A two-step electrochemical continuous preparation method for graphene oxide
By spatially confining and extruding graphite raw materials through a two-step electrochemical method, the pollution and stability problems of the chemical oxidation method of graphene oxide are solved, and efficient and green continuous preparation of graphene oxide is achieved with high yield and low environment. Influence.
Patent Information
- Application Number
- CN202211197331.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-09-29
AI Technical Summary
In the existing technology, the chemical oxidation method of graphene oxide has problems such as high pollution, easy explosion in the production process, and huge water consumption. In addition, the oxidation prepared by the one-step electrochemical method is insufficient, resulting in the product being easily disconnected and difficult to be applied to large-scale stabilization. Production.
Using a two-step electrochemical method, the graphite raw material is spatially restricted and squeezed during the two-step electrochemical reaction process of intercalation and oxidation to ensure that the reaction anode is stable and continuous during the transmission process, achieving high quality and continuous graphene oxide. , Stable electrochemical preparation.
It achieves high-quality continuous preparation of graphene oxide, reduces electrolyte pollution and water consumption, and avoids the generation of heavy metal ions and toxic gases. The preparation process is simple and easy to scale up, with high yield and high single-layer rate.
Smart Images

Figure HDA0003871040630000011 
Figure HDA0003871040630000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene oxide material preparation, and specifically is a method for continuously preparing graphene oxide by a one- or two-step electrochemical method. Background Art
[0002] Graphene materials have super high electrical conductivity, thermal conductivity, and tensile strength, and have a wide range of applications. Graphene oxide is an important derivative of graphene and is usually used as a precursor for the reduction preparation of graphene materials. At the same time, because the surface of graphene oxide contains a large number of oxygen-containing functional groups (such as hydroxyl, epoxy, and carboxyl), graphene oxide has good dispersibility and assemblability.
[0003] At present, the chemical oxidation method represented by the Hummers method is commonly used for the large-scale preparation of graphene oxide, which uses strong oxidants such as potassium permanganate to oxidize graphite raw materials to prepare graphene oxide. People have never stopped researching chemical oxidation methods, but they have never completely solved the problems of high pollution, explosive production process, and huge water consumption caused by chemical oxidation methods. The electrochemical method for preparing graphene oxide uses electrochemical oxidation to replace highly polluting strong oxidants. It is a green and environmentally friendly preparation method and is considered to be the most promising preparation method to replace chemical oxidation methods.
[0004] The common one-step electrochemical reaction process is simple, but the product generally has the problem of insufficient oxidation. By pre-intercalating the graphite raw material, the oxidation level of graphene oxide prepared by the electrochemical method can be significantly improved. A Chinese invention patent (publication number: CN 107215867 A) discloses a method for continuously preparing graphene oxide microsheets, which uses a graphite material in a continuous state as a reaction positive electrode, and sequentially prepares graphene oxide through intercalation reaction and oxidation stripping reaction. However, the graphite raw material after intercalation has a reduced strength, and the conductive path is easily disconnected during the transmission process, which is difficult to apply to large-scale stable production. Therefore, there is an urgent need for a continuous, efficient and stable two-step electrochemical method for large-scale preparation of graphene oxide. Summary of the invention
[0005] In view of the defects of the prior art, the purpose of the present invention is to propose a two-step electrochemical continuous preparation method of graphene oxide. By spatially confining and squeezing the graphite raw material during the two-step electrochemical reaction of intercalation and oxidation, it is ensured that the reaction anode is stable and continuous during the transmission process and the conductive path is maintained, thereby achieving high-quality, continuous and stable electrochemical preparation of graphene oxide.
[0006] The technical solution of the present invention is:
[0007] A two-step electrochemical continuous preparation method of graphene oxide, using graphite with a macroscopic continuous structure as raw material, the graphite raw material as an anode is limited and squeezed by the space of the conveying device during the conveying process, the cathode and the anode are energized under the condition of electrolyte immersion, and the graphite raw material passes through the intercalation tank and the oxidation tank in sequence, and intercalation reaction and oxidation reaction occur respectively. In the electrochemical reaction, the graphite raw material is used as the anode, and the anode material after the oxidation reaction is completed is stripped and cleaned to obtain the graphene oxide material;
[0008] The device for implementing the method comprises an anode 1, a conductive roller 2, a power source 3, a first guide roller 4, a second guide roller 5, a first conveyor belt 6, a second conveyor belt 7, a third guide roller 8, a conveyor belt buckle 9, an intercalation tank cathode group 10, an oxidation tank electrode group 11, an intercalation electrolyte 12, and an oxidation electrolyte 13. The specific structure is as follows: the anode 1 passes through the conductive roller 2 and enters between the first conveyor belt 6 and the second conveyor belt 7. The first conveyor belt 6 and the second conveyor belt 7 are respectively close to the upper and lower surfaces of the anode 1. The anode 1 is transported by the first conveyor belt 6 and the second conveyor belt 7 and passes through the intercalation electrolyte 12 and the oxidation electrolyte 13 in sequence; the first conveyor belt 6 bypasses the first guide roller 4 and the third guide roller 8 and closes on the upper surface of the anode 1; the second conveyor belt 7 bypasses The second guide roller 5 and the third guide roller 8 are closed on the lower surface of the anode 1; when the first conveyor belt 6 and the second conveyor belt 7 on the lower surface of the anode 1 enter the intercalation electrolyte 12, the first conveyor belt 6 and the second conveyor belt 7 are covered with conveyor belt buckles 9, so that the first conveyor belt 6 and the second conveyor belt 7 limit and squeeze the anode 1 in space. When the first conveyor belt 6 and the second conveyor belt 7 leave the oxidation electrolyte 13, the conveyor belt buckles 9 are removed to release the pressure on the anode 1; the conductive roller 2 is connected to the positive electrode of the power supply 3 through a wire, the intercalation tank cathode group 10 and the oxidation tank cathode group 11 are connected to the negative electrode of the power supply 3 through a wire, and the intercalation tank cathode group 10 and the oxidation tank cathode group 11 are immersed in the intercalation electrolyte 12 and the oxidation electrolyte 13 respectively.
[0009] In the two-step electrochemical continuous preparation method of graphene oxide, the graphite raw material with a macroscopic continuous structure is a sheet or wire prepared from one or a composite of more than two of natural graphite, artificial graphite, block graphite, flake graphite, cryptocrystalline graphite, expanded graphite or graphite powder; the preferred graphite raw material has a density range of 1.0 to 2.0 g / cm 3 Flexible graphite paper.
[0010] In the two-step electrochemical continuous preparation method of graphene oxide, the conveying device includes but is not limited to one or more combinations of a belt conveyor, a roller conveyor, a chain conveyor, a mesh belt conveyor or a suspension conveyor; the movement rate of the graphite raw material relative to the electrolyte is 0 to 100 m / h, preferably in the range of 0.1 cm / h to 50 cm / h.
[0011] In the two-step electrochemical continuous preparation method of graphene oxide, during the conveying process of the graphite raw material, the pressure applied to the graphite raw material by the conveying device is constant or variable, and the pressure ranges to which the graphite raw material is subjected in the intercalation reaction and the oxidation reaction are 0-50MPa and 0-20Mpa respectively.
[0012] In the two-step electrochemical continuous preparation method of graphene oxide, the conveying device applies pressure to the graphite raw material, including but not limited to limiting expansion space, spring tightening, electric pressurization, hydraulic pressurization or pneumatic pressurization, etc., a mixture of one or more of the above methods.
[0013] In the two-step electrochemical method for continuously preparing graphene oxide, the electrolytes in the intercalation tank and the oxidation tank are the same or different, and the electrolyte is a mixture of one or more non-reactive systems of acids or salts; wherein the acid includes but is not limited to sulfuric acid, nitric acid, perchloric acid, phosphoric acid, hydrochloric acid, acetic acid, trifluoroacetic acid, trifluoromethanesulfonic acid, chlorosulfonic acid or magic acid, and the salt includes but is not limited to ammonium sulfate, potassium sulfate, sodium sulfate, magnesium sulfate, potassium perchlorate or sodium persulfide.
[0014] In the two-step electrochemical method for continuously preparing graphene oxide, the electrolyte mass concentration range of the electrolyte in the intercalation tank is 0.01% to 100%, preferably in the range of 60% to 100%; the electrolyte mass concentration range of the electrolyte in the oxidation tank is 0.01% to 100%, preferably in the range of 20% to 85%.
[0015] In the two-step electrochemical method for continuously preparing graphene oxide, the same or different cathode materials are used in the intercalation tank and the oxidation tank; the cathode materials include but are not limited to plates, mesh materials, wire materials or rods corresponding to platinum, copper, nickel, gold or graphite; the relative positions of the anode and the cathode include but are not limited to single cathode and single anode facing each other, two cathodes sandwiching an anode or cathode surrounding the anode, and the surface distance between the anode material and the cathode material ranges from 0.1 mm to 1 m.
[0016] In the two-step electrochemical method for continuously preparing graphene oxide, the voltage applied between the anode and the cathode is a continuous DC voltage, a pulsed DC voltage or an AC voltage, and the voltage range is 0.1 to 10 kV, preferably in the range of 1 to 100 V.
[0017] The two-step electrochemical method for continuously preparing graphene oxide comprises a method for stripping the anode material after the oxidation reaction is completed, including a combination of one or more methods such as mechanical shearing, ultrasonic crushing, and high-pressure homogenization; and a method for cleaning the anode material after the oxidation reaction is completed comprises a combination of one or more methods such as centrifugal cleaning, filter press cleaning, cross-flow cleaning, etc.
[0018] The technical principle of the present invention is:
[0019] In the process of preparing graphene oxide by two-step electrochemical method, the graphite raw material serves as the reaction anode. In the intercalation reaction, the intercalator ions enter the graphite interlayer under the action of the electric field to form first-order or low-order graphite interlayer compounds. Due to the influence of intercalation and immersion, the strength of the intercalated graphite raw material decreases. In order to achieve continuous and stable preparation by two-step electrochemical method, the present invention spatially restricts and squeezes the graphite raw material in the transmission process, so that the graphite raw material after intercalation still maintains a complete structure and the conductive path is not affected, and can enter the next oxidation reaction process.
[0020] The graphite interlayer compound enters the oxidation tank and undergoes an oxidation reaction. The oxidant contains water molecules. During the electrolysis process, free radical ions are generated during the decomposition of water molecules, which oxidize the graphite interlayer compound to generate oxygen-containing functional groups. At the same time, the oxygen produced by the anode during the electrolysis process enters the graphite interlayer, increasing the interlayer spacing of the graphite interlayer compound. By spatially restricting and squeezing the graphite raw material, the graphite raw material can always maintain a stable path during the oxidation process, thereby achieving full oxidation.
[0021] After the oxidation reaction is completed, the obtained product is a block of graphene oxide, which is easy to collect, the electrolyte will not be polluted, and can be reused. The collected graphene oxide block is cleaned and peeled off to obtain a single layer of graphene oxide material.
[0022] Advantages and beneficial effects of the present invention:
[0023] 1. The electrolyte of the present invention will not be polluted, can be reused stably for a long time, has low consumption of electrolyte, and the water consumption in the preparation process is less than 40 times the mass of the product.
[0024] 2. The preparation process of the present invention will not introduce heavy metal ions, will not produce toxic and harmful gases, and will not pollute the environment.
[0025] 3. The preparation process of the present invention is continuous, simple and easy to prepare on a large scale.
[0026] 4. The yield of the graphite oxide material prepared by the present invention is 140% to 160%, the monolayer rate of the obtained graphene oxide is greater than 70%, and the carbon source molar ratio can reach 1.3. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of the structure and process of the device used in the present invention;
[0028] Figure 2 is a microstructure photograph of graphene oxide in Example 1;
[0029] In the figure, 1-anode, 2-conductive roller, 3-power supply, 4-first guide roller, 5-second guide roller, 6-first conveyor belt, 7-second conveyor belt, 8-third guide roller, 9-conveyor belt buckle, 10-intercalation tank cathode group, 11-oxidation tank cathode group, 12-intercalation electrolyte, 13-oxidation electrolyte. DETAILED DESCRIPTION
[0030] The present invention is a two-step electrochemical continuous preparation method of graphene oxide. In the specific implementation process, graphite with a macroscopic continuous structure is used as a raw material. The graphite raw material is limited and squeezed by the space of the conveying device during the conveying process. The cathode and the anode are energized under the condition of electrolyte immersion. The graphite raw material passes through the intercalation tank and the oxidation tank in sequence, and intercalation reaction and oxidation reaction occur respectively. In the electrochemical reaction, the graphite raw material is used as the anode, and the anode material after the oxidation reaction is completed is stripped and cleaned to obtain the graphene oxide material;
[0031] As attached Figure 1 As shown: the device for implementing the method includes an anode 1, a conductive roller 2, a power supply 3, a first guide roller 4, a second guide roller 5, a first conveyor belt 6, a second conveyor belt 7, a third guide roller 8, a conveyor belt buckle 9, an intercalation tank cathode group 10, an oxidation tank electrode group 11, an intercalation electrolyte 12, and an oxidation electrolyte 13. The specific structure is as follows: the anode 1 passes through the conductive roller 2 and enters between the first conveyor belt 6 and the second conveyor belt 7. The first conveyor belt 6 and the second conveyor belt 7 are respectively close to the upper and lower surfaces of the anode 1. The anode 1 is transported by the first conveyor belt 6 and the second conveyor belt 7 and passes through the intercalation electrolyte 12 and the oxidation electrolyte 13 in sequence; the first conveyor belt 6 bypasses the first guide roller 4 and the third guide roller 8 and closes on the upper surface of the anode 1; the second conveyor belt 7 bypasses The first conveyor belt 6 and the second conveyor belt 7 on the lower surface of the anode 1 are closed after passing through the second guide roller 5 and the third guide roller 8; when the first conveyor belt 6 and the second conveyor belt 7 on the lower surface of the anode 1 enter the intercalation electrolyte 12, the first conveyor belt 6 and the second conveyor belt 7 are covered with conveyor belt buckles 9, so that the first conveyor belt 6 and the second conveyor belt 7 limit and squeeze the anode 1 in space, and when the first conveyor belt 6 and the second conveyor belt 7 leave the oxidation electrolyte 13, the conveyor belt buckles 9 are removed to release the pressure on the anode 1; the conductive roller 2 is connected to the positive electrode of the power supply 3 through a wire, the intercalation tank cathode group 10 and the oxidation tank cathode group 11 are connected to the negative electrode of the power supply 3 through a wire, and the intercalation tank cathode group 10 and the oxidation tank cathode group 11 are immersed in the intercalation electrolyte 12 and the oxidation electrolyte 13 respectively.
[0032] The accompanying drawings and embodiments of the present invention are used to further describe the specific implementation methods of the present invention in detail. The following three embodiments are used to illustrate the present invention but cannot be used to limit the scope of the present invention.
[0033] Example 1.
[0034] In this embodiment, the anode 1 is graphite paper 1; the power supply 3 is a DC power supply, the intercalation electrolyte 12 is concentrated sulfuric acid (98 wt%) 12, and the oxidation electrolyte 13 is dilute sulfuric acid (70 wt%) 13
[0035] The device used in this embodiment includes graphite paper 1, conductive roller 2, DC power supply 3, first guide roller 4, second guide roller 5, first conveyor belt 6, second conveyor belt 7, third guide roller 8, conveyor belt buckle 9, intercalation tank cathode group 10, oxidation tank cathode group 11, concentrated sulfuric acid (98wt%) 12, dilute sulfuric acid (70wt%) 13. The specific structure is as follows: the graphite paper 1 passes through the conductive roller 2 and enters between the first conveyor belt 6 and the second conveyor belt 7. The first conveyor belt 6 and the second conveyor belt 7 are respectively close to the upper and lower surfaces of the graphite paper 1. The graphite paper 1 is transported by the first conveyor belt 6 and the second conveyor belt 7 and passes through the concentrated sulfuric acid (98wt%) 12 and the dilute sulfuric acid (70wt%) 13 in sequence. The first conveyor belt 6 bypasses the first guide roller 4 and the third guide roller 8 and closes on the upper surface of the graphite paper 1; the second conveyor belt 7 bypasses the second guide roller 5 and the third guide roller 8 and closes on the lower surface of the graphite paper 1. When the first conveyor belt 6 and the second conveyor belt 7 on the lower surface of the graphite paper 1 enter the concentrated sulfuric acid (98wt%) 12, the first conveyor belt 6 and the second conveyor belt 7 are covered with conveyor belt buckles 9, so that the first conveyor belt 6 and the second conveyor belt 7 limit and squeeze the graphite paper 1 in space; when the first conveyor belt 6 and the second conveyor belt 7 leave the dilute sulfuric acid (70wt%) 13, the conveyor belt buckles 9 are removed to release the pressure on the graphite paper 1. The conductive roller 2 is connected to the positive electrode of the DC power supply 3 through a wire, and the intercalation tank cathode group 10 and the oxidation tank cathode group 11 are connected to the negative electrode of the DC power supply 3 through a wire. The intercalation tank cathode group 10 and the oxidation tank cathode group 11 are immersed in the concentrated sulfuric acid (98wt%) 12 and the dilute sulfuric acid (70wt%) 13 respectively.
[0036] In this embodiment, graphite paper with a thickness of 500 microns and a width of 50 cm is used as the graphite raw material, and a graphite plate is used as the reaction anode to form cathode groups 10 and 11. The two graphite plates of each cathode group are respectively located on both sides of the graphite paper in parallel, and the distance between the graphite plate and the surface of the graphite paper is 10 cm. The DC power supply is loaded with a voltage of 5.0V. The transmission speed of the graphite paper relative to the electrolyte is 10cm / h. The anode material after the oxidation reaction is collected, sheared and filtered, and a graphene oxide dispersion can be obtained. Figure 2 As shown, the obtained graphene oxide has a monolayer rate of 80%, a sheet diameter distribution of 1 to 10 microns, a sheet thickness range of 0.5 to 10 nanometers, a carbon-oxygen molar ratio of 1.5, and a yield of 150% from graphite raw material to graphene oxide dispersion.
[0037] Example 2.
[0038] With a density of 1.5 g / cm 3, a carbon rope with a diameter of 8 mm is used as the anode 1, sulfuric acid with a mass fraction of 98% is used as the intercalation electrolyte 12, and an ammonium sulfate aqueous solution with a molar concentration of 1M is used as the oxidation electrolyte 13 to prepare graphene oxide. The other device structures are the same as those in Example 1. The specific preparation parameters of this example are as follows:
[0039] A 10V DC voltage is applied between the cathode and cathode, and the conveyor belt provides a transmission speed of 20cm / h for the graphite raw material. The anode material after the oxidation reaction is completed is collected, and ultrasonic and centrifugal treatment is performed to obtain a graphene oxide dispersion. The obtained graphene oxide has a monolayer rate of 85%, a sheet diameter distribution of 1 to 10 microns, a sheet thickness range of 0.5 to 5 nanometers, and a carbon-oxygen molar ratio of 1.5. The yield from the graphite raw material to the graphene oxide dispersion is 140%.
[0040] Example 3.
[0041] With a density of 1.6 g / cm 3 , a carbon cloth with a width of 40 cm is used as the anode 1, sulfuric acid with a mass fraction of 95% is used as the intercalation electrolyte 12, and sulfuric acid with a mass fraction of 50% is used as the oxidation electrolyte 13 to prepare graphene oxide. The other device structures are the same as those in Example 1. The specific preparation parameters of this embodiment are as follows:
[0042] A 20V DC voltage is applied between the cathode and cathode, and the conveyor belt provides a transmission speed of 30cm / h for the graphite raw material. The anode material after the oxidation reaction is completed is collected, and ultrasonic and centrifugal treatment is performed to obtain a graphene oxide dispersion. The obtained graphene oxide has a monolayer rate of 80%, a sheet diameter distribution of 1 to 20 microns, a sheet thickness range of 0.5 to 5 nanometers, and a carbon-oxygen molar ratio of 2.0. The yield from the graphite raw material to the graphene oxide dispersion is 130%.
[0043] The above results show that the present invention can realize the continuous preparation of graphene oxide, the product is fully oxidized, and it is an efficient, green, low-cost large-scale preparation method of graphene oxide, which has great application value. The above three examples are further explanations of the present invention, in which the transfer device and the spatial restriction and extrusion method of the graphite raw material can be changed and improved in several ways. The changes and improvements that do not depart from the principles of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A two-step electrochemical continuous preparation method of graphene oxide, characterized in that: Graphite with a macroscopic continuous structure is used as a raw material. The graphite raw material is used as an anode and is limited and squeezed by the space of a conveying device during the conveying process. The cathode and the anode are energized under the condition of electrolyte immersion. The graphite raw material passes through an intercalation tank and an oxidation tank in sequence, and an intercalation reaction and an oxidation reaction occur respectively. The anode material after the oxidation reaction is completed is stripped and cleaned to obtain a graphene oxide material. The device for implementing the method comprises an anode (1), a conductive roller (2), a power source (3), a first guide roller (4), a second guide roller (5), a first conveyor belt (6), a second conveyor belt (7), a third guide roller (8), a conveyor belt buckle (9), an intercalation tank cathode group (10), an oxidation tank electrode group (11), an intercalation electrolyte (12), and an oxidation electrolyte (13). The specific structure is as follows: the anode (1) passes through the conductive roller (2) and enters between the first conveyor belt (6) and the second conveyor belt (7); the first conveyor belt (6) and the second conveyor belt (7) are respectively in close contact with the upper and lower surfaces of the anode (1); the anode (1) is transported by the first conveyor belt (6) and the second conveyor belt (7) and passes through the intercalation electrolyte (12) and the oxidation electrolyte (13) in sequence; the first conveyor belt (6) bypasses the first guide roller (4) and the third guide roller (8) and closes on the upper surface of the anode (1); the second conveyor belt (7) ) bypasses the second guide roller (5) and the third guide roller (8) and closes on the lower surface of the anode (1); when the first conveyor belt (6) and the second conveyor belt (7) on the lower surface of the anode (1) enter the intercalation electrolyte (12), the first conveyor belt (6) and the second conveyor belt (7) are covered with conveyor belt buckles (9) so that the first conveyor belt (6) and the second conveyor belt (7) restrict and squeeze the anode (1) in space; when the first conveyor belt (6) and the second conveyor belt (7) leave the oxidation electrolyte (13), the conveyor belt buckles (9) are removed to release the pressure on the anode (1); the conductive roller (2) is connected to the positive electrode of the power source (3) through a wire, the intercalation tank cathode group (10) and the oxidation tank cathode group (11) are connected to the negative electrode of the power source (3) through a wire, and the intercalation tank cathode group (10) and the oxidation tank cathode group (11) are immersed in the intercalation electrolyte (12) and the oxidation electrolyte (13) respectively.
2. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The graphite raw material is a sheet or wire made from one or a composite of two or more of natural graphite, artificial graphite, block graphite, and graphite powder; the graphite raw material has a density ranging from 1.0 to 2.0 g / cm 3 Flexible graphite paper.
3. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The conveying device includes one or more combinations of a belt conveyor, a roller conveyor, a chain conveyor, a mesh belt conveyor or a suspension conveyor; the movement rate of the graphite raw material relative to the electrolyte is 0~1000m / h.
4. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: During the conveying process of the graphite raw material, the pressure applied by the conveying device to the graphite raw material is constant or variable. The pressure ranges to which the graphite raw material is subjected in the intercalation reaction and the oxidation reaction are 0~50MPa and 0~20Mpa respectively.
5. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 4, characterized in that: The conveying device applies pressure to the graphite raw material by means of limiting expansion space, spring tightening, electric pressurization, hydraulic pressurization or pneumatic pressurization, or a combination of one or more of these methods.
6. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The electrolytes in the intercalation tank and the oxidation tank are the same or different, and the electrolyte is selected from one or a mixture of two or more non-reactive systems of acids or salts; the acid includes sulfuric acid, nitric acid, perchloric acid, phosphoric acid, hydrochloric acid, acetic acid, trifluoroacetic acid, trifluoromethanesulfonic acid, chlorosulfonic acid or magic acid, and the salt includes ammonium sulfate, potassium sulfate, sodium sulfate, magnesium sulfate, potassium perchlorate or sodium persulfide.
7. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 6, characterized in that: The electrolyte mass concentration range of the electrolyte in the intercalation tank is 0.01%~100%; the electrolyte mass concentration range of the electrolyte in the oxidation tank is 0.01%~100%.
8. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The same or different cathode materials are used in the intercalation tank and the oxidation tank; the cathode materials include plates, meshes, wires or rods corresponding to platinum, copper, nickel, gold or graphite; the relative positions of the anode and cathode include single cathode and single anode facing each other, two cathodes sandwiching an anode or cathodes surrounding the anode, and the surface distance between the anode material and the cathode material ranges from 0.1mm to 1m.
9. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The voltage applied between the anode and the cathode is a continuous DC voltage, a pulsed DC voltage or an AC voltage, and the voltage range is 0.1~10kV.
10. The method for preparing graphene oxide by two-step electrochemical continuous production according to claim 1, characterized in that: The method for stripping the anode material after the oxidation reaction is completed includes a combination of one or more methods including mechanical shearing, ultrasonic crushing, and high-pressure homogenization. The method for cleaning the anode material after the oxidation reaction is completed includes a combination of one or more methods including centrifugal cleaning, filter press cleaning, and cross-flow cleaning.