A high-speed and low-loss resin composition and its application
Through the combination of low molecular weight polysenol-based resin, benzocyclobutene compound and spherical silica, the problem of insufficient dielectric properties and heat resistance of polysenol-based substrate materials in high-frequency applications is solved, and high performance is achieved High speed and low loss characteristics of printed circuit boards.
Patent Information
- Application Number
- CN202211138765.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-19
AI Technical Summary
The existing polyshenol substrate materials have problems such as excellent dielectric properties but insufficient heat resistance and formability in high frequency applications. High molecular weight leads to high viscosity and low fluidity, making it difficult to prepare high reliability printed wiring boards.
The cross-linking reaction is carried out with the benzocyclobutene compound and its derivatives by using low molecular weight polysenol resin to carry out cross-linking reaction with benzocyclobutene compound and its derivatives, and combined with spherical silica fillers, the heat resistance and forming of cured products are improved by optimizing the selection of cross-linking agents and fillers. and reduce dielectric constant and dielectric loss.
It realizes the high frequency and high speed requirements of high-performance printed circuit boards, with excellent heat and humidity resistance, low dielectric constant, low dielectric loss, low expansion coefficient and excellent processability.
Smart Images

Figure CN115433451B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of resin technology, and more particularly to a high-speed and low-loss resin composition and application thereof. Background Art
[0002] For various electronic devices, as the amount of information processing increases, the installation technology of high integration of semiconductor devices, high density of wiring, and multilayering is developing rapidly. In addition, as wiring boards used in various electronic devices, wiring boards that can cope with high frequencies, such as millimeter wave radar substrates in vehicle-mounted applications, are also sought. In order to increase the transmission speed of signals and reduce the loss during signal transmission, the substrate material used to form the substrate of the wiring board used in various electronic devices is required to have a low dielectric constant and dielectric loss factor.
[0003] It is known that polyphenylene ether has excellent dielectric properties such as dielectric constant and dielectric loss factor, and also has excellent dielectric properties in the high frequency band (high frequency region) from the MHz band to the GHz band. Therefore, research is being conducted on the use of polyphenylene ether, for example, as a high-frequency molding material. More specifically, research is being conducted on the use of polyphenylene ether as a substrate material for constituting a substrate of a printed wiring board, wherein the printed wiring board is provided in an electronic device utilizing a high frequency band.
[0004] However, when used as a molding material such as a substrate material, it is required not only to have excellent dielectric properties but also to have excellent heat resistance and moldability, etc. In this regard, since polyphenylene ether is a thermoplastic type, sufficient heat resistance may not be obtained.
[0005] As the substrate material, for example, prepreg and laminated board using the resin composition containing the modified polyphenylene ether are listed. Patent document 1 (publication number CN100547033) records the prepreg and laminated board using the polyphenylene ether resin composition, and the polyphenylene ether composition includes: polyphenylene ether and curing type crosslinking agent having polyphenylene ether part in molecular structure, vinyl benzyl etc. at its molecular end and number average molecular weight of 1000-7000. The conventional TAIC of general curing type crosslinking agent can obtain the laminated board with high heat resistance and formability etc. which will not reduce dielectric properties, but there are defects such as high water absorption and large loss after moisture absorption. With the development of the times, in the pursuit of high heat resistance, in order to further improve the transmission speed of signal, it is also required to further reduce the loss during signal transmission, so the substrate not only requires excellent heat resistance, but also needs the material with more excellent dielectric properties.
[0006] In general, polyphenylene ether has a relatively high molecular weight and a high softening point, and therefore has a tendency to have high viscosity and low fluidity. If such polyphenylene is used to form a prepreg for use in preparing a multilayer printed wiring board, and the formed prepreg is used to prepare a printed wiring board, there may be a problem of formability, that is, during preparation, for example, forming defects such as voids may occur during multilayer forming, making it difficult to prepare a highly reliable printed wiring board.
[0007] Therefore, in order to suppress the occurrence of such problems, the present inventors have studied the use of polyphenylene ethers with relatively low molecular weights. However, according to the research of the present inventors, when such polyphenylene ethers with simply reduced molecular weights are used, even when used in combination with thermosetting resins, the resin composition is not sufficiently cured, and the heat resistance of the cured product tends to be insufficiently improved.
[0008] Furthermore, Patent Document 1 discloses that a modified polyphenylene ether compound can be obtained, which can maintain excellent dielectric properties and improve solder heat resistance and formability. Furthermore, Patent Document 2 (Publication No. JP2004339328A) discloses that a polyphenylene ether resin composition can be obtained, which can produce a laminate with high heat resistance and formability even if a polyphenylene ether with a small molecular weight is used in order to not reduce dielectric properties and obtain convenience during prepreg preparation.
[0009] Furthermore, it is required to further improve the heat resistance and moldability of the cured product compared with the case of using the modified polyphenylene ether compounds disclosed in Patent Documents 1 and 2. In other words, it is required to further improve the heat resistance and moldability of the cured product while having the dielectric properties possessed by polyphenylene ether.
[0010] Therefore, in order to further improve the moldability and heat resistance of the cured product, there is a demand for a modified polyphenylene ether compound which is not only excellent in reactivity contributing to the curing reaction but also excellent in storage stability and has low viscosity and excellent fluidity. Summary of the invention
[0011] In view of this, the object of the present invention is to provide a high-speed, low-loss resin composition and its application, the cured product of the resin composition has excellent heat and moisture resistance, a higher glass brick change temperature, a lower dielectric constant, a lower dielectric loss, a lower expansion coefficient, and excellent heat resistance, and at the same time has good processability, which can fully meet the high-frequency and high-speed requirements of high-performance printed circuit boards.
[0012] In order to achieve the above object, the present invention adopts the following technical solution:
[0013] A high-speed, low-loss resin composition comprising a resin compound, at least one of a benzocyclobutene compound and a derivative thereof, an accelerator, and a filler mixture;
[0014] The resin compound contains at least one structural formula as shown in formula (1):
[0015] In formula (1), R1-R4 are independently selected from hydrogen atom, alkyl group, alkenyl group, alkynyl group or halogenated hydrocarbon, and R1-R4 may be the same, partially the same or different from each other.
[0016] The alkyl group of R1 to R4 is not particularly limited, but preferably contains at least one arylene group or benzylidene group, and is preferably an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms.
[0017] The arylene group or benzylidene group is not particularly limited and includes monocyclic aromatic groups and non-monocyclic polycyclic aromatic groups, and also includes derivatives in which the hydrogen atoms bonded to the aromatic ring are substituted by other hydrocarbon groups, acyl groups, and the like.
[0018] The resin composition can be cross-linked with a benzocyclobutene compound and its derivatives by a accelerator to obtain a cured product with high heat resistance. It is believed that the cross-linking reaction with the benzocyclobutene compound and its derivatives makes it difficult to generate high polarity bonds such as ether bonds and CN, and a cured product with low dielectric constant and low dielectric loss can be obtained.
[0019] The resin compound is not particularly limited as long as it contains at least one compound having the molecular structure of the above formula (1) in its molecular structure.
[0020] The resin compound may be a modified polyphenylene ether compound having at least one molecular structure of the above formula (1) in its molecular structure, or a polymer having a unit of the following structural formula (3) in its molecule:
[0021] In formula (3), R1-R4, R6-R8 are independently selected from hydrogen atoms, alkyl groups, alkenyl groups, alkynyl groups or halogenated hydrocarbons, i.e., R1-R4, R6-R8 can be the same group or different groups. In particular, R6-R8 are preferably hydrogen atoms or hydrocarbon groups having 1 to 7 carbon atoms.
[0022] The aforementioned resin compound may have a group represented by formula (1), and the atoms bound by the group are not particularly limited, including but not limited to modified polyphenylene ether, styrene and its derivatives, divinylbenzene and its oligomers, acenaphthylene, butadiene / styrene / divinylbenzene and other low molecular weight or high molecular weight homopolymers or copolymers and their modified bodies, maleic anhydride imide compounds, etc. In addition, as the aforementioned resin compound, the above compounds can be used alone or in combination of two or more.
[0023] The modified polyphenylene ether compound is not particularly limited as long as it has a group structure represented by the above formula (1) at a molecular terminal.
[0024] The aforementioned modified polyphenylene ether compound has a polyphenylene ether chain in the molecule, and preferably has the following structural formula (4): The SA9000 model from Sabic is particularly preferred.
[0025] In formula (4), m represents a range of 1-80, R9-R 12 are mutually independent hydrogen atoms or any other arbitrary groups. Preferably, R9-R 12 are independently hydrogen atoms or alkane groups.
[0026] The modified polyphenylene ether compound may be a graft-modified or block-modified compound of the structural unit of the formula (4) or a terminal-modified compound.
[0027] Furthermore, as the modified polyphenylene ether compound, the above compounds may be used alone or in combination of two or more.
[0028] Furthermore, the above-mentioned benzocyclobutene compound and its derivatives contain at least one structural formula as shown in formula (2):
[0029] In formula (2), R5 can be substituted arbitrarily. Preferably, R5 is a hydrocarbon group or an organic silicon resin.
[0030] The aforementioned benzocyclobutene compound and its derivatives have a group represented by formula (2), and the atoms to which the group is bonded are not particularly limited. In addition, as the aforementioned benzocyclobutene compound and its derivatives, the above compounds can be used alone or in combination of two or more.
[0031] Preferred specific examples of the aforementioned benzocyclobutene compounds and their derivatives include compounds represented by the following formula (5):
[0032]
[0033] Further, the above-mentioned promoter is at least one of a peroxide compound and its derivative, an azo compound and its derivative, or a metal organic catalyst. Preferably, the promoter is an azo compound and its derivative. Particularly preferably, it is an azo compound that does not contain other heteroatoms except the azo group. In addition, as the above-mentioned promoter, the above-mentioned compounds can be used alone or in combination of two or more.
[0034] Furthermore, the filler mixture is spherical silica. Furthermore, the spherical silica is prepared by chemical synthesis and has a specific surface area SSA ≤ 2.5 m 2 / g, average particle size 0.5μm≤D50≤5μm, maximum particle size D100≤50μm. As mentioned above, the resin composition of the present invention may contain other filling materials such as inorganic fillers. As filling materials, fillers added to improve the flame retardancy and heat resistance of the cured product of the resin composition can be listed, without special specification. Including but not limited to angular or non-chemical spherical silica, metal oxides such as alumina, metal hydroxides such as aluminum hydroxide, aluminum borate, calcium carbonate, etc. In addition, as the aforementioned filling materials, they can be used alone or in combination of two or more. In addition, when used as a filler, it can be used directly or after surface treatment with a silane coupling agent.
[0035] Furthermore, based on 100 parts by weight of the resin compound and the benzocyclobutene compound and its derivatives, the resin compound is 50-95 parts, the benzocyclobutene compound and its derivatives are 5-50 parts, the accelerator is 0.01-2 parts, and the filler mixture is 30-270 parts.
[0036] Furthermore, based on 100 parts by weight of the resin compound and the benzocyclobutene compound and its derivatives, the resin compound is 60-95 parts, the benzocyclobutene compound and its derivatives are 5-40 parts, the accelerator is 0.1-1 parts, and the filler mixture is 50-250 parts.
[0037] Furthermore, based on 100 parts by mass of the filler mixture, the spherical silicon dioxide accounts for 10-100 parts.
[0038] Furthermore, based on 100 parts by mass of the filler mixture, the spherical silicon dioxide accounts for 30-100 parts.
[0039] If the contents of the resin compound, benzocyclobutene compound and its derivatives, accelerator and filler mixture are within the above ranges, a cured product with good dielectric properties, heat resistance and anti-peeling properties can be obtained. It should be noted that if the contents of the resin compound, benzocyclobutene compound and its derivatives, accelerator and filler mixture are too small, for example, there is a risk of reduced heat resistance.
[0040] The resin composition of the present invention may further contain other ingredients besides the aforementioned resin compound, benzocyclobutene compound and its derivative, accelerator and filler mixture within the scope of not impairing the effect of the present invention. Other ingredients added to the resin composition of the present invention may include, but are not limited to, additives such as silane coupling agent, flame retardant, defoamer, antioxidant, heat stabilizer, antistatic agent, ultraviolet absorber, dye or pigment, lubricant and filler. In addition, the aforementioned resin composition may contain, in addition to the resin compound, thermosetting resins such as epoxy resin, unsaturated polyester resin, thermosetting polyimide resin, unsaturated hydrocarbon resin, etc.
[0041] As mentioned above, the resin composition of the present invention may contain a silane coupling agent. The aforementioned silane coupling agent may be contained in the resin composition, preferably, in a manner of pre-treating the surface of the filler, more preferably, in a manner of pre-treating the surface of the filler and in the resin composition at the same time. In addition, in the prepreg, it may be contained in the manner of a coupling agent for pre-treating the surface of the fibrous substrate.
[0042] The aforementioned silane coupling agent is a compound having one of vinyl, styryl, methacryloyl, acryloyl and phenylamino groups as a reactive group and having a hydrolyzable group such as methoxy or ethoxy, etc., without particular limitation. In addition, the aforementioned silane coupling agent may be used alone or in combination of two or more.
[0043] As mentioned above, the resin composition of the present invention may include a flame retardant. By containing a flame retardant, the flame retardancy of the cured product of the resin composition can be improved. The aforementioned flame retardant is not particularly limited. Including but not limited to halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants, etc., for example, bromine halogen flame retardants such as decabromodiphenyl ether, hexabromobenzene, decabromodiphenylethane, ethylene bis tetrabromophthalimide, for example, tris (2,6-dimethylphenyl) -phosphine, phenoxyphosphazene, xylene bis (diphenyl phosphine oxide), hypophosphite and other phosphorus flame retardants. In addition, as the aforementioned flame retardant, it can be used alone or in combination of two or more.
[0044] There is no particular limitation on the method for preparing the resin composition. Examples include a method of mixing the resin compound, the benzocyclobutene compound and its derivative, the accelerator, and the filler mixture at a specified content, which is not particularly limited. In general, after obtaining the resin composition, the following method can be used.
[0045] The present invention also seeks to protect the use of the high-speed, low-loss resin composition in the preparation of prepregs, resin-coated films, resin-coated metal foils, metal foil-clad laminates and wiring boards, wherein the high-speed, low-loss resin composition is a semi-cured product or a cured product.
[0046] The prepreg of the present invention should include: the aforementioned resin composition or the aforementioned semi-cured product of the resin composition and a fiber-based material.
[0047] The semi-cured product is a product obtained by curing a portion of the resin composition and then curing it further. In addition, the resin composition or the semi-cured product of the resin composition may be obtained by drying or heating the resin composition.
[0048] When preparing the aforementioned prepreg, most of the time the aforementioned resin composition is formulated into a resin varnish for use, and is attached to the fiber-based material by means of impregnation or coating.
[0049] When preparing the varnish of the resin composition, the resin composition is usually dissolved in a suitable solvent, and heating and other operations may be performed as needed, and the insoluble components are dispersed to a specified dispersion state with the assistance of a ball mill, a bead mill, a homogenizer, an emulsifier and other equipment. In particular, the solvent is not particularly required as long as it can dissolve the resin compound, the benzocyclobutene compound and its derivatives, the accelerator and the filler mixture and does not react with any of them or hinder the curing reaction of the resin composition.
[0050] The fiber-based material includes glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, pulp paper, cotton woven fabric, etc. Preferably, the glass cloth can provide the laminate with better mechanical properties, and the fiber-opening treated glass cloth is more preferred.
[0051] The method for preparing the aforementioned prepreg is not particularly required as long as it is capable of preparing the aforementioned prepreg.
[0052] The metal foil-clad laminate of the present invention should include: an insulating layer of the aforementioned resin composition cured product or the aforementioned prepreg cured product and a metal foil coated on one or both sides of the insulating layer surface. In addition, the aforementioned metal foil is subject to actual needs, and its type and thickness are not particularly limited. The thickness of the metal foil can be preferably 0.2-105 μm, and the type of metal foil can include but is not limited to copper foil, aluminum foil, etc.
[0053] The method for producing the metal-clad laminate is not particularly limited as long as it can produce the metal-clad laminate.
[0054] The resin composition of the present invention can prepare a cured product of the resin composition with low dielectric properties and high heat resistance. Therefore, the metal-clad laminate having the resin composition of the present invention cured as an insulating layer is also a metal-clad laminate having low dielectric properties and high heat resistance. In particular, the above-mentioned metal-clad laminate having the resin composition of the present invention cured as an insulating layer is also a metal-clad laminate for preparing a wiring board with low dielectric properties and high heat resistance.
[0055] The wiring board of the present invention should include: an insulating layer of the aforementioned cured resin composition or the aforementioned cured prepreg and wiring formed by metal foil covering one or both sides of the insulating layer at etched locations.
[0056] The method for producing the wiring board is not particularly limited as long as it can produce the aforementioned wiring board.
[0057] The wiring board according to the present invention is a wiring board having low dielectric properties and high heat resistance.
[0058] The metal foil with resin of the present invention should include: an insulating layer of the aforementioned resin composition or the aforementioned resin composition cured product and a metal foil. In addition, the aforementioned insulating layer may or may not include a fiber substrate as long as it includes the aforementioned resin composition or the aforementioned resin composition cured product. In addition, the aforementioned resin composition or the aforementioned resin composition semi-cured product may be obtained by drying or heating the aforementioned resin composition.
[0059] The metal foil with resin may be covered with a release film as needed to prevent contamination and damage. In addition, the release film is not particularly limited as long as it does not react with the insulating layer and can be separated from the insulating layer without residue.
[0060] The method for producing the metal foil with resin is not particularly limited as long as the method can produce the metal foil with resin.
[0061] The film with resin of the present invention should include: a resin layer of the aforementioned resin composition or the aforementioned resin composition cured product and a support film. In addition, the aforementioned resin layer, as long as it includes the aforementioned resin composition or the aforementioned resin composition cured product, may or may not include a fiber substrate. In addition, the aforementioned resin composition or the aforementioned resin composition semi-cured product may be obtained by drying or heating the aforementioned resin composition. In addition, the aforementioned support film is not particularly limited as long as it does not react with the aforementioned insulating layer and can be separated from the aforementioned insulating layer without residue.
[0062] The resin-bearing film may be covered with a release film as needed to prevent contamination and damage. In addition, the release film is not particularly limited as long as it does not react with the insulating layer and can be separated from the insulating layer without residue.
[0063] The method for producing the film with resin is not particularly limited as long as the aforementioned film with resin can be produced.
[0064] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0065] The inventors have conducted a large number of experimental studies to provide a novel resin composition having better heat resistance, dielectric properties and stripping resistance than the prior art. By comparing patent documents and experimental result data, it is found that the selection of cross-linking agent will have a greater impact on the dielectric properties of the resin composition. When a cross-linking agent containing groups such as cyano, ester and amino is used, the dielectric constant and dielectric loss performance of the final resin composition are poor. The reason is speculated to be: after the cross-linking agent containing groups such as cyano, ester and amino is used, the final cured product of the resin composition contains a large number of high polar groups. At the same time, high polar groups such as ether groups will be generated in the final cured product of the resin composition, which will make the dielectric properties of the final cured product of the resin composition worse.
[0066] Silicon powder is often used as the main filling material in the copper clad laminate industry due to its low thermal expansion coefficient and good chemical stability. However, the commonly used silicon powder has high hardness, large drilling wear, large specific surface area, difficult to disperse, poor dielectric properties, and certain defects; while the silicon dioxide particle size produced by chemical synthesis is generally at the nanometer level, difficult to disperse, and has poor dielectric properties.
[0067] Based on this, the present inventors use benzocyclobutene compounds and their derivatives as crosslinking agents, the cured product has no polar groups, and adopts at least one specific surface area of 2.5m 2 / g of chemical spherical silica is used as a filling material to solve the problems existing in the above-mentioned fillers. DETAILED DESCRIPTION
[0068] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0069] In the following examples, the ranking number and manufacturer of each material are shown in Table 1.
[0070] Table 1 Material statistics
[0071]
[0072]
[0073] Preparation method and performance test
[0074] 1. Preparation method
[0075] The resin compound, benzocyclobutene compound and its derivatives, accelerator and filler mixture are dissolved in a mixed solvent of toluene and ketones, stirred thoroughly and adjusted to a suitable viscosity. The resin glue is impregnated with 1078 glass fiber cloth to make the unit weight appropriate, and dried in an oven to remove toluene and ketone solvents to obtain 1078 prepreg, ensuring that the glue content is about 65%. Six sheets of 1078 prepreg are overlapped, and the upper and lower surfaces are equipped with copper foil of HoZ thickness. The vacuum lamination is cured in a press for 120 minutes, the curing pressure is 3MPa, and the curing temperature is 210°C to obtain a high-speed copper clad laminate. The properties of the board are shown in Table 2.
[0076] 2. Glass transition temperature (DMA) (Tg)
[0077] The Tg of the prepreg was measured using a dynamic thermomechanical analyzer "DMA850" manufactured by TA. At this time, the dynamic viscoelasticity measurement (DMA) was performed with the frequency set to 1 Hz in the flexural modulus, and the temperature at which tanδ showed a maximum when the temperature was raised from room temperature to 300°C at a heating rate of 5°C / min was set as Tg. The measured data are shown in Table 2.
[0078] 3. Glass transition temperature (TMA) (Tg)
[0079] When making the above-mentioned evaluation substrate, the number of overlapping prepregs is set to 6, thereby obtaining a copper-clad laminate (metal foil laminate) with a thickness of about 0.8 mm and a copper foil with a thickness of 18 um bonded on both sides. The copper foil on both sides of the formed copper-clad laminate was removed by etching. For the evaluation laminate thus obtained, the glass transition temperature (Tg) based on the TMA method was evaluated according to IPCTM650. A thermomechanical analysis (TMA) device (TMAQ400 manufactured by TA) was used in the measurement, and the measurement was carried out in the range of 40-260°C. The measured data are shown in Table 2.
[0080] 4. Heat resistance (TMA method: T-300)
[0081] When making the aforementioned evaluation substrate, the number of overlapping prepreg sheets was set to 6, thereby obtaining a copper-clad laminate (metal-clad laminate) with a thickness of about 0.8 mm and a copper foil with a thickness of 18 μm bonded on both sides. According to IPC-TM-650, the delamination time at 300°C was measured to evaluate the heat resistance of the aforementioned evaluation substrate. The measured data are shown in Table 2.
[0082] 5. Copper foil peel strength HVLP3) (N / mm)
[0083] When making the aforementioned evaluation substrate, the number of overlapping prepreg sheets was set to 6, thereby obtaining a copper-clad laminate (metal-clad laminate) with a thickness of about 0.8 mm and a copper foil with a thickness of 18 μm bonded on both sides. The copper foil on both sides of the formed copper-clad laminate was treated with a 3 mm characteristic tape, and the remaining copper foil was removed by etching, and the sample was tested using a peel strength tester. The measured data are shown in Table 2.
[0084] 6. Water absorption
[0085] The water absorption rate after 180 minutes of moisture absorption was measured using a high pressure accelerated aging tester at 2 MPa and 120°C. The measured data are shown in Table 2.
[0086] 7. Dielectric loss factor
[0087] The dielectric loss factor of the evaluation substrate at 10 GHz and 15 GHz was measured using the cavity perturbation method. Specifically, the dielectric loss factor of the evaluation substrate at 10 GHz and 15 GHz was measured using a network analyzer (E5071C manufactured by Keysight Technologies). The measured data are shown in Table 2.
[0088] Table 2 Performance test table
[0089]
[0090]
[0091] Table 2 (Continued) Performance Test Table
[0092]
[0093]
[0094] As can be seen from Table 2, by using the resin compound, benzocyclobutene compound and its derivatives, promoter and filler mixture as in the examples, and using a suitable ratio, the obtained high-speed circuit substrate can obtain lower dielectric loss and high heat resistance, and at the same time enable the board to obtain lower water absorption.
[0095] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high-speed, low-loss resin composition, It is characterized in that A mixture comprising a resin compound, at least one of a benzocyclobutene compound and a derivative thereof, an accelerator and a filler; The resin compound is SA9000 produced by Sabic; The benzocyclobutene compound and its derivatives include the compound represented by the following formula (5): ; The accelerator is an azo compound and its derivatives; Based on 100 parts by weight of the resin compound and the benzocyclobutene compound and its derivatives, the resin compound is 60-95 parts, the benzocyclobutene compound and its derivatives are 5-40 parts, the accelerator is 0.1-1 parts, and the filler mixture is 50-250 parts; The filler mixture contains 30-100 parts of spherical silicon dioxide based on 100 parts by mass; the spherical silicon dioxide is prepared by chemical synthesis and has a specific surface area SSA ≤ 2.5 m 2 / g, average particle size 0.5μm≤D50≤5μm, maximum particle size D100≤50μm.
2. A use of the high-speed, low-loss resin composition as claimed in claim 1 in the preparation of prepregs, films with resins, metal foils with resins, metal foil-clad laminates and wiring boards, It is characterized in that The high-speed and low-loss resin composition is a semi-cured product or a cured product.