I-line single-component photoresist composition, preparation method and pattern forming method thereof
By using a calixarene derivative molecule of diazonaphthoquinone group and a specific solvent combination, the shortcomings of traditional photoresists in high resolution and ultra-thin film layers are solved, and a photoresist with high contrast and low edge roughness is achieved. , suitable for nanoscale pattern preparation, improving the adhesion and film-forming quality of photoresist.
Patent Information
- Application Number
- CN202211011328.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-22
AI Technical Summary
Traditional I-line photoresist is difficult to achieve high resolution, ultra-thin film layer and high film retention rate, and its contrast and adhesion are insufficient to meet the needs of nanoscale pattern preparation.
Calixarene derivative molecules containing diazonaphthoquinone groups are used as single-component photosensitive materials, combined with specific organic solvents and dissolution accelerators, to selectively regulate the branched chain structure to form a photoresist with high contrast and low edge roughness. composition.
It achieves high-resolution, low-roughness ultra-thin film layer coating, which is suitable for I-line interference lithography, near-field lithography and SP lithography. It significantly improves the adhesion and film-forming quality of photoresist and avoids Pinhole defects.
Smart Images

Figure CN115407608B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoresists, and in particular to an I-line (365nm) single-component photoresist composition, a preparation method and a pattern forming method thereof. Background Art
[0002] As the performance requirements of semiconductor devices increase, the critical dimensions of lithography patterns are getting smaller and smaller, which places stringent requirements on lithography technology. Traditional lithography is constrained by the diffraction effect of light and it is difficult to break through the resolution limit below a quarter wavelength. Although the EUV lithography technology currently developed based on the route of continuously shortening the wavelength can achieve a lithography size of 10 nanometers, it is expensive and technically complex, and there are only a handful of institutions and companies that can introduce and meet its supporting conditions. Therefore, it is necessary to develop new lithography technologies that break through the traditional diffraction limit to achieve high-resolution, low-cost nano-graphic imaging.
[0003] Near-field lithography can break the bottleneck of the diffraction limit of traditional resolution, improve the resolution under long-wavelength light sources, and break through the difficulties of current optical lithography technology. However, due to the characteristics of evanescent waves, its practical working distance is greatly limited. The surface plasma primitive (SP) lithography technology developed in recent years has greatly expanded the working distance of near-field lithography, so that the transmission depth of the evanescent wave carrying high-frequency light field information can cover the thickness range of the photoresist film layer, thus having practical application value. At present, it has been reported that the exposure of nano-patterns with a size much smaller than the wavelength of the light source has been successfully achieved by combining an I-line light source with an SP lithography structure design (see Chinese patent CN101726998A).
[0004] However, the current commercial I-line photoresist is mainly based on the diazonaphthoquinone compound's dissolution inhibition effect on phenolic resin materials. The photoresist system has the advantages of high resolution, high contrast, good etching resistance, good heat resistance, stable storage, simple and controllable synthesis method, etc. However, the photoresist designed based on the pattern size and film thickness of the traditional I-line photolithography layer is difficult to meet the requirements of ultra-thin film layer, high film retention rate, high resolution, low roughness, etc. required for high-resolution lithography.
[0005] According to the general relationship between photoresist structure and performance, to achieve high resolution and low roughness, it is necessary to use resin materials with a small molecular weight and a narrow molecular weight distribution. However, on the one hand, the synthesis of phenolic resins with a highly narrow molecular weight distribution is difficult; on the other hand, diazonaphthoquinone compounds have limited inhibitory effects on the dissolution of low molecular weight phenolic resins, which can easily lead to a decrease in film retention and contrast.
[0006] In addition, for the ultra-thin film layer (thickness less than 30nm) required for high-resolution lithography, conventional resin materials are prone to pinhole defects and insufficient adhesion due to interface effects, which seriously affects the quality of lithography. For SP lithography, which requires special substrate materials (mainly metal) and is difficult to flexibly process the substrate surface, the above effects are particularly obvious. Summary of the invention
[0007] 1. Technical issues to be resolved
[0008] In response to the above problems, the present disclosure provides an I-line single-component photoresist composition, a preparation method and a pattern forming method thereof, which are used to solve the technical problems that traditional photoresists are difficult to achieve the ultra-thin film layer required for high-resolution lithography and to achieve high-resolution graphic preparation.
[0009] (II) Technical solution
[0010] The present disclosure provides an I-line single-component photoresist composition for use in I-line high-resolution lithography, comprising: an organic solvent; a single-component photosensitive material, which is a calixarene derivative molecule containing a diazonaphthoquinone group and has a structure shown in Formula I:
[0011]
[0012] Wherein, R1 is a diazonaphthoquinone group or a hydroxyl group, and at least a part of R1 in the structure of Formula I is a diazonaphthoquinone group; R2 is one of a linear alkane chain and its derivatives, a phenyl group and its derivatives; and n is 4, 6 or 8.
[0013] Furthermore, when R2 is a derivative of a linear alkane chain, the length of the linear alkane chain is 2 to 8 carbons, and the end of the linear alkane chain is one of alcohol hydroxyl, carboxyl, epoxy, ether, thioether, ester, and amide substituents.
[0014] Furthermore, when R2 is a derivative of phenyl, the hydrogen on the phenyl group is partially replaced by one of alkyl, hydroxyl, amino and carboxyl groups.
[0015] Furthermore, the grafting rate of the diazonaphthoquinone group in the structure of formula I is 45% to 65%.
[0016] Furthermore, the organic solvent includes a mixture of one or more of n-butyl acetate, ethyl acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and propylene glycol methyl ether.
[0017] Furthermore, the weight percentage of the organic solvent is 85% to 98%.
[0018] Furthermore, the I-line single-component photoresist composition further comprises a mixture of one or more of a dissolution promoter, a leveling agent, a surfactant, and a stabilizer.
[0019] Another aspect of the present disclosure provides a method for preparing an I-line single-component photoresist composition, wherein the single-component photosensitive material in the I-line single-component photoresist composition has a structure shown in Formula I, wherein R1 is a diazonaphthoquinone group or a hydroxyl group, and at least part of R1 in the structure of Formula I is a diazonaphthoquinone group; R2 is one of a linear alkane chain and its derivatives, a phenyl group and its derivatives; n is 4, 6 or 8;
[0020]
[0021] The preparation method comprises: dissolving resorcinol in methanol, adding concentrated hydrochloric acid, dripping a reactant corresponding to the substituent R2, and reacting and purifying to obtain a first product of a calixarene structure; dissolving the first product, dripping triethylamine, and then adding sulfonyl chloride containing a diazonaphthoquinone group, and reacting and purifying to obtain a single-component photosensitive material of formula I structure; dissolving the single-component photosensitive material in an organic solvent, and filtering to obtain an I-line single-component photoresist composition.
[0022] Another aspect of the present disclosure provides a method for pattern formation using an I-line single-component photoresist composition, comprising: cleaning a substrate; optionally coating an adhesion-promoting layer; then coating the aforementioned I-line single-component photoresist composition, and exposing to form a pattern; or plating a metal layer on the substrate; optionally coating an adhesion-promoting layer; then coating the aforementioned I-line single-component photoresist composition, and exposing to form a pattern.
[0023] Another aspect of the present disclosure provides a use of the aforementioned I-line single-component photoresist composition in I-line interference lithography, near-field lithography, and SP lithography.
[0024] (III) Beneficial effects
[0025] The I-line single-component photoresist composition, preparation method and pattern forming method disclosed herein, by using a calixarene derivative molecule containing a diazonaphthoquinone structure, enables the photoresist composition to have the characteristics of high film retention rate and low roughness, can achieve high-quality pinhole-free thin film coating with good adhesion, can form an ultra-thin film layer with a thickness of less than 50nm, achieve nanometer-level resolution, and is suitable for non-traditional high-resolution lithography technologies such as I-line interference lithography, near-field lithography, and SP lithography. Furthermore, by selectively regulating the side chains of calixarene, a pinhole-free ultra-thin film layer with adjustable adhesion and hydrophilicity can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematically shows an electron microscope schematic diagram of comparative example 1 in the present disclosure at a film thickness of 30 nm;
[0027] Figure 2 Schematically shows an electron microscope schematic diagram of comparative example 3 in the present disclosure at a film thickness of 30 nm;
[0028] Figure 3 Schematically shows an electron microscope schematic diagram at a film thickness of 30 nm according to Example 1 of the present disclosure;
[0029] Figure 4 Schematically showing the test results of contact angles according to Examples 1 to 3 and Comparative Example 1 in the present disclosure;
[0030] Figure 5 The result diagram of the SP lithography experiment in Comparative Example 4 according to the present disclosure is schematically shown;
[0031] Figure 6 Schematically shows the result of SP lithography experiment in Example 3 of the present disclosure;
[0032] Figure 7 The result diagram of the SP lithography experiment in Example 4 of the present disclosure is schematically shown;
[0033] Figure 8 The result diagram of the high-resolution interference lithography experiment in Example 3 of the present disclosure is schematically shown. DETAILED DESCRIPTION
[0034] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0035] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0036] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.
[0037] In view of the problem that current commercial I-line photoresist materials are mainly designed for hundreds of nanometers thick and micron-level graphics, and are difficult to meet the requirements for nanometer-level high-resolution graphics preparation, the present disclosure provides an I-line single-component photoresist composition suitable for high-resolution lithography, a preparation method and a pattern forming method thereof.
[0038] The present disclosure provides an I-line single-component photoresist composition, which is applied to I-line high-resolution lithography, comprising: an organic solvent; a single-component photosensitive material, which is a calixarene derivative molecule containing a diazonaphthoquinone group and has a structure shown in Formula I:
[0039]
[0040] Wherein, R1 is a diazonaphthoquinone group or a hydroxyl group, and at least a part of R1 in the structure of Formula I is a diazonaphthoquinone group; R2 is one of a linear alkane chain and its derivatives, a phenyl group and its derivatives; and n is 4, 6 or 8.
[0041] The main component of the I-line single-component photoresist for high-resolution lithography disclosed in the present invention is a calixarene derivative molecule containing a diazonaphthoquinone group (DNQ), which is used as a single-component photosensitive material, and is specifically a molecular glass compound with a sulfonate structure formed by a calixarene derivative with different side chains and a diazonaphthoquinone sulfonyl chloride molecule. As shown in the structure of formula I, R1 is a benzene ring substituent group, R2 is a branched substituent group, and R1 can be Different types of DNQ groups (mainly diazonaphthoquinone sulfonates) or hydroxyl groups, at least part of R1 in the calixarene derivative molecules shown in the structure of formula I is a diazonaphthoquinone group. The above main component is preferably dissolved in an organic solvent as the only component to form the I-line single-component photoresist composition disclosed in the present invention.
[0042] The principle that the I-line single-component photoresist composition disclosed in the present invention can achieve high resolution is as follows: First, the DNQ group in the single-component photosensitive material itself has a strong hydrophobicity, which reacts under ultraviolet exposure to become a strongly hydrophilic carboxylic acid group, achieving a high dissolution contrast, as shown in Formula II. Secondly, in addition to its own hydrophobicity, its DNQ group forms an intermolecular hydrogen bond with the unsubstituted hydroxyl groups on other molecules, achieving the effect of intermolecular dissolution inhibition, further increasing the contrast. Finally, since the entire system is composed of uniform small molecules, the solubility of the product after exposure in the developer is significantly higher than that of traditional phenolic resin molecules, which is also an important factor in forming a high contrast. In summary, since the single-component photosensitive material has the characteristics of "polarity conversion of the molecule itself + mutual dissolution inhibition between molecules + highly soluble small molecule materials", the effects of high contrast, high resolution and low edge roughness of the I-line single-component photoresist composition are achieved.
[0043]
[0044] Based on this, the single-component photoresist composition disclosed in the present invention is based on a calixarene small molecule containing a diazonaphthoquinone group as the main component or even the only component, which can form an ultra-thin film layer with excellent film quality, helps to achieve nanometer-level resolution, and is suitable for non-traditional high-resolution lithography technologies such as I-line interference lithography, near-field lithography, and SP lithography.
[0045] Based on the above embodiments, when R2 is a derivative of a linear alkane chain, the length of the linear alkane chain is 2 to 8 carbons, and the end of the linear alkane chain is one of alcohol hydroxyl, carboxyl, epoxy, ether, thioether, ester, and amide substituents.
[0046] When R2 is a derivative of a linear alkane chain, the end of the linear alkane chain can be selected from alcohol hydroxyl, carboxyl, epoxy, ether, thioether, ester, amide, etc. Among them, the length of the linear alkane chain is 2 to 8 carbons, preferably 5 to 6 carbons. If the carbon chain is too short, pinholes are easily generated. If the carbon chain is too long, sensitivity and adhesion will decrease. When R2 is a linear alkane chain, the length of the linear alkane chain is also 2 to 8 carbons, preferably 5 to 6 carbons.
[0047] Based on the above embodiment, when R2 is a derivative of phenyl, the hydrogen on the phenyl group is partially replaced by one of alkyl, hydroxyl, amino and carboxyl groups.
[0048] When R2 contains at least one benzene ring structure, the hydrogen on the benzene ring may be partially replaced by an alkyl group, a hydroxyl group, an amino group, or a carboxyl group, among which tert-butyl group is preferred.
[0049] The present disclosure can further improve the film-forming properties of photoresist by selectively regulating the substituent group R2 on calixarene. When R2 is a linear alkane chain, for example, when R2 is changed from a short-chain alkane to a long-chain alkane, although its hydrophobicity gradually increases, flexibility is also stronger, and the film layer is more flat and uniform. Hydrophobicity and flexibility work together to effectively solve the problems such as pinholes and adhesion of the film layer. But if the chain length of R2 is too long, the system will cause adhesion to decrease due to excessive hydrophobicity. Therefore, the present disclosure proposes a clear R2 preferential range. When R2 is a substituted phenyl group, the structural rigidity is enhanced, and the etching resistance of the photoresist composition is improved, but the increase of its hydrophobicity also causes the adhesion of the photoresist to decrease to a certain extent. When the substituent is 4-tert-butylphenyl, its film quality can be effectively improved. Therefore, the present disclosure can significantly improve the physical properties such as the film retention rate, film quality (pinholes), and adhesion of the photoresist composition obtained by subsequent preparation by introducing a suitable substituent group in the preparation process of the main component.
[0050] In particular, for SP high-resolution lithography where the substrate requires specific metal materials (such as gold, silver, aluminum, etc.), it is difficult to obtain a highly hydrophobic surface that matches conventional commercial I-line photoresists because the substrate surface cannot be flexibly surface treated. This will lead to a decrease in the quality of the existing commercial photoresist film layer (especially pinhole defects) and adhesion, making it impossible to achieve high-resolution graphics preparation. The single-component photoresist composition disclosed in the present invention can regulate the film layer properties of the obtained photoresist composition by specially selecting the branched structure of the cup-shaped aromatic derivative containing the diazonaphthoquinone structure during the preparation process, and can achieve high-quality pinhole-free thin film coating with good adhesion, as well as the preparation of sub-50nm high-resolution lithography graphics. The present disclosure provides new solutions for ultra-thin film layers, contact angle regulation, and pinhole defect suppression in material structure design, and is suitable for non-traditional high-resolution lithography technologies such as I-line interference lithography, near-field lithography, and SP lithography.
[0051] Based on the above examples, the grafting rate of the naphthoquinone diazide group in the structure of formula I is 45% to 65%.
[0052] The grafting rate of the diazonaphthoquinone group has good lithography performance within this range. A grafting rate that is too low will result in a poor film retention rate, and a grafting rate that is too high will result in poor adhesion.
[0053] Based on the above embodiment, the organic solvent includes a mixture of one or more of n-butyl acetate, ethyl acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and propylene glycol methyl ether.
[0054] The organic solvent can make the photoresist in a liquid state, which is convenient for coating. The single-component photosensitive material is mixed with the organic solvent to form a photoresist composition. The solvent used in the present disclosure can be a component selected from n-butyl acetate, ethyl acetate, γ-butyrolactone, propylene glycol methyl ether acetate (PGMEA), propylene glycol methyl ether and a mixture thereof. The above organic solvent has a good coverage for dissolving a variety of photoresist components with different polarities.
[0055] Based on the above embodiment, the weight percentage of the organic solvent is 85% to 98%.
[0056] The weight ratio range of the above organic solvent is conducive to forming an ultra-thin film layer with a thickness of less than 50 nm. If the solvent ratio is too low, it will be difficult to form an ultra-thin film layer by spin coating.
[0057] Based on the above embodiments, the I-line single-component photoresist composition further includes a mixture of one or more of a dissolution promoter, a leveling agent, a surfactant, and a stabilizer.
[0058] In order to improve the relevant properties of the photoresist composition, a dissolution promoter not exceeding 1% by weight may be optionally added to the formulation, and its composition is preferably a small molecule material containing 2 to 4 phenolic hydroxyl groups (such as bisphenol A, triphenol A), which is used to further adjust the solubility difference between the exposure area and the non-exposure area. If the addition ratio of this component is too large, the film retention rate will decrease, and if the number of phenolic hydroxyl groups is too large, the contrast will decrease and the roughness of the pattern edge will increase.
[0059] In addition, other additives not exceeding 0.1% by weight may be added to the formula, including leveling agents, surfactants, stabilizers, etc., including but not limited to any one or more of small molecule amines, siloxanes, ethylene oxide / propane and fluorinated alkane molecules.
[0060] It should be noted that the above dissolution promoters, leveling agents, surfactants, and stabilizers are not essential components of the I-line single-component photoresist composition disclosed herein, but are only components that can be added in small amounts according to usage requirements.
[0061] In summary, the photoresist composition disclosed in the present invention uses a calixarene derivative molecule containing a diazonaphthoquinone structure as the main component, can achieve high-quality pinhole-free thin film coating with good adhesion, can form an ultra-thin film layer with a thickness of less than 50 nm, and achieve nanometer-level resolution.
[0062] The photoresist formula and the molecular structure control method for film layer characteristics proposed in the present disclosure are different from the existing photoresist system. In terms of lithography resolution and pattern quality, the typical resolution of traditional I-line lithography is above 0.5 microns, and the corresponding photoresist molecular structure is difficult to meet the requirements of nano-level high-resolution lithography technology; while the calixarene derivative molecule containing diazonaphthoquinone groups proposed in the present disclosure is targeted at the new high-resolution I-line lithography technology with a feature size of less than 100 nanometers.
[0063] From the perspective of the photoresist film layer, the photoresist formula and high-quality film layer control method proposed in the present disclosure are applicable to ultra-thin photoresist film layers (below 50 nanometers), which is also compatible with the above-mentioned high-resolution requirements. Traditional commercial I-line photoresist materials are mainly aimed at the film thickness of micrometer level. Even for photoresists with higher resolution, there are problems such as poor film quality, pinhole defects and insufficient film retention rate when forming ultra-thin film layers below 50 nanometers. From the perspective of the photoresist material system, traditional I-line photolithography uses a multi-component photoresist formula with phenolic resin as the main film-forming molecule, while the present disclosure uses a small molecule based on a diazonaphthoquinone group as the main component or even the only component, which has been significantly improved in terms of cost and performance.
[0064] The present disclosure also provides a method for preparing an I-line single-component photoresist composition, wherein the single-component photosensitive material in the I-line single-component photoresist composition has a structure shown in Formula I, wherein R1 is a diazonaphthoquinone group or a hydroxyl group, and at least part of R1 in the structure of Formula I is a diazonaphthoquinone group; R2 is one of a linear alkane chain and its derivatives, a phenyl group and its derivatives; n is 4, 6 or 8;
[0065]
[0066] The preparation method comprises: dissolving resorcinol in methanol, adding concentrated hydrochloric acid, dripping a reactant corresponding to the substituent R2, and reacting and purifying to obtain a first product of a calixarene structure; dissolving the first product, dripping triethylamine, and then adding sulfonyl chloride containing a diazonaphthoquinone group, and reacting and purifying to obtain a single-component photosensitive material of formula I structure; dissolving the single-component photosensitive material in an organic solvent, and filtering to obtain an I-line single-component photoresist composition.
[0067] The present invention uses alkyl and aromatic aldehydes with different chain lengths and containing different groups to react with resorcinol to synthesize a series of calixarene derivatives, and then uses diazonaphthoquinone groups to selectively protect the hydroxyl group to obtain I-line single-component molecular glass photoresists of different structural types. This type of photoresist can effectively regulate the quality and hydrophilicity of the ultra-thin film layer formed by adjusting the regularity of the structure, and effectively suppress pinhole defects.
[0068] The present disclosure also provides a method for pattern formation using an I-line single-component photoresist composition, comprising: cleaning a substrate; optionally coating an adhesion-promoting layer; and then coating the aforementioned I-line single-component photoresist composition, and performing exposure to form a pattern;
[0069] Or plate a metal layer on the substrate; optionally coat an adhesion-promoting layer; and then coat the aforementioned I-line single-component photoresist composition, and perform exposure to form a pattern.
[0070] The semiconductor substrate is cleaned, then coated with an adhesion-promoting layer, and then coated with a prepared photoresist composition, and an exposure process is performed to form a pattern. If applied to SP lithography, the substrate needs to be plated with a metal layer first, and then subjected to an adhesion-promoting treatment and then coated with a photoresist. The material of the adhesion-promoting layer can be commercial HMDS, which can enhance the adhesion between the substrate and the photolithographic material. Among them, the coating of the adhesion-promoting layer is conducive to the film formation of the photoresist composition disclosed in the present invention, but it is not a necessary step.
[0071] The present disclosure also provides an application of the aforementioned I-line single-component photoresist composition in I-line interference lithography, near-field lithography, and SP lithography.
[0072] The photoresist composition disclosed herein is suitable for I-line high-resolution lithography technology with a feature size of less than 100 nm and a film thickness of less than 50 nm, such as I-line interference lithography, near-field lithography, SP lithography, etc. It can form an ultra-thin pinhole-free film layer and has good substrate adhesion.
[0073] The present disclosure is further described below through specific embodiments. The above-mentioned I-line single-component photoresist composition, preparation method and pattern forming method thereof are specifically described in the following examples. However, the following examples are only used to illustrate the present disclosure, and the scope of the present disclosure is not limited thereto.
[0074] 1. Composition of I-line single-component photoresist composition
[0075] The I-line single-component photoresist composition of this embodiment includes an organic solvent and a single-component photosensitive material, wherein the single-component photosensitive material is a calixarene derivative molecule containing a diazonaphthoquinone group, and has a structure shown in Formula I:
[0076]
[0077] Among them, R1 is a diazonaphthoquinone group or a hydroxyl group, and at least a part of R1 in the structure of Formula I is a diazonaphthoquinone group; R2 is one of a linear alkane chain and its derivatives, a phenyl group and its derivatives, and n is 4.
[0078] 2. Preparation method of I-line single-component photoresist composition
[0079] In this embodiment, the preparation method of the I-line single-component photoresist composition is described by taking n=4, R1 being a 1,2-naphthoquinone-2-azide-4-sulfonyl chloride substituent, the grafting rate being 50%, and R2 being a n-hexane substituent as an example.
[0080] In the first step, resorcinol (100 mmol) was dissolved in 50 mL of methanol, and concentrated HCl (17 mL) was added, and then the system was cooled to 0°C, and n-heptanal (105 mmol) was slowly added dropwise to the reaction system using a constant pressure dropping funnel. After the addition was completed, the reaction system was heated to room temperature, and then refluxed for 3 hours. After the reaction was complete, the system was cooled to room temperature, and then 3 times of water was added for precipitation, the solid was filtered out, dried, and then purified by column chromatography to obtain calixarene.
[0081] In the second step, the purified calixarene (2 mmol) is dissolved in a mixed solvent (30 mL) of DMF / Actone = 2 / 1, and the system is cooled to 0°C, and then triethylamine (4 mmol) is added dropwise to the reaction system, and then 1,2-naphthoquinone-2-azide-4-sulfonyl chloride is dissolved in the above mixed solvent and slowly added to the reaction system using a constant pressure dropping funnel, and the reaction system is heated to room temperature and reacted for 24 hours. After the reaction is completed, the mixed system is added to 3 times the amount of water for precipitation, the solid is filtered out, dried, and purified by column chromatography to obtain the final target single-component photosensitive material product, i.e., the main component of the photoresist.
[0082] When R2 is other substituent groups, the corresponding aldehyde can be replaced with the aldehyde derivative required by the corresponding product. When R2 is a special group such as a terminal hydroxyl group, the aldehyde derivative raw material needs to be replaced with the corresponding epoxy olefin; when R2 is a special group such as an ether chain containing multiple oxygens, it is necessary to synthesize a calixarene with a hydroxyl group at the end of R2 by the above method, then protect the phenolic hydroxyl group, then add an ether chain to the end of the alcoholic hydroxyl group, and finally remove the protecting group to obtain the target product. When the grafting rate of calixarene is other values, it is only necessary to adjust the addition ratio of 1,2-naphthoquinone-2-azide-4-sulfonyl chloride in the second step to obtain the target single-component photosensitive material product, that is, the main component of the photoresist.
[0083] Take 3g of the main component of the photoresist synthesized above, dissolve it in 150mL PGMEA, shake it thoroughly to dissolve, and then filter it with a filtration device to obtain a single-component photoresist composition. The solid content of the photoresist can be adjusted according to different thickness requirements. The solubility difference problem of photoresist components with different substituents can be solved by using different solvents.
[0084] When R2 is substituted by other alkyl groups, aryl groups, etc., the above synthesis scheme can also be used. When n is other values and other grafting rates are 45-65%, other schemes are also feasible. For the convenience of comparison, only the case where n is 4 and the DNQ grafting rate is 50% is selected for performance comparison.
[0085] 3. Preparation of photoresist
[0086] Preparation: The formulation of the photoresist composition is adjusted according to different exposure and film thickness requirements, and prepared according to the following scheme. Weigh 5 parts of the main component by weight, dissolve it in 95 parts of solvent (if other additives are added, the solvent ratio is reduced accordingly), ultrasonicate for more than 30 minutes to fully dissolve, and filter with a filter membrane with a pore size of less than 0.2 microns to obtain the I-line single-component photoresist composition disclosed in the present invention. Among them, FC-4430 is a leveling agent purchased from 3M Company.
[0087] The solvent is at least one selected from the following four solvents.
[0088] Solvent 1: Propylene glycol methyl ether acetate (PGMEA)
[0089] Solvent 2: Ethyl lactate
[0090] Solvent 3: Propylene glycol monomethyl ether (PGME)
[0091] Solvent 4: Butyl acetate
[0092] The photoresist compositions prepared in different comparative examples are shown in Table 1:
[0093] Table 1 Photoresist compositions prepared in different examples and comparative examples
[0094]
[0095] 4. Pattern formation and performance test results
[0096] If interference lithography is used, the semiconductor substrate is cleaned, then coated with an adhesion-promoting layer, and then coated with a prepared photoresist composition, and then an exposure process is performed to form a pattern. If SP lithography is used, the substrate is first cleaned, then the substrate is plated with a metal layer, and then an adhesion-promoting layer and a photoresist composition are coated, and then an exposure process is performed to form a pattern. The pattern formation and performance test results are shown in Table 2:
[0097] Table 2 Pattern formation and performance test results of different examples and comparative examples
[0098]
[0099]
[0100] Adhesion and film pinhole test method: Take 100 mL of the photoresist solution in the embodiment, spin-coat it on a 1-inch silicon wafer that has been ultrasonically treated with acetone + alcohol, and then bake it on a hot plate at 100°C for 5 minutes, and then observe the film surface through a scanning electron microscope.
[0101] Adhesion and photolithography pattern quality test: Through normal coating, photolithography, and development, observe with a scanning electron microscope.
[0102] Film retention rate test: Take 100mL of the photoresist solution in the embodiment, spin-coat it on a 1-inch silicon wafer that has been ultrasonically treated with acetone + alcohol, then bake it on a 100℃ hot plate for 5 minutes, soak it in MF-319 developer for 30 seconds, and test the film thickness loss. Loss of 0-3nm is good, 3-10nm is poor, and more than 10nm is poor.
[0103] 1) Film quality
[0104] ①Whether there is a pinhole problem
[0105] Regarding the pinhole problem of the membrane layer, when R2 is a shorter chain alkane, due to its low hydrophobicity and the small flexible group, the membrane quality is poor under the ultra-thin film layer, and pinholes and other membrane problems are prone to occur. By increasing the chain length and replacing it with a longer flexible alkyl chain or a heteroalkane containing a hydrophilic group, the pinhole problem of the membrane layer can be effectively solved. When R2 is substituted with an aromatic group, since it is a rigid group, there are no pinholes and other membrane quality problems. See the attached drawings for the electron microscope schematic diagrams of some embodiments and comparative examples of the membrane layer. Figure 1 This is a schematic diagram of electron microscopy of comparative example 1 at a film thickness of 30 nm. Figure 2 This is a schematic diagram of electron microscopy of comparative example 3 at a film thickness of 30 nm. Figure 3 The electron microscope diagram of Example 1 at a film thickness of 30nm is shown in Figure 1. Comparative Examples 1 to 3 have more pinholes, while Examples 1 to 5 have almost no pinholes observed, and the pinhole problem of the film layer has been effectively solved. It can be seen from Examples 1 to 5 that the addition of a small amount of additives and the change of solvents have little effect on the film layer quality and lithography performance; it can be seen from Example 6, Comparative Example 1 and Comparative Example 10 that the addition of a leveling agent has little effect on improving the pinholes of the film layer.
[0106] ② Adhesion and film retention rate
[0107] In Examples 1 to 3 and 5, and Comparative Examples 1 to 5, when R2 is an alkyl chain, as the carbon chain increases, the adhesion shows a fluctuating change from good to bad, then to good, and finally to bad again. The reason may be caused by the hydrophobicity and flexibility of the substituent group. When the number of carbon atoms in the substituent increases from 1 to 4, the hydrophobicity is the dominant factor, so the adhesion becomes worse; when it increases from 4 to 6, the flexibility of the group is the dominant factor, and the adhesion becomes better. In Example 4, when its substituent R2 is 4-tert-butylphenyl, the adhesion is good.
[0108] In Comparative Examples 6 to 8, when R2 has a hydroxyl group at the end or an ether bond in the side chain, the film retention rate of the photoresist material decreases, while in other cases the film retention rate is good.
[0109] It can be seen from comparative example 3 and comparative example 9 that when the grafting rate of the DNQ group is equal to or exceeds 75%, the adhesion of the film layer deteriorates due to the overall strong hydrophobicity.
[0110] ③Hydrophilicity
[0111] As the length of the R2 alkyl chain increases, the contact angle test shows that the hydrophobicity of the ultra-thin film layer of the photoresist material increases. When R2 is an alkane chain with a terminal hydroxyl group or an alkane containing an ether bond or a thioether, the film quality is good and is more hydrophilic than the alkyl chain. Figure 4 The contact angle test results of some embodiments are shown in FIG.
[0112] Contact angle tests of some embodiments are shown in Table 2. The contact angle test results of embodiments 1 to 3 and comparative example 1 are shown in Table 2. The test results show that as the carbon chain gradually increases, the hydrophobicity of the photoresist film layer of the system gradually increases.
[0113] 2) Lithography quality: Apply this system photoresist to SP high-resolution lithography and interference lithography
[0114] Photolithography process: Spin coating, 1000-4000 rpm, 30 seconds for spin coating, film thickness less than 50nm; pre-baking, 100℃, 5 minutes; exposure using I-line 365nm SP lithography machine or I-line high-resolution interference lithography machine, dose of 10-200mJ / cm 2 ; Post-baking, 100℃, 2 minutes; Development, 2.83% TMAH aqueous solution, soaking for 60s, 25℃.
[0115] In Comparative Examples 1 to 2, although pinholes appeared in the film layer, the quality of the photolithography pattern was good; in Comparative Examples 3 to 5, the film layer had adhesion problems, resulting in curved lines in the high-resolution photolithography pattern, partial separation from the substrate, and poor imaging quality; in Comparative Examples 6 to 8, when the film retention rate was poor, the photolithography pattern could not be exposed.
[0116] In embodiments 1 to 5, when the film layer is relatively good, the photoresist used in the present disclosure can expose a good 128nm period high-resolution pattern under the ultra-thin film layer using SP lithography technology, and can expose a good 104nm period high-resolution interference lithography pattern, such as Figures 5 to 8 As shown, Figure 5 The SP lithography experiment result in Comparative Example 4, the pattern period is 128nm; Figure 6 The SP lithography experiment result in Example 3, the pattern period is 128nm; Figure 7 The SP lithography experiment results in Example 4, the pattern period is 128nm; Figure 8 This is the result of the high-resolution interference lithography experiment in Example 3, and the pattern period is 104nm.
[0117] The novel I-line high-resolution photoresist design strategy proposed in the present disclosure achieves nanometer-level resolution based on a calixarene small molecule containing a diazonaphthoquinone group as the main component or even the only component; at the same time, a calixarene branch chain regulation strategy is also proposed, so that the photoresist composition formulated based on the regulated single-component main component can achieve a pinhole-free ultra-thin film layer with adjustable adhesion and hydrophilicity.
[0118] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. An I-line single-component photoresist composition, used for I-line high-resolution lithography, It is characterized in that It is composed of an organic solvent and a single-component photosensitive material, or a mixture of one or more of a dissolution promoter, a leveling agent, a surfactant, and a stabilizer, and the organic solvent and the single-component photosensitive material; The single-component photosensitive material is a calixarene derivative molecule containing a diazonaphthoquinone group and has a structure shown in Formula I: Formula I; Among them, R 1 The 1,2-naphthoquinone-2-azide-4-sulfonyl-O-group and the hydroxyl group are at least partially the 1,2-naphthoquinone-2-azide-4-sulfonyl-O-group, and the grafting rate of the 1,2-naphthoquinone-2-azide-4-sulfonyl-O-group is 50%-65%; n is 4, 6 or 8; R 2 One of n-butyl, n-pentyl, n-hexyl and 4-tert-butylphenyl; The organic solvent is propylene glycol methyl ether acetate, ethyl lactate or propylene glycol monomethyl ether.
2. The I-line single-component photoresist composition according to claim 1, It is characterized in that The weight percentage of the organic solvent is 85% to 98%.
3. A method for preparing the I-line single-component photoresist composition according to claim 1, It is characterized in that include: Dissolve resorcinol in methanol, add concentrated hydrochloric acid, and dropwise add the substituent R 2 The corresponding reactants are reacted and purified to obtain a first product with a calixarene structure; The first product is dissolved, triethylamine is added dropwise, and then sulfonyl chloride containing a diazonaphthoquinone group is added, and the reaction is performed and purified to obtain a single-component photosensitive material with a structure of formula I; The single-component photosensitive material is dissolved in an organic solvent, and filtered to obtain an I-line single-component photoresist composition.
4. A method for patterning using an I-line single-component photoresist composition, It is characterized in that include: cleaning the substrate; optionally applying an adhesion promoting layer; Then coating the I-line single-component photoresist composition according to any one of claims 1 to 2, and performing exposure to form a pattern; or coating the substrate with a metal layer; optionally applying an adhesion promoting layer; Then, the I-line single-component photoresist composition according to any one of claims 1 to 2 is coated and exposed to form a pattern.
5. Use of the I-line single-component photoresist composition according to any one of claims 1 to 2 in I-line interference lithography, near-field lithography, and SP lithography.
Citation Information
Patent Citations
Method for realizing improvement of surface plasma photoetching quality by utilizing metallic reflecting film structure
CN101726998A
Positive photoresist composition
US4859563A
1,2-naphthoaguinone-2-diazidosulfonate photosenisitizer, method for preparing the photosensitizer and photoresist composition