A sodium sulfide composite cobalt catalyst and its preparation method and application
By preparing Na2S/Co9S8/Co composite catalyst in sodium-sulfur batteries, the dendritic crystallization and low Coulomb efficiency of sulfur positive electrode materials in sodium-sulfur batteries are solved, the conductivity and reaction kinetics of the battery are improved, and more efficient Electrochemical properties.
Patent Information
- Application Number
- CN202210974457.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-15
AI Technical Summary
As the positive electrode material, sulfur in existing sodium-sulfur batteries has problems such as dendritic formation, low Coulomb efficiency and damage to the electrode structure. The commercial Na2S particles are large in size and low electronic conductivity, resulting in unsatisfactory electrochemical performance.
By mixing sodium sulfate, cobalt sulfate and conductive carbon black with organic polymer polymer polymer and performing high-temperature reduction and annealing, Na2S/Co9S8/Co composite catalyst is prepared, so that the Na2S and Co9S8 particles are evenly distributed in the carbon material network, and electron conduction is improved rate and catalytic activity.
The activation voltage of Na2S is reduced for the first charging, the reaction kinetics and battery safety are improved, and the electrochemical performance and capacity efficiency of sodium-sulfur batteries are significantly improved.
Smart Images

Figure CN115425192B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to electrochemical sodium-sulfur batteries, and more specifically, relates to a sodium sulfide composite cobalt catalyst and a preparation method and application thereof. Background Art
[0002] In recent years, in order to successfully achieve the strategic goal of clean and sustainable energy, it is necessary to consider replacing the existing fossil fuel-dominated development model with the best new energy. Sulfur (S) is a promising cathode material with a theoretical specific capacity of up to 1675 mAh g -1 , lithium-sulfur batteries have been widely studied. Due to the scarcity of metallic lithium resources and geographical restrictions, the sodium-sulfur battery system has a huge price advantage. Therefore, sodium-sulfur batteries are a strong competitor for large-scale energy storage batteries and power batteries.
[0003] In sodium-sulfur batteries, when sulfur is used as the positive electrode, sodium (Na) needs to be paired as the negative electrode. The use of sodium metal will bring safety hazards, and there are serious problems of dendrite formation and low Coulomb efficiency during the charge and discharge process. In addition, S will expand by 160% in volume during the complete sodiumization process, which will cause structural damage to the electrode and aggravate the shuttle effect caused by the dissolution / diffusion of sodium polysulfide. The dissolution of polysulfides and subsequent side reactions with the electrolyte directly lead to the loss of active materials, resulting in rapid capacity decay. Sodium sulfide (Na2S) is the final discharge product and is a more ideal initial positive electrode material compared to elemental S. Na2S is in an expanded state and tends to shrink during the initial de-sodiumization process, which can provide gaps for volume expansion during the subsequent sodiumization process. On the other hand, Na2S is in a fully sodiumized state and can be paired with a sodium-free negative electrode, such as hard carbon or tin alloy materials, to achieve a full battery without metallic sodium.
[0004] At present, commercial Na2S particles are large in size, have low electronic conductivity, high activation voltage for the first charge, and poor electrochemical performance in sodium-sulfur batteries. Therefore, developing a nano-sized and highly active Na2S cathode material is of great significance to improving the performance of sodium-sulfur batteries. Summary of the invention
[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a sodium sulfide composite cobalt catalyst and a preparation method and application thereof. The preparation method comprises uniformly mixing sodium sulfate, cobalt sulfate, conductive carbon black and organic polymer macromolecules, and obtaining a sodium sulfide composite cobalt-containing catalyst Na2S / Co9S8 / Co by high-temperature reduction annealing. Na2S particles and Co9S8 particles are uniformly distributed in a network formed by a carbon material. The carbon substrate can effectively improve the electronic conductivity of the material and improve the conductivity of the positive electrode.
[0006] To achieve the above object, according to one aspect of the present invention, a method for preparing a sodium sulfide composite cobalt catalyst is provided, the preparation method comprising the following steps:
[0007] (1) dissolving an organic polymer in a solvent to obtain a precursor solution;
[0008] (2) adding sodium sulfate, cobalt sulfate and a conductive carbon material to a precursor solution to obtain a dispersion;
[0009] (3) mixing the dispersion evenly, evaporating the dispersion until the organic solvent in the dispersion is completely volatilized, and cooling and drying the dispersion to obtain a solid powder;
[0010] (4) ball milling the obtained solid powder to obtain sodium sulfate powder uniformly coated with carbon material and cobalt sulfate powder uniformly coated with carbon material;
[0011] (5) The obtained powder is subjected to thermal reduction to obtain a sodium sulfide composite cobalt catalyst.
[0012] Furthermore, the organic polymer is one or more of polyacrylonitrile, polyvinyl pyrrolidone and polydopamine.
[0013] Furthermore, the organic polymer is polyvinyl pyrrolidone.
[0014] Furthermore, the mass concentration of the organic polymer in the precursor solution is 0.01-0.02 g / mL.
[0015] Furthermore, the conductive carbon is one or more of Ketjen black, acetylene black, and Super P.
[0016] Furthermore, the mass ratio of sodium sulfate, cobalt sulfate and conductive carbon in the dispersion is (4-2):1:1.
[0017] Furthermore, the volatilization temperature is 50 to 80°C.
[0018] Furthermore, the reduction pyrolysis conditions are: 1-5 °C·min -1 The temperature is raised to 800-900°C at a heating rate and kept at this temperature for 2-4 hours.
[0019] The present invention also provides a sodium sulfide composite cobalt catalyst, which is prepared by adopting the preparation method of the sodium sulfide composite cobalt catalyst as described above.
[0020] The present invention provides an application of the sodium sulfide composite cobalt catalyst as described above in a sodium-sulfur battery electrode.
[0021] In general, compared with the prior art, the sodium sulfide composite cobalt catalyst provided by the present invention and its preparation method and application have the following beneficial effects:
[0022] 1. A composite material of sodium sulfide and cobalt catalyst was successfully obtained by high-temperature reduction of sodium sulfate and cobalt sulfate. When sodium sulfide was used to prepare the positive electrode of sodium ion battery, the highly active Na2S was fully activated for the first time with a voltage reduced to 1.95V. The polar Co9S8 had a good adsorption effect on sodium polysulfide, which alleviated the capacity decay caused by the shuttle effect during battery operation. Nano-Co, as a catalytic active center, improved the charging efficiency of Na2S and effectively improved the reaction kinetics. The above advantages successfully realized Na2S as the positive electrode of sodium-sulfur battery and made the battery operate safely.
[0023] 2. The composite material Na2S / Co9S8 / Co of sodium sulfide composite cobalt catalyst was prepared by in situ reduction of sodium sulfate and cobalt sulfate. Na2S particles and Co9S8 particles were evenly distributed in the network formed by carbon material. The carbon substrate can effectively improve the electronic conductivity of the material and improve the conductivity of the positive electrode.
[0024] 3. When it is used to prepare the positive electrode of sodium-sulfur battery, the high activity of nano-sized Na2S reduces the first charge activation voltage, and the nano-Co particles have a good catalytic effect and improve the reaction kinetics. On the other hand, the polar Co9S8 has a good adsorption effect on the intermediate product sodium polysulfide, effectively inhibiting the shuttle effect. The synergistic effect of the catalysis and adsorption of Co and Co9S8 in the composite material, Na2S / Co9S8 / Co has a higher reaction activity and first specific capacity, which reduces the first activation voltage of Na2S, accelerates the reaction kinetics, and significantly improves the electrochemical performance of the battery.
[0025] 4. The size of Na2S particles is 500nm~1μm. Compared with the size of commercial Na2S particles (>2μm), the size of in-situ obtained Na2S is significantly reduced, and the fine Na2S, Co9S8 and Co particles are evenly distributed in the carbon matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 a, b, c, and d are scanning electron microscope images of Na2S / Co9S8 / Co prepared in Example 1 of the present invention, respectively;
[0027] Figure 2 is the XRD pattern of the Na2S / Co9S8 / Co sample prepared in Example 1;
[0028] Figure 3The cyclic voltammogram of Na2S / Co9S8 / Co and Na2S prepared in Example 1 as the positive electrode of sodium-sulfur battery;
[0029] Figure 4 This is the first cycle charge and discharge curve of Na2S / Co9S8 / Co prepared in Example 1 as the positive electrode of a sodium-sulfur battery. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0031] The present invention provides a method for preparing a sodium sulfide composite cobalt catalyst, the preparation method comprising the following steps:
[0032] Step 1: dissolving an organic polymer macromolecule in a solvent to obtain a precursor solution containing the organic polymer macromolecule.
[0033] The organic polymer is one or more of polyacrylonitrile (PAN), polyvinyl pyrrolidone (PVP), and polydopamine (PDA). Preferably, the organic polymer is polyvinyl pyrrolidone (PVP). The solvent is one or more of anhydrous methanol, anhydrous ethanol, N,N-dimethylformamide (DMF), and N-methylpyrrolidone (NMP). Preferably, the solvent is anhydrous ethanol. The mass concentration of the organic polymer in the precursor solution is 0.01 to 0.02 g / mL.
[0034] Step 2: adding sodium sulfate, cobalt sulfate and conductive carbon material to the precursor solution to obtain a dispersion.
[0035] The conductive carbon is one or more of Ketjen black, acetylene black, and Super P. Preferably, the conductive carbon is Ketjen black. The mass ratio of sodium sulfate, cobalt sulfate, and conductive carbon in the dispersion is (4-2):1:1.
[0036] Step 3, stirring and ultrasonicating the dispersion to make the dispersion evenly mixed, then evaporating until the organic solvent is completely volatilized, cooling and drying to obtain a solid.
[0037] In this embodiment, the volatilization temperature is 50 to 80°C.
[0038] Step 4: ball-milling the obtained solid powder to obtain solid powder of sodium sulfate and cobalt sulfate uniformly coated with carbon material of small particle size.
[0039] Solid powder is subjected to planetary ball milling at a ball milling speed of 300-400 rpm, ball milling for 20-40 minutes, pausing for 20-40 minutes, and repeating this process 10-20 times. Preferably, the ball milling speed is 400 rpm, ball milling for 30 minutes, pausing for 30 minutes, and repeating this process 15 times.
[0040] Step 5: thermally reducing the fine solid powder to obtain the sodium sulfide composite cobalt catalyst.
[0041] The conditions for reduction pyrolysis are: 1~5℃·min -1 The temperature is raised to 800-900°C at a heating rate and kept at this temperature for 2-4 hours. Preferably, the reduction pyrolysis conditions are: 1-5°C·min -1 The temperature is raised to 800-900°C at a heating rate and kept at this temperature for 2-4 hours.
[0042] The present invention also provides a sodium sulfide composite cobalt catalyst, which is prepared by the preparation method of the sodium sulfide composite cobalt catalyst as described above. The present invention also provides an application of the sodium sulfide composite cobalt catalyst as described above in a sodium-sulfur battery electrode. The sodium sulfide composite cobalt catalyst Na2S / Co9S8 / Co and a conductive agent are dispersed in an organic solvent, stirred until uniformly dispersed, and a proper amount is added dropwise to a self-supporting electrode (carbon cloth), and the volatilized solvent is dried to obtain a composite positive electrode.
[0043] The amount of Na2S / Co9S8 / Co and the conductive agent used is consistent with the conventional amount in the art, and the types are also conventional substances. Preferably, the amount of the conductive agent used is 2-15% of the mass of the composite material Na2S / Co9S8 / Co.
[0044] The conductive agent is one or more of Ketjen black, acetylene black, Super P, carbon nanotubes, graphene or graphite powder. The organic solvent is N-methylpyrrolidone (NMP). The organic solvent is N-methylpyrrolidone (NMP).
[0045] The present invention is further described in detail below with reference to several specific embodiments.
[0046] Example 1
[0047] A Na2S / Co9S8 / Co composite material, the preparation process is as follows:
[0048] (1) Preparation of precursor solution: The solute in the precursor solution is 1 g of polyvinyl pyrrolidone and the solvent is 100 mL of anhydrous ethanol.
[0049] (2) adding 4 g of sodium sulfate, 1 g of cobalt sulfate, and 1 g of Ketjen black to the precursor solution and stirring for 1 h until the solution is evenly dispersed to obtain a dispersion;
[0050] (3) stirring and ultrasonicating the obtained dispersion for 1 h each to make it uniformly mixed, then placing it in an oven at 70 degrees to evaporate the anhydrous ethanol completely, and cooling and drying it to obtain a solid;
[0051] (4) ball milling the obtained solid powder at a ball milling speed of 400 rpm, ball milling for 30 minutes and pausing for 30 minutes, and repeating for 16 times to obtain a solid powder of sodium sulfate and cobalt sulfate uniformly coated with carbon materials of small particle size;
[0052] (5) The obtained fine powder was placed in a corundum crucible and heated in a tube furnace accompanied by H2 / Ar mixed gas at 5℃·min -1 The temperature was heated to 100℃ and stabilized for 2h; then the temperature was increased to 2℃·min -1 The temperature was raised to 800°C for reduction for 2 h, and then naturally cooled to room temperature to obtain a sodium sulfide composite cobalt catalyst.
[0053] Example 2
[0054] A Na2S / Co9S8 / Co composite material, the preparation process is as follows:
[0055] (1) Preparation of precursor solution: The solute in the precursor solution is 1 g of polyvinyl pyrrolidone and the solvent is 100 mL of anhydrous ethanol.
[0056] (2) Add 4 g of sodium sulfate, 1 g of cobalt sulfate, and 1 g of Super P to the precursor solution and continue stirring for 1 h until the solution is evenly dispersed to obtain a dispersion;
[0057] (3) stirring the obtained dispersion by ultrasonic stirring for 1 h each time to make it uniformly mixed, placing it in an oven at 70 degrees to evaporate the anhydrous ethanol completely, and cooling and drying it to obtain a solid;
[0058] (4) ball milling the obtained solid powder at a ball milling speed of 400 rpm, ball milling for 30 minutes and pausing for 30 minutes, and repeating for 16 times to obtain a solid powder of sodium sulfate and cobalt sulfate uniformly coated with carbon materials of small particle size;
[0059] (5) The obtained fine powder was placed in a corundum crucible and heated in a tube furnace accompanied by H2 / Ar mixed gas at 5℃·min -1 The temperature was heated to 100℃ and stabilized for 2h; then the temperature was increased to 2℃·min -1 The temperature was raised to 800°C for reduction for 2 hours and then naturally cooled to room temperature to obtain a composite material of sodium sulfide and cobalt catalyst.
[0060] Example 3
[0061] A Na2S / Co9S8 / Co composite material, the preparation process is as follows:
[0062] 1) Prepare the precursor solution: the solute in the precursor solution is 1 g of polyvinyl pyrrolidone and the solvent is 100 mL of anhydrous ethanol.
[0063] (2) Add 4 g of sodium sulfate, 1 g of cobalt sulfate, and 1 g of acetylene black to the solution and continue stirring for 1 h until the solution is evenly dispersed to obtain a dispersion;
[0064] (3) stirring the obtained dispersion by ultrasonic stirring for 1 h each time to make it uniformly mixed, placing it in an oven at 70 degrees to evaporate the anhydrous ethanol completely, and cooling and drying it to obtain a solid;
[0065] (4) ball milling the obtained solid powder at a ball milling speed of 400 rpm, ball milling for 30 minutes and pausing for 30 minutes, and repeating for 16 times to obtain a solid powder of sodium sulfate and cobalt sulfate uniformly coated with carbon materials of small particle size;
[0066] (5) The obtained fine powder was placed in a corundum crucible and heated in a tube furnace accompanied by H2 / Ar mixed gas at 5℃·min -1 The temperature was heated to 100℃ and stabilized for 2h; then the temperature was increased to 2℃·min -1 The temperature was raised to 800°C for reduction for 2 hours and then naturally cooled to room temperature to obtain a composite material of sodium sulfide and cobalt catalyst.
[0067] Comparative Example 1
[0068] The sodium sulfide material (Na2S) provided in this comparative example has a preparation process that is different from that of Na2S / Co9S8 / Co in that no cobalt source (cobalt sulfate) is added, and the other steps are consistent with those of Application Example 1.
[0069] Application Examples
[0070] A composite material of sodium sulfide composite cobalt-containing catalyst (denoted as Na2S / Co9S8 / Co) was prepared using Example 1 and used as a test object, wherein the sample prepared in Comparative Example 1 (Na2S) was used as a control example, and all samples were loaded on carbon cloth and used to assemble batteries, as positive electrodes, and applied to sodium-sulfur batteries for performance testing. The carbon cloth was a cut 10 mm disc, the ratio of active material to Ketjen black was 8:1, dispersed in N-methylpyrrolidone (NMP), and 60 μL was dropped on the carbon cloth. The test battery model was a 2032 coin battery, and the tested electrolyte was NaTFSI dissolved in DOL and DME, with 2% NaNO3 added.
[0071] Test results see Figure 1 to Figure 4 shown.
[0072] Figure 1 This is a scanning electron microscope photo of the composite material of sodium sulfide and cobalt-containing catalyst prepared in Example 1. Figure 1 It can be seen that Na2S particles and Co9S8 particles are evenly distributed in the network formed by the carbon material, and the size of Na2S particles is about 500nm~1μm. Figure 1 It can be seen from the X-ray energy spectrum that the elements sodium, sulfur, cobalt and carbon are evenly distributed in the material.
[0073] Figure 2 This is the XRD pattern of the Na2S / Co9S8 / Co sample prepared in Example 1. Figure 2 It can be seen that at a reduction temperature of 900°C, it is basically consistent with the Na2S, Co9S8 and Co standard cards, and the substances generated are mainly Na2S, Co9S8 and Co.
[0074] Figure 3 Figure 1 shows the cyclic voltammogram of the positive electrode of the sodium-sulfur battery using Na2S / Co9S8 / Co and Na2S. Figure 3 As shown, the first activation voltage of the Na2S / Co9S8 / Co positive electrode is 1.95 V, and Na2S is activated and charged to generate elemental S, whose oxidation peak is at 2.2 V. The first activation voltage of Comparative Example 1 (Na2S) is 2.2 V, because the cobalt-containing catalyst in Example 1 improves the reaction kinetics and accelerates the conversion of Na2S.
[0075] Figure 4 The charge and discharge curve of the Na2S / Co9S8 / Co cathode material prepared in Example 1 is shown in FIG. Figure 4 It can be seen that at a current density of 0.2C, its initial charge and discharge specific capacity is 507mAh g -1 and 248mAh g -1 The first coulombic efficiency is 48.9%. The specific capacity of the Na2S / Co9S8 / Co cathode is calculated based on Na2S, and its theoretical specific capacity is 687 mAh g -1 .
[0076] In summary, the Na2S / Co9S8 / Co provided by the present invention and Na2S alone (Comparative Example 1) have high reactivity.
[0077] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a sodium sulfide composite cobalt catalyst, characterized in that: The preparation method comprises the following steps: (1) dissolving an organic polymer in a solvent to obtain a precursor solution; (2) adding sodium sulfate, cobalt sulfate and a conductive carbon material to a precursor solution to obtain a dispersion; (3) mixing the dispersion evenly, evaporating the dispersion until the organic solvent in the dispersion is completely volatilized, and cooling and drying the dispersion to obtain a solid powder; (4) ball milling the obtained solid powder to obtain sodium sulfate powder uniformly coated with carbon material and cobalt sulfate powder uniformly coated with carbon material; (5) The obtained powder is subjected to pyrolysis reduction to obtain a sodium sulfide composite cobalt catalyst, wherein the sodium sulfide composite cobalt catalyst is Na2S / Co9S8 / Co.
2. The method for preparing a sodium sulfide composite cobalt catalyst as claimed in claim 1, wherein: The organic polymer macromolecule is one or more of polyacrylonitrile, polyvinyl pyrrolidone and polydopamine.
3. The method for preparing a sodium sulfide composite cobalt catalyst as claimed in claim 2, wherein: The organic polymer macromolecule is polyvinyl pyrrolidone.
4. The method for preparing a sodium sulfide composite cobalt catalyst as claimed in claim 1, wherein: The mass concentration of the organic polymer in the precursor solution is 0.01-0.02 g / mL.
5. The method for preparing a sodium sulfide composite cobalt catalyst as claimed in claim 1, wherein: The conductive carbon is one or more of Ketjen black, acetylene black, and Super P.
6. The method for preparing a sodium sulfide composite cobalt catalyst as claimed in claim 5, wherein: The mass ratio of sodium sulfate, cobalt sulfate and conductive carbon in the dispersion is (4-2):1:
1.
7. The method for preparing a sodium sulfide composite cobalt catalyst according to claim 1, wherein: The volatilization temperature is 50-80°C.
8. The method for preparing the sodium sulfide composite cobalt catalyst according to any one of claims 1 to 7, characterized in that: The conditions for reduction pyrolysis are: 1~5℃·min -1 The temperature is raised to 800-900°C at a heating rate and kept at this temperature for 2-4 hours.
9. A sodium sulfide composite cobalt catalyst, characterized in that: The catalyst is prepared by the preparation method of the sodium sulfide composite cobalt catalyst according to any one of claims 1 to 8.
10. Use of the sodium sulfide composite cobalt catalyst according to claim 9 in sodium-sulfur battery electrodes.