.
[0048] (3)H-HE-Pt clusters Preparation of / XC-72: Add 5mg H-Pt-Clclusters / XC-72 and 500μL 0.5wt.% nafion ethanol mixed solution into a 5mL screw-capped glass bottle, ultrasonicate for 30min to mix the two evenly, take 10μL of the ultrasonicated slurry and drop it on the surface of a 5mm diameter glassy carbon electrode as the working electrode, wait for it to dry naturally, and use an infrared lamp to irradiate for 3 minutes to make the solid firmly adsorbed on the electrode surface. A saturated calomel electrode (SCE) and a gold wire are used as the reference electrode and the counter electrode, respectively. The electrolyte solution is a 0.1M H2SO4 aqueous solution. In the voltage range of 0 to -0.4V relative to the saturated calomel electrode, the voltage is 5mV s -1 After 15 scans, a highly exposed platinum nanocluster HER electrocatalyst was obtained, named H-HE-Pt clusters / XC-72.
[0049] Figure 1 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters HADDF-STEM (High Angle Annular Dark Field Scanning Transmission Electron Microscope) image of / XC-72. Figure 1 It can be seen that the highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt clusters / The average particle size of XC-72 is 1.1nm, and no agglomeration occurs.
[0050] Figure 2 The catalyst H-HE-Pt prepared in Example 1 clusters / XC-72 X-ray photoelectron spectrum, by Figure 2 It can be seen that as the scanning continues, the Cl species content gradually decreases and disappears completely after 15 cycles. This shows that the highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters / The surface of XC-72 is not covered with ligand.
[0051] Example 2
[0052] Na-HE-Pt clusters / The preparation of XC-72 comprises the following steps:
[0053] (1) Preparation of Na-Pt-Cl cluster solution: 0.5 mL of 4.0 mg / mL Na2PtCl6 aqueous solution and 20 mL of deionized water were added to a 100 mL beaker and irradiated with a UV lamp for 40 min. The UV lamp had an emission wavelength of 270 nm and a power density of 2.0 mW cm -2 , the color of the solution deepened, and when irradiated with laser light, the Tyndall phenomenon occurred, and the resulting solution was named Na-Pt-Cl clusters solution;
[0054] (2) Preparation of Na-Pt-Cl clusters / XC-72: Weigh 51.6 mg of Cabot Vulcan XC-72, with a mass ratio of platinum to Cabot Vulcan XC-72 of 1:60, and add it to the Na-Pt-Cl clusters solution obtained in step (1), and stir magnetically for 3 h to ensure that the Na-Pt-Cl clusters are adsorbed on the carbon carrier Cabot Vulcan XC-72, and filter under reduced pressure and freeze-dry for 36 h to obtain a black powder. The entire step is performed in the dark and protected from light. The obtained black powder is named Na-Pt-Cl clusters / XC-72;
[0055] (3)Na-HE-Pt clusters Preparation of / XC-72: Add 5mg Na-Pt-Clclusters / XC-72 and 400μL 1.0wt.% nafion ethanol mixed solution into a 5mL screw-capped glass bottle, and mix them evenly by ultrasonication for 45min. Take 10μL of the slurry after ultrasonication and apply it on the surface of a 5mm diameter glassy carbon electrode as the working electrode. After it is dried naturally, use an infrared lamp to irradiate for 4 minutes to make the solid firmly adsorbed on the electrode surface. A saturated calomel electrode (SCE) and a gold wire are used as the reference electrode and the counter electrode, respectively. The electrolyte solution is a 0.25M H2SO4 aqueous solution. In the voltage range of 0 to -0.4V relative to the saturated calomel electrode, the reaction mixture is heated at 20mV s -1 After 10 scans, a highly exposed platinum nanocluster HER electrocatalyst was obtained, named Na-HE-Pt clusters / XC-72.
[0056] Example 3
[0057] K-HE-Pt clusters The preparation of CNT includes the following steps:
[0058] (1) Preparation of K-Pt-Cl cluster solution: 0.5 mL of 5.0 mg / mL K2PtCl6 aqueous solution and 20 mL of deionized water were added to a 100 mL beaker and irradiated with a UV lamp for 60 min. The UV lamp had an emission wavelength of 285 nm and a power density of 3.0 mW cm -2 , the color of the solution deepened, and when irradiated with laser light, the Tyndall phenomenon occurred, and the resulting solution was named K-Pt-C1clusters solution;
[0059] (2) Preparation of K-Pt-C1 clusters / CNT: Weigh 150.5 mg of carbon nanotubes (CNT), with a mass ratio of platinum to carbon nanotubes (CNT) of 1:150, add to the K-Pt-Cl clusters solution obtained in step (1), stir magnetically for 4 h to ensure that K-Pt-C1 clusters are adsorbed on the carbon nanotubes (CNT), filter under reduced pressure and freeze-dry for 48 h to obtain a black powder. The entire step is performed in the dark and protected from light. The obtained black powder is named K-Pt-Cl clusters / CNT.
[0060] (3) K-HE-Pt clusters Preparation of / CNT: Add 5mg K-Pt-C1clusters / CNT and 250μL 1.5wt.% nafion ethanol mixed solution into a 5mL screw-capped glass bottle, ultrasonicate for 60min to mix the two evenly, take 10μL of the ultrasonicated slurry and drop it on the surface of a 5mm diameter glassy carbon electrode as the working electrode, wait for it to dry naturally, and irradiate it with an infrared lamp for 5 minutes to make the solid firmly adsorbed on the electrode surface. The saturated calomel electrode (SCE) and gold wire are used as the reference electrode and counter electrode respectively, and the electrolyte solution is a 0.5M H2SO4 aqueous solution. In the voltage range of 0 to -0.4V relative to the saturated calomel electrode, the voltage is 50mV s -1 After 50 scans, a highly exposed platinum nanocluster HER electrocatalyst was obtained, named K-HE-Pt clusters / CNT.
[0061] H-HE-Pt prepared in Example 1 clusters / XC-72 and comparative Cabot carbon black Vulcan XC-72, commercial 20wt.% Pt / C as HER electrocatalyst in PEMWE:
[0062] (1) Acidic HER test was performed on a CHI 660e electrochemical workstation. clusters / XC-72 and Cabot carbon black Vulcan XC-72 for comparison, commercial 20wt.% Pt / C as working electrode, saturated calomel electrode (SCE) and gold wire as reference electrode and counter electrode respectively. The electrolyte solution is 0.5M H2SO4 solution saturated with H2. In the test voltage range of 0~-0.4V (vs.SCE) relative to saturated calomel electrode, the -1 Cyclic voltammetry scans were performed for 10 cycles with the rotating disk speed at 1600 rpm.
[0063] (2) The demonstration of the proton exchange membrane water electrolyzer (PEMWE) device was carried out on a Gamry electrochemical workstation, using a two-electrode system, in which the carbon paper loaded with catalyst was used as the cathode and the porous titanium mesh loaded with IrO2 was used as the anode. Titanium plates were used as bipolar plates, nafion 212R membranes were used as diaphragms, and ultrapure water was passed through both ends. The preparation method of the carbon paper loaded with catalyst was as follows: the mass ratio of nafion solution to catalyst was 1:9, and the mass ratio of catalyst to carbon paper area was 1:10 mg / cm 2 The volume ratio of ethanol to water was 1:1, and the mixture was coated on carbon paper after ultrasonic treatment for 30 min. The final catalyst loading was 0.1 mg cm -2 .
[0064] (3) The preparation method of the titanium mesh loaded with IrO2 is as follows: the mass ratio of the nafion solution to the catalyst is 1:9, and the mass ratio of IrO2 to the area of the titanium mesh is 2:1 mg / cm 2 The volume ratio of ethanol to water was 1:1, and the titanium mesh was coated after ultrasonication for 30 min. The final IrO2 loading on the titanium mesh was 2.0 mg cm -2 .
[0065] Figure 3 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters Linear sweep voltammetry curves of Pt / C, Cabot Carbon Black Vulcan XC-72 and commercial 20wt.%Pt / C, Figure 3 It can be seen that at a current density of 10 mA cm -2 The highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters The HER overpotentials of Pt / C were 18 mV, >100 mV and 38 mV, respectively. clusters The HER activity of / XC-72 is significantly higher than that of several other catalysts, indicating that the high-exposed Pt nanocluster HER electrocatalyst H-HE-Ptclusters / XC-72 has excellent HER activity.
[0066] Figure 4 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters Mass activity curves of / XC-72 and commercial 20wt.%Pt / C, by Figure 4 It can be seen that in the entire voltage range, the high-exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters The mass activity of / XC-72 is higher than that of commercial 20wt.%Pt / C, and at 50mV overpotential, the high-exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters The mass activity of / XC-72 is 147 times that of commercial 20wt.% Pt / C, which is one of the highest levels reported in the current literature. clusters / XC-72 has the characteristics of high exposure and high atomic utilization.
[0067] Figure 5 Highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters / XC-72 and commercial 20wt.%Pt / C electrolysis curves. Figure 5 It can be seen that at a current density of 1A cm -2 The highly exposed platinum nanocluster HER electrocatalyst H-HE-Pt prepared in Example 1 clusters The PEMWE operating voltages of / XC-72 and commercial 20wt.%Pt / C are 1.74V and 1.95V, respectively. This indicates that the highly exposed Pt nanocluster HER electrocatalyst H-HE-Pt clusters / XC-72 has excellent catalytic activity as a cathode material for PEMWE and has potential industrial application value.
[0068] The above embodiments are only preferred implementation modes of the present invention and are only used to explain the present invention rather than to limit the present invention. Any changes, substitutions, modifications, etc. made by those skilled in the art without departing from the spirit of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a highly exposed platinum nanocluster HER electrocatalyst, characterized in that: The steps include: (1) Using ultraviolet light to irradiate a platinum-containing precursor solution, the color of the solution deepens and the Tyndall phenomenon occurs; the platinum-containing precursor is one or more of H2PtCl6, Na2PtCl6, and K2PtCl6; (2) mixing the solution obtained in step (1) with the carbon carrier, stirring for adsorption, filtering and drying to obtain a black powder; The entire process in step (2) is carried out in the dark, wherein the stirring adsorption time is 1 to 4 hours; the drying is freeze drying, and the drying time is 24 to 48 hours; the carbon carrier is Cabot carbon black Vulcan XC-72 or carbon nanotubes CNT; the mass ratio of platinum to carbon carrier is 1:30 to 1:150; (3) mixing the black powder in step (2) with a nafion solution, ultrasonicating, and drop-coating the resulting slurry on a glassy carbon electrode, followed by electrochemical reduction to obtain a highly exposed platinum nanocluster HER electrocatalyst; The electrochemical reduction operation in step (3) comprises: using a saturated calomel electrode and a gold wire as a reference electrode and a counter electrode, respectively; the electrolyte solution is a 0.05-0.5 M H2SO4 solution; and the voltage is in the range of 0-0.4 V relative to the saturated calomel electrode at a rate of 5-50 mV s -1 Scan 10 ~ 50 circles.
2. The method for preparing a highly exposed platinum nanocluster HER electrocatalyst according to claim 1, characterized in that: The platinum-containing precursor solution in step (1) is a 3-5 mg / mL H2PtCl6 solution.
3. The method for preparing a highly exposed platinum nanocluster HER electrocatalyst according to claim 1, characterized in that: The wavelength of the UV lamp emitted in step (1) is in the range of 240 nm to 285 nm, and the power density is in the range of 1 to 3 mW cm -2 ; The UV light irradiation time in step (1) is 20 to 60 min.
4. The method for preparing a highly exposed platinum nanocluster HER electrocatalyst according to claim 1, characterized in that: The nafion solution in step (3) is a 0.5 wt.% to 1.5 wt.% nafion ethanol mixed solution, and the preparation steps include: mixing a commercial nafion solution with an ethanol solution, stirring evenly, to obtain a 0.5 wt.% to 1.5 wt.% nafion ethanol mixed solution.
5. The method for preparing a highly exposed platinum nanocluster HER electrocatalyst according to claim 1, characterized in that: The ratio of the mass of the black powder in step (3) to the volume of the nafion solution is 1:100 to 1:50 mg / μL; and the ultrasonic time in step (3) is 30 to 60 min.
6. The method for preparing a highly exposed platinum nanocluster HER electrocatalyst according to claim 1, characterized in that: The slurry is dropwise coated on the glassy carbon electrode, and after it is naturally dried, it is irradiated with an infrared lamp for 3 to 5 minutes to allow the solid to be firmly adsorbed on the electrode surface.
7. The high-exposed platinum nanocluster HER electrocatalyst prepared by the preparation method according to any one of claims 1 to 6.
8. Application of the highly exposed platinum nanocluster HER electrocatalyst described in claim 7 in acidic electrocatalyzed hydrogen production reaction and PEMWE demonstration device.