Biodegradable nonwoven fabric

By optimizing the biodegradable non-woven fabric of polylactic acid-based polymer fiber, combined with thermomechanical analysis and thermocompression bonding technology, the problem of cracking and stability of the molded body during the thermoforming process is solved, and efficient and stable molding and beverage extraction are achieved. performance.

CN115434076BActive Publication Date: 2024-10-25MITSUI CHEM ASAHI LIFE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211101406.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-10-14
Filing Date
2017-10-12
Publication Date
2024-10-25
Estimated Expiration
2037-10-12

AI Technical Summary

Technical Problem

It is difficult to obtain a molded body with no cracks, uneven stretching and beautiful shape during the thermoforming process of existing biodegradable non-woven fabrics, and the thermal stability is insufficient, causing the molded body to easily break bags and leak contents during use.

Method used

Biodegradable non-woven fabrics composed of polylactic acid polymer fibers are used, and their dimensional change rate and thermal adhesion at 80°C to 140°C are optimized through thermomechanical analysis to ensure that thermoforming can be completed in a shorter time and Apply a load to the molded body at 30 to 100°C to suppress bag breakage, and combine it with appropriate fiber structure and thermal compression bonding technology to improve the thermal stability and appearance quality of the molded body.

Benefits of technology

It achieves the formation of crack-free, uniformly stretched and beautiful-shaped molded bodies in a shorter time, improves the handleability and appearance quality during thermoforming, and ensures that the molded bodies have excellent shape stability and beverage extractability in a thermal environment. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115434076B_ABST
    Figure CN115434076B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a biodegradable nonwoven fabric having high elongation, high thermal stability and excellent formability while being biodegradable. The present invention is a nonwoven fabric composed of fibers of a polylactic acid polymer and having a unit area weight of 20 to 300 g / m 2 A biodegradable nonwoven fabric for thermoforming, preferably characterized in that it is composed of long fibers of a polylactic acid polymer, has an elongation in the MD direction at 120°C of 50% or more, and has a dimensional change rate in the MD direction at 80°C to 140°C obtained by thermomechanical analysis of ±4% or less, and a method for manufacturing a molded body using the same, and a molding method for a biodegradable beverage extraction container characterized in that the elongation change rate in the MD direction of the molded body when a load of 0.05N / 2mm is applied at 30 to 100°C by thermomechanical analysis (TMA) is 4% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application filed on October 12, 2017, with application number 201780062701.X, and invention name “Biodegradable Nonwoven Fabric”. Technical Field

[0002] The present invention relates to a biodegradable nonwoven fabric and a formed body having high elongation, high thermal stability and excellent molding and processing properties. Background Art

[0003] Molded articles made of biodegradable nonwoven fabrics are known to be used in various fields and their applications are widely developed. Molded articles can be obtained by thermoforming nonwoven fabrics, but it is difficult to obtain a molded article with no cracks, little stretching unevenness, and a beautiful shape that follows the shape of the molding die during thermoforming.

[0004] The following Patent Document 1 discloses a method for obtaining a biodegradable long-fiber nonwoven fabric formed from a polylactic acid-based polymer and an aliphatic polyester copolymer. By forming a sea-island type composite long fiber in which a polylactic acid-based polymer forms a sea portion and an aliphatic polyester copolymer forms an island portion, the aliphatic polyester copolymer forming the island portion is exposed on the fiber surface, thereby obtaining a nonwoven fabric with improved thermal bonding and formability. However, in thermoforming, it is not sufficient to obtain a molded body with no cracks, less stretching unevenness, and a beautiful shape that follows the shape of the molding mold in a shorter time.

[0005] In addition, the following cited documents 2 and 3 disclose methods for obtaining biodegradable nonwoven fabrics for molding formed from polylactic acid or polybutylene succinate. However, since the constituent fibers are partially formed by heat pressing, the adhesion between the fibers is too strong, and it is difficult to obtain a molded body with no bag breakage and a deep molding depth during thermoforming.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 5486331

[0009] Patent Document 2: Japanese Patent No. 3432340

[0010] Patent Document 3: Japanese Patent Application Publication No. 2000-136479 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] In view of the above-mentioned problems of the prior art, an object of the present invention is to provide a nonwoven fabric which has high elongation, high thermal stability and excellent moldability while being biodegradable.

[0013] Solutions for solving problems

[0014] The present inventors have conducted intensive research and repeated experiments to solve the above problems. As a result, they focused on the properties of the nonwoven fabric before molding and found that, by using fibers of a polylactic acid polymer, having an elongation of 50% or more in the MD direction at 120°C and a dimensional change rate of ±4% or less in the MD direction at 80°C to 140°C as determined by thermomechanical analysis, a molded product without cracking during thermoforming, less uneven stretching, and a beautiful shape can be obtained in a shorter time, and a molded product with good handling properties during thermoforming, a nonwoven fabric that can follow a complex molded shape, and excellent appearance can be obtained. Furthermore, the present inventors also found that, with respect to the thermal stability of the molded product, the elongation change rate in the MD direction when a load of 0.05 N / 2 mm is applied to the molded product sheet constituting the container at 30 to 100°C is 4% or less, and thus, the expansion of the contents during extraction can be prevented, and the container can be prevented from being broken due to contact or friction with the beams inside the extractor, etc., and thus the present invention was completed.

[0015] That is, the present invention is as follows.

[0016] [1] A biodegradable nonwoven fabric for thermoforming, which is composed of fibers of a polylactic acid polymer and has a unit weight of 20 to 350 g / m 2 .

[0017] [2] The biodegradable nonwoven fabric according to [1], wherein the elongation in the MD direction at 120°C is 50% or more, and the dimensional change rate in the MD direction at 80°C to 140°C obtained by thermomechanical analysis is ±4% or less.

[0018] [3] The biodegradable long-fiber nonwoven fabric according to [1] or [2], wherein the storage modulus of the nonwoven fabric in a temperature range of 90°C to 150°C in a temperature dependency test for evaluating dynamic viscoelasticity is 10 to 500 MPa.

[0019] [4] The biodegradable nonwoven fabric according to any one of [1] to [3], wherein the value obtained by dividing the warp tear strength of the nonwoven fabric by the weight per unit area is 0.002 to 0.5 N / (g / m 2 ).

[0020] [5] The biodegradable nonwoven fabric according to any one of [1] to [4], wherein the birefringence of the fibers in the nonwoven fabric is 0.002 to 0.10.

[0021] [6] The biodegradable nonwoven fabric according to any one of [1] to [5] above, wherein the fibers in the nonwoven fabric further contain 0.5 to 30% by weight of an aliphatic ester copolymer in addition to the polylactic acid polymer, based on the total resin weight.

[0022] [7] The biodegradable long-fiber nonwoven fabric according to any one of [1] to [6] above, wherein the average fiber diameter of the nonwoven fabric is 1 to 40 μm and the nonwoven fabric is composed of long fibers.

[0023] [8] The biodegradable nonwoven fabric according to any one of [1] to [7], wherein the maximum value of the loss tangent (tan δ) of the nonwoven fabric in a temperature dependency test for dynamic viscoelasticity evaluation is 0.5 or less.

[0024] [9] The biodegradable nonwoven fabric according to any one of [1] to [8], wherein the storage modulus of the nonwoven fabric at 10 to 70°C in a temperature dependency test for evaluating dynamic viscoelasticity is 200 MPa or more.

[0025]

[10] The biodegradable nonwoven fabric according to any one of [1] to [9], wherein the R / Ave value of the 2.5 cm square unit area weight of a stretched sheet obtained by simultaneously stretching the nonwoven fabric in both MD / CD directions at a temperature of 120°C to an area ratio of 6.25 times is within 1.0.

[0026]

[11] The method for producing a biodegradable nonwoven fabric according to any one of [1] to

[10] , comprising the step of heat-setting at a fixed length within a range of 50°C to 160°C.

[0027]

[12] A method for producing a molded article, comprising the step of integrally processing the biodegradable long-fiber nonwoven fabric according to any one of [1] to

[10] by thermoforming.

[0028]

[13] The method according to

[12] , comprising the step of preheating the nonwoven fabric to 55°C to 160°C.

[0029]

[14] A molded article comprising the biodegradable nonwoven fabric according to any one of [1] to

[10] above, and having a molding index of 1.1 or more.

[0030]

[15] A group of formed bodies, which is composed of the biodegradable nonwoven fabric described in any one of the above [1] to

[10] , has a forming index of 1.1 to 20 times, and the R / Ave value of the unit area weight of the fabric pieces collected from the same position on the bottom of at least 10 or more formed bodies formed by continuous nonwoven fabric using the same forming machine is within 0.5.

[0031]

[16] A biodegradable beverage extraction container, which is the molded body described in the above

[14] , characterized in that the elongation change rate in the MD direction when a load of 0.05 N / 2 mm is applied to the molded body sheet constituting the container at 30 to 100°C using thermomechanical analysis (TMA) is less than 4%.

[0032]

[17] The beverage extraction container according to

[16] above, wherein the capacity change when immersed in boiling water is 20% to 90%.

[0033]

[18] The beverage extraction container according to

[16] or

[17] above, characterized in that the orientation degree of the nonwoven fabric molded body is 0.010 or more.

[0034]

[19] The beverage extraction container according to any one of

[16] to

[18] above, wherein the nonwoven fabric molded body has a crystallinity of 30 to 70%.

[0035] Effects of the Invention

[0036] The biodegradable nonwoven fabric of the present invention can be used to obtain a molded product with no cracks during thermoforming, less uneven stretching, and beautiful shapes in a shorter time. In addition, it can obtain a molded product with good handleability during thermoforming and excellent appearance because the nonwoven fabric can follow complex molding shapes during thermoforming, such as a food container. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram of a typical example of the structure of the beverage extraction container according to another embodiment of the present invention.

[0038] Figure 2 It is a schematic diagram for explaining a typical example of a beverage extraction container with a lid according to another embodiment of the present invention.

[0039] Figure 3 This is a graph showing the evaluation of the temperature dependency of the storage modulus in Example 10 and Comparative Example 1.

[0040] Figure 4 This is a graph showing the evaluation of the temperature dependency of the loss tangent value in Example 10 and Comparative Example 1. DETAILED DESCRIPTION

[0041] Hereinafter, embodiments of the present invention will be described in detail.

[0042] The biodegradable nonwoven fabric of the present embodiment has appropriate elongation and dimensional change rate under a thermal environment and can exhibit high molding processability.

[0043] The biodegradable nonwoven fabric of this embodiment has molding processing characteristics. In the past, in the manufacture of biodegradable nonwoven fabrics with molding processing characteristics, the characteristics of the yarns just after spinning were focused on, the elongation was expressed, and the thermal compression bonding processing of the nonwoven fabric was improved. In contrast, in the biodegradable nonwoven fabric of this embodiment, the characteristics of the nonwoven fabric itself used for molding and the characteristics of the molded body itself were focused on, and a nonwoven fabric with high molding processing characteristics and an extraction container (molded body) with excellent thermal stability were obtained.

[0044] [Polylactic acid polymer]

[0045] As the polylactic acid polymer (hereinafter also referred to as PLA) constituting the fiber of the biodegradable nonwoven fabric of the present embodiment, there can be listed a polymer selected from the group consisting of a polymer of D-lactic acid, a polymer of L-lactic acid, a copolymer of D-lactic acid and L-lactic acid, a copolymer of D-lactic acid and hydroxycarboxylic acid, a copolymer of L-lactic acid and hydroxycarboxylic acid, and a polymer of a copolymer of D-lactic acid, L-lactic acid and hydroxycarboxylic acid, or a mixture of two or more of the polymers. The D / L ratio of the polylactic acid polymer can be set within a range that does not hinder the spinnability and nonwoven fabric properties, and the D body ratio in the total polylactic acid weight is preferably 0 to 15%, more preferably 0.1 to 10%, and further preferably 0.1 to 6%. If the D body ratio is within these ranges, the spinnability is good, and a nonwoven fabric can be obtained stably. In addition, the melting point, crystallinity, etc. are within an appropriate range, and a nonwoven fabric with desired properties is easily obtained.

[0046] The MFR of the polylactic acid polymer of the present embodiment is preferably 20 to 120 g / 10 minutes, more preferably 30 to 70 g / 10 minutes. If the MFR is 20 g / 10 minutes or more, the melt viscosity is suitable, and the fiber is easily thinned in the spinning process, so the spinnability is good. On the other hand, if the MFR is 120 g / 10 minutes or less, the melt viscosity is suitable, so there is less occurrence of single filament breakage in the spinning process, and the spinnability is good.

[0047] [Aliphatic polyester copolymer]

[0048] Examples of aliphatic polyester copolymers include poly(α-hydroxy acids) or copolymers containing them as main repeating unit elements, poly(ω-hydroxyalkanoates) such as poly(ε-caprolactone) and poly(β-propiolactone), poly(β-polyhydroxyalkanoates) such as poly-3-hydroxypropionate, poly-3-hydroxyheptanoate, and poly-3-hydroxyoctanoate, or copolymers of repeating unit elements constituting these and repeating unit elements constituting poly-3-hydroxyvalerate and poly-4-hydroxybutyrate. In addition, examples include polyalkylene dicarboxylates containing polycondensates of diols and dicarboxylic acids, such as polyethylene oxalate, polyethylene succinate, polyethylene adipate, polyethylene azelate, polybutylene oxalate, polybutylene succinate, polybutylene adipate, polybutylene sebacate, polyhexane sebacate, polyneopentyl oxalate, or polyalkylene dicarboxylate copolymers constituting repeating unit elements constituting these.

[0049] Furthermore, a mixture obtained by selecting a plurality of these biodegradable polymers and mixing them can be mentioned. As the aliphatic polyester copolymer, polybutylene succinate (hereinafter also referred to as PBS) is preferred from the viewpoint of compatibility with polylactic acid and spinnability.

[0050] The MFR of the aliphatic ester copolymer is preferably 100 g / 10 minutes or less, which has good stretchability in the spinning process, more preferably 20 to 80 g / 10 minutes, and further preferably 30 to 70 g / 10 minutes. In addition, the melt flow ratio of the polylactic acid polymer to the aliphatic polyester copolymer needs to be in the range of 0.2 to 1.5. That is, 0.2 ≤ [melt flow of the aliphatic polyester copolymer / melt flow of the polylactic acid polymer] ≤ 1.5, preferably 0.3 to 1.4. If the melt flow ratio is within these ranges, the spinnability is good, and the dispersibility of the aliphatic polyester copolymer becomes good, so that stable thermal adhesiveness is obtained.

[0051] In addition to the aforementioned polylactic acid polymer, the aforementioned fiber may further contain an aliphatic ester copolymer of 0.5 to 30 weight % based on the total resin weight. The amount of the aliphatic polyester copolymer added is 0.5 to 30 weight %, preferably 3 to 27 weight %, and more preferably 5 to 25 weight % when the total amount of the resin is 100 weight %. If the addition amount is 0.5 weight % or more, it is easy to adjust the crystallinity of the nonwoven fabric, and the thermal properties become good. On the other hand, if the addition amount is 30 weight % or less, crystallization is accelerated, and the fibers or the fibers and the equipment will not adhere to each other during spinning, so stable production can be carried out.

[0052] The manufacturing method of the nonwoven fabric of the present embodiment is not limited, and the nonwoven fabric can be obtained by a known spunbond method, meltblown method, air-laid method, carding method, papermaking method, etc. As a bonding method of the nonwoven fabric, embossing, thermal bonding, columnar flow interlacing, mechanical interlacing, needle punching, etc. can be used. From the viewpoint of being able to produce efficiently and suppressing the fuzzing after molding, it is preferably a long-fiber nonwoven fabric, and then manufactured by a spunbond method.

[0053] In the case of the spunbond method, the resin is heated and melted and ejected from the spinning nozzle, and the obtained spun filaments are cooled using a known cooling device and pulled thin using a suction device such as an air suction device. Next, the filaments discharged from the suction device are opened and accumulated on a conveyor belt to form a web. Next, the web formed on the conveyor belt is partially heat-pressed using a partial heat-pressing device such as a heated embossing roll, thereby obtaining a long-fiber spunbond nonwoven fabric.

[0054] When the spunbond method is used, there is no particular limitation. In order to improve the uniformity of the web, for example, a method of charging the fibers by a corona device, such as disclosed in Japanese Patent Laid-Open No. 11-131355, is used; a device for controlling the airflow, such as a flat dispersion plate, is used to adjust the velocity distribution of the airflow in the ejection part of the ejector, so that the fibers are opened and then ejected to suppress the scattering of the web while stacking it on the collecting surface, thereby forming a further preferred manufacturing method.

[0055] The nonwoven fabric obtained by the spunbond method has strong fabric strength and physical properties such as no shedding of short fibers due to damage of the bonding parts. In addition, due to low cost and high productivity, it is used in a wide range of applications, mainly in sanitation, civil engineering, construction, agriculture and gardening, and daily materials.

[0056] The biodegradable nonwoven fabric of the present embodiment is characterized in that the dimensional change rate in the MD direction at 80° C. to 140° C. obtained by thermomechanical analysis is ±4% or less.

[0057] The biodegradable nonwoven fabric of the present embodiment has a dimensional change rate in the MD direction at 80°C to 140°C obtained by thermomechanical analysis of ±4% or less, preferably ±2% or less. When the dimensional change rate is not too high, the nonwoven fabric has appropriate softness near the molding temperature, and can follow the molding of complex shapes, and can obtain a molded body with few broken bags, few uneven surfaces of the formed molded body, and few elongation unevenness such as partial elongation of the nonwoven fabric, and a beautiful shape and excellent appearance. On the other hand, when the dimensional change rate is less than minus 4%, that is, when the shrinkage is too large, the fabric is unstable due to the heat caused by preheating during molding and the radiation heat of the mold, and the shape of the obtained molded body is poor, and a molded body with large capacity cannot be obtained. On the other hand, when the dimensional change rate exceeds plus 4%, that is, when the elongation is too large, the fabric is unstable due to the heat caused by preheating during molding and the radiation heat of the mold, and the shape of the obtained molded body is deteriorated.

[0058] As a specific method for making the dimensional change rate within the range, for example, the resin type of the biodegradable nonwoven fabric, the resin mixing ratio, the resin temperature during spinning, the ejection amount, speed, atmosphere temperature, cooling and other spinning conditions, pre-pressing, roller temperature during heat pressing, pressure, speed, aging and other conditions, storage conditions, etc. Specifically, for example, a fabric with less dimensional change can be obtained by increasing the spinning speed, lowering the atmosphere temperature, raising the cooling conditions, performing heat pressing at a high temperature, and heat setting the pre-pressed nonwoven web to a fixed length at a temperature that is not too high.

[0059] The biodegradable nonwoven fabric of the present embodiment is characterized in that the elongation in the MD direction at 120°C is 50% or more.

[0060] The biodegradable nonwoven fabric of the present embodiment needs to have elongation when heated during the molding process. Therefore, for example, the nonwoven fabric needs to be formed of low-stretch yarns, the fibers need to elongate when heated, or the constituent fibers of the nonwoven fabric need to be offset. Therefore, for the elongation when heated of the biodegradable nonwoven fabric of the present invention, the elongation at a temperature of 120°C is 50% or more, preferably 50% to 500%, more preferably 100% to 400%, and further preferably 180% to 350%. If the elongation is within the range, the moldability is good, and the greater the elongation, the easier it is to form a deep drawing with a deep molding depth.

[0061] As a specific method for making the elongation at 120°C fall within the range, for example, the method can be carried out by adjusting the resin type of the biodegradable nonwoven fabric, the resin mixing ratio, the resin temperature during spinning, the ejection amount, speed, atmospheric temperature, spinning conditions such as cooling, pre-pressing, roller temperature during thermocompression bonding, pressure, speed, aging, storage conditions, etc. Specifically, for example, by not too high a spinning speed during spinning, thermocompression bonding at a temperature not too high, obtaining a nonwoven web in a state where the atmospheric temperature during spinning is not too low, and performing thermocompression bonding, etc., a nonwoven fabric having appropriate bonding points and high elongation can be obtained.

[0062] The biodegradable nonwoven fabric of the present embodiment preferably has a value obtained by dividing the warp tear strength by the weight per unit area of ​​0.002 to 0.5 N / (g / m 2 ), more preferably 0.005 to 0.2 N / (g / m 2 ). The warp tear strength is strongly related to the strength, elongation and bonding strength of the fibers. When the warp tear strength is too low, the fiber strength is low or the bonding between the fibers is too strong. On the other hand, when the warp tear strength is too high, the fiber strength and elongation are high or the bonding between the fibers is too weak. The fiber strength and bonding strength between the fibers that affect the tear strength can be adjusted to an appropriate range by spinning conditions such as spinning speed and resin temperature, embossing, calendering, processing temperature during hot pressing, processing speed, aging conditions, etc.

[0063] When the value obtained by the warp tear strength divided by the weight per unit area is not too large, the fibers constituting the biodegradable nonwoven fabric are appropriately bonded, and even after molding, the fibers are also appropriately bonded, so even after molding, the fibers are not easy to float and are not easy to produce fluff. Then, when the value obtained by the warp tear strength divided by the weight per unit area is not too large, there is appropriate rigidity, even under process tension, there is also appropriate tension, and the nonwoven fabric is easy to pass through the process, which is suitable. On the other hand, when the value obtained by the warp tear strength divided by the weight per unit area is not too low, there is appropriate bonding between the fibers, and the fiber strength is not too low, and the biodegradable nonwoven fabric has appropriate elongation and strength, and it is easy to handle.

[0064] The weft tear strength is preferably set within a range where fibers constituting the biodegradable nonwoven fabric are appropriately bonded to each other, and the nonwoven fabric is preferably set within a range where the nonwoven fabric can pass through the process while having appropriate rigidity while having warp tear strength.

[0065] The birefringence of the biodegradable nonwoven fabric (long fibers constituting the biodegradable nonwoven fabric sampled from the nonwoven fabric) of the present embodiment (i.e., not the birefringence of the long fibers constituting the nonwoven fabric just after spinning) is preferably 0.002 to 0.10, more preferably 0.005 to 0.10, and further preferably 0.010 to 0.025. When the birefringence is not too high, a biodegradable nonwoven fabric with high elongation can be obtained, and when the birefringence is not too low, stability in a thermal environment can be obtained. The birefringence of the biodegradable nonwoven fabric (fibers constituting the biodegradable nonwoven fabric sampled from the nonwoven fabric) of the present embodiment is a characteristic of the biodegradable nonwoven fabric, and the birefringence of the long fibers constituting the biodegradable nonwoven fabric before hot pressing and just after spinning is not particularly limited as long as it is within a range that does not hinder the spinnability, hot pressing properties, and elongation performance of the nonwoven fabric.

[0066] The crystallinity of the biodegradable nonwoven fabric of the present embodiment (the fiber constituting the biodegradable nonwoven fabric sampled from the nonwoven fabric) is preferably 30 to 70%, more preferably 35 to 62%, and further preferably 38 to 57%. When the crystallinity is not too low, there will be no situation where the shape of the molded body is deformed due to shrinkage when the cloth falls off the molding die during the molding process. On the other hand, when the crystallinity is not too high, the bag can be processed without breaking during the molding process.

[0067] The nonwoven fabric of this embodiment has a weight per unit area of ​​20 to 300 g / m 2 , preferably 20 to 250 g / m 2 If the unit area weight is 20g / m 2 If the strength is above 300 g / m 2 Then, the molding process can be performed without placing a heavy burden on the molding equipment.

[0068] The average fiber diameter of the biodegradable nonwoven fabric of this embodiment (the fibers constituting the biodegradable nonwoven fabric sampled from the nonwoven fabric) is preferably 1 to 40 μm, more preferably 10 to 40 μm, and further preferably 15 to 35 μm. The permeability and content retention can be appropriately selected by the unit area weight and the average fiber diameter. If the average fiber diameter is not too small, the container can retain the content (good powder leakage), and if the average fiber diameter is not too large, the liquid permeability will not be too slow.

[0069] There is no particular limitation on the shape of the fibers constituting the biodegradable nonwoven fabric of this embodiment. Circular, flat, C-shaped, Y-shaped, V-shaped and other irregular cross-sections may be used, preferably a circular cross-section, and further may be an island-in-the-sea structure, a core-sheath structure, or a spliced ​​structure.

[0070] The shape of the biodegradable nonwoven fabric of the present embodiment may be, for example, a layer of a multi-layered nonwoven fabric such as SS, SMS, SMMS, SMSM, etc. Here, S refers to a spunbond long-fiber nonwoven fabric, and M refers to a meltblown ultrafine nonwoven fabric. Alternatively, a short-fiber nonwoven fabric layer may be laminated using the biodegradable nonwoven fabric as a base material.

[0071] The biodegradable nonwoven fabric of the present embodiment is obtained by known spunbonding, meltblowing, flash evaporation, thermal bonding, air-laid, columnar interlacing, mechanical interlacing, etc. From the viewpoint of the strength of the nonwoven fabric, a long-fiber nonwoven fabric obtained by spunbonding is preferred.

[0072] The fiber constituting the biodegradable nonwoven fabric of the present embodiment may be a low-stretch composite fiber containing at least a polylactic acid polymer and preferably also aliphatic polyester copolymer. For the low-stretch composite fiber of polylactic acid polymer fiber and aliphatic polyester copolymer, the crystal orientation degree of the spinning process is suppressed to a low level, the crystallinity is low, the stretchability is good, and high elongation and high stretching can be achieved. It is preferred to use a fiber obtained at a low spinning speed of 500 to 3000 m / min, more preferably a spinning speed of 700 to 2700 m / min, and further preferably 900 to 2500 m / min. Generally, when the spinning speed is fast, the silk just after spinning forms a silk with high crystallinity and orientation, and when the spinning speed is slow, a silk with low crystallinity and low orientation is formed.

[0073] In the manufacture of the fibers constituting the biodegradable nonwoven fabric of the present embodiment, one or more of other resins, copolymers other than aliphatic polyester copolymers, flame retardants, inorganic fillers, softeners, plasticizers, pigments, antistatic agents, etc. may be added to the fibers constituting the nonwoven fabric as needed.

[0074] The heat pressing in the manufacture of the biodegradable nonwoven fabric of the present embodiment may be embossed, but since the heat stretchability is easily increased, it is preferred to integrate the fibers of the pre-heat pressing nonwoven web by point bonding. There is no particular limitation on the pre-heat pressing method, but preferably, a method using a pair of embossing rollers having a concave-convex pattern on at least one surface, a method using a pair of smooth rollers having a flat surface, etc. are listed, and a method of joining the nonwoven fabrics by needle punching, hydroentanglement, etc. may also be used.

[0075] In the case of obtaining a nonwoven fabric integrated by point bonding, by performing preheating and pressing and thermal bonding in two stages, the fiber bonding in the biodegradable nonwoven fabric remains at a light thermal bonding, and the point bonding on the fiber surface becomes the main part. Even if an embossed pattern is added by preheating and pressing, the thermal bonding on the surface is suppressed in the second stage, and a slight thermal shrinkage is exhibited around the embossed pattern. The embossed pattern falls off or weakens, and the overall unit area weight of the biodegradable nonwoven fabric is unevenly reduced.

[0076] When embossing in pre-compression bonding is combined with hot compression bonding, the compression bonding by embossing is preferably not too strong in order to prevent excessive concentration of stress during heat stretching. There is no particular restriction on the compression bonding area ratio in embossing, but high-frequency and weak bonding is preferred. The compression bonding area ratio is preferably 3 to 50% relative to the total area of ​​the nonwoven fabric, and more preferably 5 to 40%.

[0077] The second step of thermal bonding is not particularly limited as long as the method can suppress the thermal bonding of the nonwoven fabric on the surface, but it is preferable to use a felt roll calendering process or a hot air process.

[0078] In addition, when embossing is performed as a common processing method used in thermal bonding of nonwoven fabrics, the fibers are firmly pressed together by thermal pressing, so the fiber shape cannot be maintained at the pressed part, the fibers are in a crushed shape, and the fibers are thermally bonded to each other to form a film, forming an embossed pattern. When a nonwoven fabric containing a portion that has been excessively crystallized and filmized is stretched in a hot environment, it may be difficult to obtain a high elongation. In addition, in a molded body using a nonwoven fabric made by embossing, since it contains a filmized portion, the liquid permeability is deteriorated in applications that require liquid permeability, which may cause problems.

[0079] When the biodegradable nonwoven fabric of the present embodiment is pre-bonded, first, a pair of embossing rolls having a concave-convex pattern on at least one surface are used to perform thermal bonding at a roll temperature of 25 to 100° C., preferably 35 to 80° C., and a line pressure of 50 to 1000 N / cm, preferably 200 to 700 N / cm, thereby obtaining a pre-heat-pressed biodegradable nonwoven fabric. Next, the pre-heat-pressed biodegradable nonwoven fabric is thermally bonded at a roll temperature of 50 to 160° C., preferably 80 to 150° C., using a felt-covered roller calender roll, thereby melting the surfaces of the fibers at the interlaced points between the fibers and bonding them to each other in a point-like manner, thereby increasing the frequency of the presence of the bonding portion. Furthermore, the point-like bonding is a weaker bond than the usual thermal bonding, so that the stretching process can be uniformly performed with a small stress, and is therefore suitable for thermoforming accompanied by a large stretch.

[0080] As a method for obtaining the biodegradable nonwoven fabric of the present embodiment, fixed-length heat setting is preferably performed. The nonwoven web just after spinning is heated by applying heat under tension during hot pressing, so that a nonwoven fabric with good surface properties and heat extensibility is obtained, and it will not break during molding, and a molded body with a beautiful shape is obtained, so it is preferred. As a method for fixed-length heat setting, a common method can be used, and hot air drying, pin chain tenter drying, heating plate, calendering, felt roller calendering, hot air processing, hot pressing, etc. can be used. As a temperature range for fixed-length heat setting, if it is a temperature at which the resin constituting the nonwoven fabric does not adhere to the device and the fibers of the nonwoven fabric are properly bonded, it is not particularly limited, but it is preferably 50°C to 160°C, more preferably 70°C to 160°C, and further preferably 80°C to 150°C. When the temperature for fixed-length heat setting is not too high, contamination from the nonwoven fabric is not easily attached to the device, and a nonwoven fabric with good handling and productivity can be obtained. On the other hand, when the viscosity is not too low, the fibers of the nonwoven fabric can be properly bonded to each other.

[0081] In the past, as a non-woven fabric with thermoformability, the elongation during heat treatment was obtained by reducing the crystallinity and orientation of the fiber just after spinning. However, the state in which the crystallinity and orientation of the fiber just after spinning are low is a state of residual instability to heat, and it is difficult to make the state of thermocompression bonding appropriate when forming a non-woven fabric. For example, in the case of thermocompression bonding by embossing, a state in which there are many crystalline parts is formed in the embossed part, and on the other hand, a state in which there are many non-crystalline parts is formed in the non-embossed part. During thermoforming, the boundary part and the embossed part of the embossed part and the non-embossed part are easily destroyed, and it is possible to be difficult to obtain a molded body that will not break during thermoforming and has a beautiful shape. In addition, as a method for setting the crystallinity and orientation to be low, the spinning conditions can also be adjusted, but when the spinning speed is reduced and the fiber is not stretched, a non-woven web with low crystallinity and orientation is formed. If thermocompression bonding is performed under the state in which the crystallinity and orientation are low, there is a situation in which excessive crystallization is carried out and a non-woven fabric with excellent formability cannot be obtained. Therefore, in the present embodiment, in order to stabilize the processing in the unstable state of the nonwoven fabric, it is preferable to perform thermocompression bonding, felt roll calendering, hot air processing, aging, etc.

[0082] So far, as a method for obtaining thermoformability, it is necessary to suppress oriented crystallization during spinning as described in Patent Documents 1 to 3 and Japanese Patent Gazette No. 01-047581. The spinning speed is slowed down to form a structure with many non-crystalline parts. However, non-woven fabrics with many non-crystalline parts are in a state that is easily affected by heat, and most of them have no dimensional stability under hot environments. Here, if the resin properties of polylactic acid are compared with polyester, polylactic acid requires sufficient time / heat during thermoforming due to its low melting point, small difference between melting point and glass transition temperature, and slow crystallization time. However, if embossing is performed in order to improve the thermal stability of the non-woven fabric, shrinkage occurs and it is difficult to make the non-woven fabric. Therefore, the biodegradable non-woven fabric of this embodiment with dimensional stability is preferably subjected to fixed-length heat setting in which heat can be applied under tension.

[0083] Furthermore, in this embodiment, as the thermal property evaluation of the molded nonwoven fabric, the storage modulus and the loss tangent value in the temperature dependency evaluation of the dynamic viscoelasticity are focused on, and these parameters are optimized, thereby obtaining good ductility and heat resistance stability as the molded nonwoven fabric.

[0084] In order to obtain a non-woven fabric with excellent ductility, it is important to control the mobility and orientation of the amorphous part of the resin. Therefore, in the past, methods such as reducing the crystallinity and orientation of the fiber just after spinning were used. However, in actual molding, the non-woven fabric is used in a temperature environment such as transportation at room temperature, preheating, and heating caused by thermoforming, and it is difficult to evaluate the suitability solely with these physical property values. Therefore, the storage modulus and the loss tangent value in the temperature dependence evaluation of the dynamic viscoelasticity that evaluates the rigidity and softness of the resin relative to temperature changes are used to evaluate the suitability in the molding process, and the manufacturing conditions of the non-woven fabric are optimized, thereby obtaining a non-woven fabric with excellent ductility and thermal stability.

[0085] For the nonwoven fabric of the present embodiment, the storage modulus in the temperature range of 90°C to 150°C in the evaluation of the temperature dependence of dynamic viscoelasticity is always 15 to 500 MPa, preferably 20 to 300 MPa, more preferably 20 to 200 MPa, and particularly preferably 25 to 150 MPa. When the storage modulus at 90°C to 150°C is within this range, when hot press molding is performed, a molded body having excellent appearance with excellent appearance and good shape can be obtained, which can follow the deformation caused by the mold, has less bag breakage, has less unevenness on the surface of the formed molded body, and has less unevenness in elongation such as partial elongation of the nonwoven fabric. On the other hand, when the storage modulus is lower than this range, the mechanical strength of the nonwoven fabric is excessively reduced due to the heat during molding, so it is easy to cause uneven stretching due to the shape of the mold, uneven heating temperature, etc. On the other hand, when the storage modulus exceeds this range, even if heat is provided during molding, the fabric is easy to break when stretched by the mold due to the higher mechanical strength.

[0086] For the nonwoven fabric of the present embodiment, the storage modulus in the temperature range of 10°C to 70°C in the temperature dependence evaluation of dynamic viscoelasticity is always 200 MPa, preferably 250 MPa or more, and more preferably 300 MPa or more. When the storage modulus at 10°C to 70°C is within this range, the nonwoven fabric will not break or deform during the molding process, and the nonwoven fabric can be well conveyed.

[0087] For the nonwoven fabric of the present embodiment, the maximum value of the loss tangent value (tanδ) in the temperature dependency test of dynamic viscoelasticity evaluation is 0.5 or less, preferably 0.45 or less, and more preferably 0.4 or less. The maximum value of tanδ obtained in the temperature dependency test of dynamic viscoelasticity represents the degree of freedom of the molecules, and the larger the value, the wider the movable area of ​​the molecules. That is, if tanδ at any temperature is greater than 1, the degree of freedom of the molecules at that temperature is large, the fabric is unstable to heat, and thermal shrinkage is induced.

[0088] For the nonwoven fabric of the present embodiment, the rate of change of the storage modulus with respect to temperature in the temperature dependence test of dynamic viscoelasticity evaluation is preferably 3 to 50 MPa, more preferably 5 to 35 MPa, and further preferably 10 to 25 MPa. If the rate of change of the storage modulus with respect to temperature is within the above range, the followability to the molding die during thermoforming is appropriate, and molding can be performed without uneven molding or broken bags. When the rate of change of the storage modulus with respect to temperature is less than the above range, the rigidity of the sheet is high during molding, so the followability to the molding die is poor, resulting in broken bags due to sheet rupture. On the other hand, when the rate of change of the storage modulus with respect to temperature is greater than the above range, the followability becomes too good for deformation during molding, resulting in meshes and broken bags due to overstretching.

[0089] The rate of change of storage modulus with respect to temperature can be calculated by the following formula, which is obtained by dividing the change of storage modulus by the value of temperature change when performing a temperature dependency test of dynamic viscoelasticity:

[0090] Temperature dependence test of dynamic viscoelasticity = -Δ storage modulus / Δ temperature.

[0091] In particular, in the molding process, molding is performed in multiple rows to improve productivity, so uneven heating in the row direction and other precision unevenness are likely to occur on the equipment. Therefore, by ensuring that the storage modulus, loss tangent value, and storage modulus change rate with respect to temperature in the temperature dependence evaluation of the dynamic viscoelasticity of the nonwoven fabric are within the above-described ranges, bag breakage and uneven molding during molding can be suppressed, and stable production in terms of quality can be achieved.

[0092] There is no particular limitation on the specific method for making the storage modulus and loss tangent value in the dynamic viscoelasticity evaluation fall within the above ranges. The inventors have completed the present invention by making the heat-pressing method of the spun fabric and the birefringence of the fibers in the nonwoven fabric obtained by heat-pressing the fabric the most appropriate values. As a specific method, for example, the method can be carried out by adjusting the resin type of the nonwoven fabric, the mixing ratio of the resin, the spinning conditions such as the resin temperature, the ejection amount, the speed, the atmosphere temperature, and the cooling during spinning, the pre-pressing, the roller temperature, pressure, speed, aging, and storage conditions during heat-pressing, and the like. Specifically, for example, by making the spinning speed during spinning not too high, performing heat-pressing at a temperature not too high, obtaining the nonwoven web and performing heat-pressing in a state where the atmosphere temperature during spinning is not too low, etc., a nonwoven fabric having appropriate bonding points and high elongation can be obtained.

[0093] During molding, the nonwoven fabric is stretched simultaneously in the flow direction and the width direction of the nonwoven fabric through a die. Therefore, the present inventors evaluated the uniform moldability of the nonwoven fabric by simultaneously stretching in biaxial directions and evaluating the weight non-uniformity per unit area in addition to the conventional tensile test in the uniaxial direction as an index for evaluating the uniformity after molding in thermoforming.

[0094] The biodegradable nonwoven fabric of the present embodiment is characterized in that the value of R / Ave is 1.0 or less with respect to the unit weight per square unit of 2.5 cm of the stretched sheet formed by simultaneously stretching the sheet to an area ratio of 6.25 times in the MD / CD biaxial directions at a temperature of 120°C. For the biodegradable long-fiber nonwoven fabric of the present embodiment, the value of R / Ave is 1.0 or less, preferably 0.7 or less with respect to the unit weight per square unit of 2.5 cm of the stretched sheet formed by simultaneously stretching the sheet to an area ratio of 6.25 times in the MD / CD biaxial directions at a temperature of 120°C. When the value of R / Ave is not too high, the stretching during the forming of the nonwoven fabric becomes uniform, and the retention and liquid permeability of the content powder also become uniform.

[0095] As a specific method for making the R / Ave of the MD / CD biaxially stretched sheet fall within the range, for example, it can be achieved by adjusting the resin type of the biodegradable nonwoven fabric, the resin mixing ratio, the resin temperature during spinning, the ejection amount, speed, atmosphere temperature, cooling and other spinning conditions, pre-pressing, roller temperature during thermocompression, pressure, speed, aging and other conditions, storage conditions, etc. Specifically, for example, by slowing down the spinning speed, increasing the atmosphere temperature, lowering the cooling conditions, thermocompression bonding at a high temperature, and heat setting the pre-pressed nonwoven web at a sufficiently high temperature to a fixed length, a nonwoven fabric with a reduced R / Ave of the MD / CD biaxially stretched sheet can be obtained.

[0096] The biodegradable nonwoven fabric of this embodiment can be integrally processed by thermoforming to form a molded body. There is no particular limitation on the shape of the molded body, and it is preferred to select a semicircular, cylindrical, elliptical, triangular, quadrilateral, etc. according to the purpose of use. In the case of obtaining a molded body with a larger area and capacity than the original nonwoven fabric used in molding, a molding mold that increases the surface area of ​​the nonwoven fabric before and after molding can be appropriately selected.

[0097] The method for forming the shaped nonwoven fabric of the present embodiment is not particularly limited as long as it includes a thermoforming step, and may include a preheating step before thermoforming and a shape-retaining step for maintaining capacity after thermoforming.

[0098] By including a preheating process before thermoforming, the temperature of the nonwoven fabric immediately before forming can be controlled, and the characteristic values ​​of the nonwoven fabric such as the storage modulus can be made into values ​​suitable for forming. The preferred range of the temperature of the nonwoven fabric immediately before forming is 55 to 160°C, the further preferred range is 60 to 130°C, and the particularly preferred range is 70 to 120°C. If the temperature of the nonwoven fabric immediately before forming is below 50°C, the storage modulus is high, and the followability to the forming mold during forming becomes poor, so it is easy to produce poor forming such as broken bags and uneven forming. On the other hand, if the temperature immediately before forming is above 140°C, the storage modulus is too low, and the stress applied to the fabric cannot be fully withstood during forming, resulting in poor forming such as broken bags.

[0099] When the nonwoven fabric used in this embodiment is made of polylactic acid, the crystallization speed is very slow, so during molding, the shrinkage of the molded body due to the residual stress when the sheet is stretched occurs earlier than the crystallization of the sheet, and a molded body with a small capacity is easily formed. Therefore, in order to make the molded body quench and solidify and obtain the shape-keeping effect, a shape-keeping step is included after molding, thereby obtaining a molded body with a large capacity.

[0100] By combining these preheating and shape-keeping steps to perform thermoforming, a process capable of continuous uniform molding can be formed. By molding the nonwoven fabric of this embodiment using these molding processes, a uniform molded body can be provided. For example, the value of R / AVE of the weight per unit area of ​​the cloth collected from the same position at the bottom of a molded body of a product with more than 10 commercially available molded bodies attached at the same time can be within 0.5, and when used for a filter for food, etc., a product can be provided without leakage of contents and without problems in appearance.

[0101] The degree of molding of the biodegradable nonwoven fabric of the present embodiment is represented by a molding index. The molding index refers to a value obtained by dividing the surface area of ​​the molded body by the area of ​​the planar nonwoven fabric before molding (the opening area in the case of a container shape) used in the molded body and defined by the following formula (1):

[0102] Forming index = (surface area of ​​the molded body cm 2 ) / (area of ​​nonwoven fabric before molding cm 2 ).

[0103] The molding index of the molded body composed of the biodegradable nonwoven fabric of the present embodiment is preferably 1.1 or more, more preferably 1.1 to 20, further preferably 1.5 to 10, and most preferably 2.5 to 6. When the molding index is large, it means that the nonwoven fabric has a large elongation. On the other hand, when the molding index is small, it means that the elongation of the nonwoven fabric is small. The biodegradable nonwoven fabric of the embodiment has a high elongation, so it is possible to produce a molded product with a high elongation and a large molding index. When the molding index is not too large, the bag can be molded without breaking. When the molding index is not too small, the container can have an appropriate size when the content is filled.

[0104] In the thermoforming, from the viewpoint of the resin properties of polylactic acid, if it is considered that compared with polyester resin, polyester has a high melting point, a large difference between the melting point and the glass transition temperature, and a fast crystallization rate, so the mold temperature during molding can be increased to obtain a molded body, while polylactic acid has a low melting point, a small difference between the melting point and the glass transition temperature, and a slow crystallization rate, so it is difficult to provide sufficient heat to the nonwoven fabric for molding, and the molding temperature may not be increased. Therefore, the biodegradable nonwoven fabric of this embodiment is preferably heat-set at a fixed length in order to make the shape of the nonwoven fabric before molding firm.

[0105] It should be noted that the general resin properties of polylactic acid and polyester are as follows. In order of polylactic acid and polyester, melting point: 170°C, 260°C, recrystallization temperature: 70°C, 120°C, glass transition temperature 55-60°C, 70-80°C, specific heat: 1.38 J / g·K, 1.00-1.15 J / g·K, thermal conductivity 0.13 W / m·K, 0.2-0.33 W / m·K, semi-crystallization time: 500-900 seconds, 50-100 seconds.

[0106] The nonwoven fabric of this embodiment can be used as a beverage extraction container in a further suitable embodiment by adjusting the molding conditions and controlling the properties of the molded product. [Background Technology]

[0108] Conventionally, as a method for easily extracting extracts such as black tea, green tea, coffee powder, medicine, and Chinese medicine, there is known a method of sealing the extract in a beverage extraction container, using an extractor, and injecting hot water into the container to extract the beverage, such as a single-serve method. As beverage extraction containers, there are beverage extraction containers having pleated paper inside a resin container, beverage extraction containers having nonwoven fabric molded into a container shape inside a resin container, and beverage extraction containers using a molded body obtained by molding nonwoven fabric into a container shape.

[0109] For beverage extraction containers with resin containers, a hole needs to be opened at the bottom of the container in order to ensure a hot water outlet. A needle is provided at the bottom of the container installation portion of the extraction machine.

[0110] Japanese Patent Application Publication No. 2015-85086 discloses a beverage extraction container used in the above-mentioned extractor. In such a beverage extraction container having a molded body formed in a container shape inside a resin container, it is necessary to provide a space at the bottom of the resin container so that a needle does not pierce the molded body, which increases the size of the container and increases the volume during transportation, display, and storage, thus causing problems in terms of handling.

[0111] Generally, when extracting an extract, hot water is poured in, causing the extract to swell. In a beverage extraction container formed into a container-shaped body, the contents swell during extraction, and the container swells and contacts the needle provided in the extractor, causing the nonwoven fabric to break and leak the contents.

[0112] [Problems to be solved by the invention]

[0113] [Solutions to solve the problem]

[0114] In view of the problems of the aforementioned prior art, in the present invention (other embodiments), in order to form a beverage extraction container with excellent shape stability in a thermal environment and beverage extraction performance, in-depth research and repeated experiments have been conducted. It was found that a beverage extraction container with no cracks, good content retention (less powder leakage), and beautiful shape and good shape stability in a thermal environment can be obtained, thereby completing the present invention.

[0115] [Patent Solution]

[0116] Specifically, this is achieved by controlling the properties of the nonwoven fabric after molding as follows.

[0117] (i) the elongation change rate in the MD direction when a load of 0.05 N / 2 mm is applied to the molded body sheet constituting the container at 30 to 100° C. by thermomechanical analysis (TMA) is 4% or less;

[0118] (ii) The capacity change when immersed in boiling water is 20% to 90%.

[0119] (iii) the orientation degree of the nonwoven fabric formed is 0.010 or more;

[0120] (iv) The crystallinity of the nonwoven fabric formed body is 30 to 70%.

[0121] [Effects of the invention]

[0122] By using a biodegradable nonwoven fabric to form a beverage extraction container that satisfies the above characteristics, the shape stability and beverage extraction performance under a hot environment are excellent, and thus the container can be suitably used as a container for extracting black tea, green tea, coffee powder, medicine, Chinese medicine, etc. [Drawings]

[0124] Figure 1 It is a schematic diagram of a typical example of the structure of the beverage extraction container according to another embodiment of the present invention.

[0125] Figure 2 It is a schematic diagram for explaining a typical example of a beverage extraction container with a lid according to another embodiment of the present invention.

[0126] Figure 3 This is a graph showing the evaluation of the temperature dependency of the storage modulus in Example 10 and Comparative Example 1.

[0127] Figure 4 This is a graph showing the evaluation of the temperature dependency of the loss tangent value in Example 10 and Comparative Example 1. [Specific implementation method]

[0129] Hereinafter, embodiments (other embodiments) of the present invention will be described in detail.

[0130] The beverage extraction container of the present embodiment has a suitable structure and molding conditions for the nonwoven fabric constituting the container, and can exhibit shape stability and beverage extraction properties during beverage extraction.

[0131] [Explanation of terms]

[0132] The beverage extraction container of this embodiment represents a nonwoven fabric molded body that has been molded. A lid may be provided to fill and seal the beverage.

[0133] [Raw materials of containers]

[0134] As the raw material of the nonwoven fabric constituting the beverage extraction container of the embodiment of the present application, biodegradable resins, in particular polylactic acid polymers (hereinafter also referred to as PLA) can be used. As polylactic acid polymers, polymers selected from the group consisting of polymers of D-lactic acid, polymers of L-lactic acid, copolymers of D-lactic acid and L-lactic acid, copolymers of D-lactic acid and hydroxycarboxylic acid, copolymers of L-lactic acid and hydroxycarboxylic acid, and copolymers of D-lactic acid, L-lactic acid and hydroxycarboxylic acid, or a mixture of two or more of the polymers. The D / L ratio of the polylactic acid polymer can be set within the range that does not hinder the productivity and properties of the nonwoven fabric, and the D body ratio in the total polylactic acid weight is preferably 0 to 15%, more preferably 0.1 to 10%, and further preferably 0.1 to 6%. If the D body ratio is within these ranges, the crystallinity, melting point, etc. of the nonwoven fabric constituting the beverage extraction container are within an appropriate range, and it is easy to obtain the desired properties as a beverage extraction container.

[0135] Furthermore, other raw materials such as aliphatic polyester copolymers may be used within the range that does not hinder biodegradability. Examples of aliphatic polyester copolymers include poly(α-hydroxy acids) or copolymers having them as main repeating unit elements, poly(ε-caprolactone), poly(ω-hydroxyalkanoates) such as poly(β-propiolactone), poly-3-hydroxypropionate, poly-3-hydroxyheptanoate, poly-3-hydroxyoctanoate, or copolymers of repeating unit elements constituting these and repeating unit elements constituting poly-3-hydroxyvalerate, poly-4-hydroxybutyrate. In addition, polyalkylene dicarboxylates, such as polyethylene oxalate, polyethylene succinate, polyethylene adipate, polyethylene azelate, polybutylene oxalate, polybutylene succinate, polybutylene adipate, polybutylene sebacate, polyhexane sebacate, polyoxalate neopentyl or polyalkylene dicarboxylate copolymers of repeating unit elements that form them can be listed. And then, various polymers that select these biodegradable properties and mix them can be listed. As aliphatic polyester copolymers, from the viewpoint of compatibility with polylactic acid, preferably polybutylene succinate (hereinafter also referred to as PBS) is used. The aliphatic polyester copolymers can improve the stretchability and adhesiveness of the nonwoven fabric during molding, and are easy to obtain good properties such as desired shape, capacity, and surface fuzzing prevention.

[0136] [Addition ratio of aliphatic ester copolymer]

[0137] The aliphatic polyester copolymer added to the nonwoven fabric constituting the beverage extraction container according to the embodiment of the present application may contain, in addition to the aforementioned polylactic acid polymer, 0.5 to 30% by weight of an aliphatic ester copolymer based on the total resin weight. The amount of the aliphatic polyester copolymer added is 0.5 to 30% by weight, preferably 3 to 27% by weight, and more preferably 5 to 25% by weight, when the total amount of the resin is 100% by weight. If the amount added is within the range, the crystallinity can be easily adjusted, and a beverage extraction container with excellent thermal properties can be obtained.

[0138] [Other additives]

[0139] The nonwoven fabric constituting the beverage extraction container of the embodiment of the present application may further contain one or more of other resins, copolymers other than aliphatic polyester copolymers, flame retardants, inorganic fillers, softeners, plasticizers, pigments, antistatic agents, water permeating agents, etc., as needed in the fibers constituting the nonwoven fabric.

[0140] [Long fibers (including non-woven fabrics), short fibers]

[0141] The nonwoven fabric constituting the beverage extraction container according to the embodiment of the present application is obtained by a known spunbond method, meltblown method, airlaid method, carding method, papermaking method, etc. As a bonding method of the nonwoven fabric, embossing, thermal bonding, columnar flow interlacing, mechanical interlacing, needle punching, etc. can be used. From the viewpoint of the strength of the beverage extraction container and the less shedding of fibers during beverage extraction, a continuous long fiber nonwoven fabric obtained by a spunbond method is preferred.

[0142] The nonwoven fabric constituting the beverage extraction container of the embodiment of the present application is not particularly limited as long as it has stretchability that can obtain a molded shape. It is preferred to use fibers obtained by a spunbond method at a low spinning speed of 500 to 3000 m / min, more preferably a spinning speed of 600 to 2700 m / min, and further preferably 700 to 2500 m / min. Generally, when the spinning speed is fast, the yarn just after spinning forms a yarn with high crystallinity and orientation, and when the spinning speed is slow, a yarn with low crystallinity and low orientation is formed. The beverage extraction container formed using a nonwoven fabric with suitable crystallinity and orientation does not break (the bag will not break during molding), and the content retention is excellent.

[0143] Generally, when short-fiber nonwoven fabrics are formed, the bonding between the filaments is lost, and the filaments float from the surface of the beverage extraction container, which may increase fuzz or fiber shedding. As the beverage extraction container according to the embodiment of the present application, long-fiber nonwoven fabrics are preferred.

[0144] [Morphology of long fibers]

[0145] The shape of the long fiber nonwoven fabric constituting the beverage extraction container according to the embodiment of the present application may be, for example, a layer of a multi-layer laminated nonwoven fabric such as SS, SMS, SMMS, SMSM, etc. It should be noted that S refers to a long fiber nonwoven fabric of a spunbond method, and M refers to an ultrafine nonwoven fabric of a meltblown method. When a multi-layer laminated nonwoven fabric such as SMS, SMMS, SMSM, etc. is used, a beverage extraction container having reduced fiber dispersion unevenness, excellent content retention, and excellent powder leakage can be obtained.

[0146] [Nonwoven fabric lamination method]

[0147] The nonwoven fabric constituting the beverage extraction container of the embodiment of the present application is laminated by 1 layer, 2 layers, 3 layers or more, for example, at least 1 layer among the multiple layers uses a low melting point resin, or uses sheath-core fibers with a melting point difference, thereby imparting and improving the adhesion of the fibers, thereby reducing the generation of surface fuzz in the beverage extraction container and improving the sealing performance with the cover.

[0148] [Fiber shape]

[0149] There is no particular limitation on the shape of the nonwoven fabric fibers constituting the extraction container of the present application. A circular, flat, C-shaped, Y-shaped, V-shaped or other irregular cross-section may be used, preferably a circular cross-section. The structure may further be an island-in-the-sea structure, a core-sheath structure, or a spliced ​​structure.

[0150] [Embossed or not]

[0151] The nonwoven fabric constituting the extraction container for extraction according to the embodiment of the present application may be embossed, but point bonding may also be performed on the surface of the fiber of the nonwoven fabric. There is no particular limitation on the method of point bonding, but preferably a method using a pair of embossing rollers having a concave-convex pattern on at least one surface, a method using a pair of smooth rollers having a flat surface, and the like are listed. In addition, needle punching, hydroentanglement, felt roll calendering, and the like may also be performed. Point bonding refers to a state where the heat bonding is kept at a light level, and the point bonding on the fiber surface forms the main body. Even if an embossed pattern is added by preheating and bonding, the heat bonding suppressed on the surface in the second stage will slightly shrink around the embossed pattern, and the embossed pattern will fall off or weaken, while the nonwoven fabric as a whole will have an unevenly reduced weight per unit area.

[0152] The ratio of the pressed area by embossing and point bonding is not particularly limited, but is preferably 3 to 50%, more preferably 5 to 40%, relative to the entire area of ​​the nonwoven fabric. The pressed area ratio can be measured using a microscope on the surface of the nonwoven fabric constituting the beverage extraction container.

[0153] [General molding method]

[0154] The beverage extraction container of the embodiment of the present application can be obtained by three-dimensionally molding the nonwoven fabric formed by the biodegradable resin. As the molding method, for example, vacuum molding, pressure molding, compression molding, etc. can be used. From the viewpoint of being not easily affected by the air permeability of the nonwoven fabric, compression molding is preferably used. As a molding mold, it can be appropriately selected according to the purpose, and a normal temperature or hot mold of a mold such as a metal, wooden, plastic, etc. concave-convex mold, a convex mold, a concave mold, etc. can be used, but in order to improve the followability with the mold and obtain a nonwoven molded body with no broken bags and good shape, a hot mold is preferably used.

[0155] [Explanation of molding and preheating taking into account polymer characteristics]

[0156] From the perspective of the resin properties of polylactic acid, if it is considered that compared with polyester resin, polyester has a high melting point, a large difference between the melting point and the glass transition temperature, and a fast crystallization rate, so the mold temperature during molding can be increased to obtain a molded body, while polylactic acid has a low melting point, a small difference between the melting point and the glass transition temperature, and a slow crystallization rate, so it is difficult to provide sufficient heat to the non-woven fabric for molding, and it may not be possible to increase the molding temperature. Therefore, the beverage extraction container of the embodiment of the present application is preferably preheated to a non-woven fabric before molding to a temperature above the glass transition temperature and below the melting point during the molding process. By preheating the non-woven fabric, the followability of the non-woven fabric to the mold is improved, and a non-woven fabric molded body with no broken bags, less uneven stretching, and good shape can be obtained.

[0157] It should be noted that the general resin properties of polylactic acid and polyester are as follows. In order of polylactic acid and polyester, melting point: 170°C, 260°C, recrystallization temperature: 70°C, 120°C, glass transition temperature 55-60°C, 70-80°C, specific heat: 1.38 J / g·K, 1.00-1.15 J / g·K, thermal conductivity 0.13 W / m·K, 0.2-0.33 W / m·K, semi-crystallization time: 500-900 seconds, 50-100 seconds.

[0158] As a method for heating or preheating the nonwoven fabric, a method of heating the nonwoven fabric using a heating furnace, infrared heater, hot air heater, heat transfer wire heater, or the like using infrared rays, hot air, electric heating wire, or the like may be used.

[0159] [Temperature of nonwoven fabric before molding]

[0160] The temperature of the nonwoven fabric before molding is preferably 55°C to 160°C, more preferably 60°C to 150°C, and further preferably 75°C to 140°C. If the temperature of the nonwoven fabric before molding is within the range, the desired container shape can be obtained. If the temperature of the nonwoven fabric before molding is too high, heat shrinkage occurs during container manufacturing, and the shape of the obtained beverage extraction container is deformed or the thickness is uneven, resulting in uneven stretching, etc. As a beverage extraction container, the shape retention, extraction, and content retention may be insufficient. If the temperature of the nonwoven fabric before molding is too low, the bag will break during molding, and the container shape may not be obtained.

[0161] [Mold temperature during molding]

[0162] The temperature of the molding die can be appropriately selected as long as the nonwoven fabric does not break or stick to the molding die during molding, and is preferably 30 to 160°C, more preferably 80 to 150°C, and further preferably 100 to 140°C.

[0163] The temperature of the nonwoven fabric before molding and the temperature of the molding die are preferably selected in consideration of the balance between the two. The smaller the difference between the temperature of the nonwoven fabric before molding and the temperature of the molding die, the less uneven stretching of the nonwoven fabric can be, which is preferred from the viewpoint of the shape retention, extraction performance, and content retention performance of the obtained beverage extraction container.

[0164] [Combination of preheating and mold assembly]

[0165] The fabric temperature and mold temperature during the molding process can be appropriately selected, but in order to obtain a beverage extraction container with a good shape at room temperature, it is preferred to perform thermoforming using a concave-convex mold, preheat the nonwoven fabric before thermoforming, and improve the thermal conductivity of the nonwoven fabric. This can suppress shrinkage when the mold is removed.

[0166] [Heat setting, cooling]

[0167] In order to obtain a container with a good shape, the beverage extraction container of the embodiment of the present application can use the following method: blowing hot air during molding, still contacting the hot mold for a certain period of time after molding, etc., setting sufficient heat setting time, disassembling from the mold after sufficient cooling, and further contacting the hot mold, cooling mold, etc. after thermoforming. As the time for heat setting, it can be appropriately selected in consideration of productivity, but it is preferably more than 0.01 seconds, more preferably more than 0.2 seconds, 0.2 seconds to 300 seconds. By extending the heat setting time, the shrinkage after molding and the shrinkage during boiling water immersion can be suppressed. The cooling after molding can be implemented by blowing cold air after molding, using a cooled mold, a normal temperature mold, etc. It is effective to reduce the non-woven fabric after molding to below the glass transition temperature of the raw material. Thus, the shrinkage just after molding can be suppressed, and a beautifully shaped molded body can be obtained after molding.

[0168] [Container shape]

[0169] The shape of the beverage extraction container of the present application embodiment is not particularly limited if it is a container shape, for example, preferably a shape with a bent bottom, a cylindrical shape, a truncated cone shape, a dome shape, a hemispherical shape, a bowl shape, etc. They can be obtained by forming the shape of the mold used during molding into a shape with a bent bottom, a cylindrical shape, a truncated cone shape, a dome shape, a hemispherical shape, a bowl shape, etc. The nonwoven fabric molded body that becomes the beverage extraction container can be enclosed in or not enclosed in a resin container for use. When not enclosed in a resin container, the container volume will not be large, and it is also excellent from the viewpoint of handleability and manufacturing cost.

[0170] [Forming Index]

[0171] The degree of molding of the nonwoven fabric of the beverage extraction container according to the embodiment of the present application is represented by a molding index. The molding index refers to a value obtained by dividing the surface area of ​​the molded body by the area of ​​the planar nonwoven fabric used in the molded body before molding (the opening area in the case of a container shape) and defined by the following formula (1):

[0172] Forming index = (surface area of ​​the molded body cm 2 ) / (area of ​​nonwoven fabric before molding cm 2 ).

[0173] The molding index of the molded body composed of the nonwoven fabric of the beverage extraction container according to the embodiment of the present application is preferably 1.1 or more, more preferably 1.1 to 20, further preferably 1.5 to 10, further more preferably 2.0 to 6, and most preferably 2.5 to 6.0. A large molding index indicates that the nonwoven fabric has a large elongation. On the other hand, a small molding index indicates that the elongation of the nonwoven fabric is small. When the molding index is not too large, the bag can be molded without breaking, and the content retention of the obtained molded body is good. When the molding index is not too small, the container can have an appropriate size when the content is filled.

[0174] [Bonding with other materials]

[0175] The beverage extraction container according to the embodiment of the present application does not deny the combination with unstretched paper or nonwoven fabric. However, in order to produce the container shape, steps such as bonding and adhesion are added, which may cause difficulties in production.

[0176] [Explanation of common extraction methods]

[0177] When using a beverage extraction container and an extractor (e.g., single-serve method) for extraction, hot water is poured into the beverage extraction container filled with the extract installed in the device. The beverage extraction container needs to have thermal stability and stability against stress changes caused by swelling of the extract.

[0178] [Shrinkage during extraction, TMA shrinkage of molded body]

[0179] The maximum value of the dimensional change rate in the MD direction when a load of 0.05 N / 2 mm is applied to the nonwoven fabric formed body sheet constituting the container by thermomechanical analysis (TMA) at 30 to 100° C. is preferably 4% or less, more preferably 3% or less. If the maximum value of the dimensional change rate is within the range, during beverage extraction, due to the stress applied by the expansion of the extract during heat and extraction, the fiber elongation or breakage or the intersection between the fibers is less likely to fall off or shift, so the beverage extraction container is not easy to expand, will not contact the needle of the extractor, and the nonwoven fabric is not easy to break. The dimensional change rate can be measured as in the examples.

[0180] In the beverage extraction container according to the embodiment of the present application, the MD direction refers to a direction in which the number of fibers arranged in the same direction is greater, and is a mechanical flow direction in the production of nonwoven fabrics.

[0181] [Capacity change when immersed in boiling water]

[0182] The capacity change of the extraction container of the embodiment of the present application when immersed in boiling water is preferably 20 to 90%, more preferably 30 to 85%, further preferably 30 to 80%, and most preferably 45 to 75%. If the capacity change is within the range, a balance between the dimensional changes of the extract and the beverage extraction container can be achieved during beverage extraction, and the non-woven fabric molded body can be used without bag breakage caused by insufficient strength and elongation of the non-woven fabric itself, or contact with extraction machine parts (such as a needle provided at the lower part of the beverage extraction container) to cause bag breakage. In the method of extracting a beverage by injecting hot water into a container using a beverage extraction device, such as a single-serve method, when using a beverage extraction container, it is preferred that the heat shrinkage is small from the viewpoint of shape stability and preventing the cover from peeling off.

[0183] On the other hand, the technology of the present application achieves a balance between the expansion of extracts such as black tea, green tea, coffee powder, medicine, Chinese medicine, etc. caused by the injection of hot water and the dimensional change of the beverage extraction container, thereby obtaining a beverage extraction container with excellent stability during extraction.

[0184] [Birefringence]

[0185] The birefringence of the nonwoven fabric molded body constituting the extraction container of the embodiment of the present application is preferably 0.010 or more, more preferably 0.012 to 0.050, and further preferably 0.012 to 0.030. When the birefringence is not too high, the fibers can be molded without excessive orientation during molding, forming a state in which the bonding between the fibers is properly maintained, and the fibers can be inhibited from floating on the surface of the extraction container. When the birefringence is not too low, the orientation is not excessively reduced, the nonwoven fabric is less attached to the molding mold during molding, and the surface properties of the resulting container become good. Furthermore, if the birefringence is within the range, the shape retention of the extraction container during beverage extraction in a hot environment can be improved. If the birefringence is too high, the adhesion between the fibers deteriorates, and fuzz is easily generated on the surface of the extraction container.

[0186] [Crystallinity]

[0187] The crystallinity of the nonwoven fabric molded body constituting the extraction container for extraction according to the embodiment of the present application is preferably 30 to 70%, more preferably 30 to 60%, and further preferably 40 to 50%. When the crystallinity is within the range, the shape of the beverage extraction container will not be deformed in a hot environment, and the shape retention of the extraction container during beverage extraction in a hot environment can be improved.

[0188] [Converted weight per unit area of ​​nonwoven fabric constituting beverage extraction container]

[0189] The total weight per unit area of ​​the nonwoven fabric molded body constituting the extraction container for extraction according to the embodiment of the present application is 20 to 350 g / m 2 , preferably 20 to 300 g / m 2 , more preferably 30 to 300 g / m 2 , most preferably 50 to 250 g / m 2 If the total unit area weight is 20g / m 2 If the strength of the beverage extraction container is above 350 g / m 2 The following process can be performed without placing a heavy burden on the molding equipment when obtaining the beverage extraction container. It should be noted that the total unit area weight of the nonwoven fabric used in the beverage extraction container can be calculated from the area (m2) of the nonwoven fabric before molding. 2 ), the weight (g) of the nonwoven fabric used in beverage containers is calculated.

[0190] [Average fiber diameter of nonwoven fabric constituting beverage extraction container]

[0191] The average fiber diameter of the nonwoven fabric molded body constituting the extraction container for extraction according to the embodiment of the present application is preferably 8 to 50 μm, more preferably 10 to 40 μm, and further preferably 15 to 30 μm. When the average fiber diameter is not too small, the container can hold the contents (good powder leakage), and when the average fiber diameter is not too large, the liquid flow rate is not too slow.

[0192] [Weight per unit area of ​​nonwoven fabric constituting beverage extraction container]

[0193] The nonwoven fabric molded body constituting the extraction container according to the embodiment of the present application preferably has a weight per unit area of ​​12 to 200 g / m 2 , more preferably 18 to 100 g / m 2 , more preferably 30 to 80 g / m 2 , most preferably 30 to 60 g / m 2 If the weight per unit area of ​​the nonwoven fabric is within the range, the nonwoven fabric can be used as a container to retain the contents (good powder leakage resistance) and the liquid flow rate will not be too slow.

[0194] [Powder leakage]

[0195] When using the extraction container for extraction of the embodiment of the present application and using an extractor to extract black tea, green tea, coffee powder, medicine, Chinese medicine, etc., the amount of powder contained in the extract can be formed into the desired amount of powder by appropriately selecting the fiber diameter, total unit weight, unit weight, molding conditions, etc. of the non-woven fabric molding. The amount of powder can be less than 0.25g, and further less than 0.20g. In the case of reducing the amount of tea leaves and powder extracted in the beverage, appropriately selecting molding conditions such as reducing the fiber diameter, reducing the total unit weight, reducing the unit weight, reducing the temperature unevenness in the non-woven fabric during molding, and eliminating the molding unevenness can be sufficient. On the other hand, in the case of residual tea leaves and other extracts in the beverage, appropriately selecting molding conditions such as increasing the fiber diameter, increasing the total unit weight, increasing the unit weight, and increasing the temperature unevenness in the non-woven fabric during molding can be sufficient.

[0196] [Capacity changes before and after extraction]

[0197] The capacity change of the extraction container before and after extraction of the embodiment of the present application can be -30 to 30%, -20 to 20%, or -10 to 10%. If the capacity change before and after extraction is within the range, the balance of the size change of the extract and the beverage extraction container can be achieved during beverage extraction, and the non-woven fabric molded body can be used without bag breakage caused by insufficient strength and elongation of the non-woven fabric itself, or contact with extraction machine parts (such as a needle set at the lower part of the beverage extraction container).

[0198] [For surface fuzzing]

[0199] The number of raised fibers of the nonwoven fabric constituting the extraction container for extraction according to the embodiment of the present application is preferably 10 or less, more preferably 0 to 9, and still more preferably 0 to 3. When the number of raised fibers is within the range, the appearance of the product is good, and there is no deterioration in the surface properties due to friction between the beverage extraction containers due to vibration during transportation, and there is no concave-convexity of the container installation part of the extraction machine caused by fiber jamming, and the handling is excellent.

[0200] [build]

[0201] After the extraction container for extraction of the embodiment of the present application is filled with the contents, it can be covered with a cover such as a film or a nonwoven fabric. There is no particular limitation on the method of sealing the cover, and methods such as coating an adhesive or a thermoplastic resin, coating an adhesive on the cover, adding or mixing a thermoplastic resin to the cover, or using a nonwoven fabric whose sheath has a lower melting point than the core resin in the case of a nonwoven fabric can be used. When the cover is used in an extractor, it can be installed to the extent that the contents do not spill out when the cover is peeled off.

[0202] Example

[0203] The present invention is specifically described below by way of examples.

[0204] First, the measuring method, the evaluating method, etc. are described.

[0205] (Evaluation of properties of nonwoven fabrics)

[0206] (1) Average fiber diameter (μm)

[0207] 5 cm from both ends of a sample such as a fiber web or nonwoven fabric is removed, and an appropriate number of fibers are collected from each 10 cm wide area of ​​the fabric. The fiber diameters are measured at 30 points using a microscope, and the average of the measured values ​​is calculated.

[0208] (2) Weight per unit area (g / m 2 )

[0209] According to JIS L-1913, the total area is 1500cm 2 The sample is cut into pieces (for example, 3 pieces of 20 cm width x 25 cm length) and converted into a unit mass to obtain the value.

[0210] (3) Birefringence (Δn)

[0211] The distribution of the average refractive index observed from the side of the fiber can be measured by the interference fringe method using BX53 manufactured by OLYMPUS. This method can be applied to fibers with a circular cross section. The refractive index of the fiber is characterized by the refractive index n|| for polarized light with an electric field vector parallel to the fiber axis and the refractive index n⊥ for polarized light with an electric field vector perpendicular to the fiber axis, and the birefringence is represented by Δn=(n||-n⊥).

[0212] If polarized light is irradiated on a fiber, it is divided into two polarized lights that vibrate at right angles to each other. The refractive index of the fiber is different depending on the direction of the axis, so the distances traveled by the two lights are different. This is the delay, represented by R. If the diameter of the fiber cross section is d0, there is a relationship between the birefringence and the following formula: R = d0(n||-n⊥) = d0Δn.

[0213] Using an optically flat slide and a cover glass, the fiber collected from the sample is immersed in an inactive sealant for the fiber. In the measurement section, the fibers are not overlapped with each other, and the fiber axis is perpendicular to the optical axis of the polarizing microscope and the interference fringes. The interference fringes pattern is measured to find the delay, the birefringence of the fiber is measured, and the average value of 10 points is measured.

[0214] (4) Elongation at 120°C (%)

[0215] Remove 5 cm from both ends of the sample, cut a 3 cm wide and 10 cm long sample, and use a tensile tester with a clamp interval of 2 cm, a tensile speed of 200 mm / min, and a temperature of 120°C to measure 5 points in the longitudinal direction, and calculate the average value. It should be noted that after the sample is placed in the constant temperature chamber for 1 minute, the chamber temperature is confirmed to be 120°C and the measurement is started.

[0216] (5) Value obtained by dividing the warp tear strength by the unit area weight (-)

[0217] Remove 5 cm from both ends of the sample, cut out three samples with a width of 10 cm and a length of 6.5 cm, and measure the warp tear strength (N) using an Elmendorf tear tester to find the average value, which is then divided by the weight per unit area to calculate.

[0218] (6) Dimensional change rate in MD direction obtained by mechanical thermal analysis (%)

[0219] After removing 5 cm from both ends of the sample, a sample with a width of 2 mm and a length of 25 mm with a unit area weight of ±10% obtained in (2) was cut off. The sample was measured using TMAQ400 manufactured by TA Instruments, with a film / fiber clamping device used for the upper clamping device and an aluminum ball manufactured by TA Instruments used for the lower clamping device, at a heating rate of 10°C / min and a gripping length of 15 mm until the initial load was 0.005 N and the temperature was between 30°C and 160°C. The dimensional change rate (%) was calculated from dimensional change (μm) / {grip length (mm)×1000}×100 at 80°C to 140°C. The measurement was performed with N=3 and the average value was calculated.

[0220] (7) Evaluation of temperature dependence of storage modulus

[0221] A sample with a width of 5 mm and a length of 25 mm was cut and measured using DMA2980 manufactured by TA Instruments Japan and a film / fiber clamp at a heating rate of 3°C / min and a grasping length of 10 mm until an initial load of 0.010 N, a frequency of 1 Hz, a strain of 1%, and a temperature of 30°C to 150°C.

[0222] It should be noted that the rate of change of the storage modulus with respect to temperature can be calculated by dividing the change of the storage modulus in the temperature dependency test of the dynamic viscoelasticity by the value of the temperature change using the following formula:

[0223] Temperature dependence test of dynamic viscoelasticity = -Δ storage modulus / Δ temperature.

[0224] (8) Raising grade (grade)

[0225] A 25mm×300mm test piece was collected in the MD direction, and the friction piece load was 250g using the Japan Society for the Promotion of Science fastness tester. The same cloth was used on the friction piece side, and the test was performed 50 times. The following evaluation criteria were used for the test. It should be noted that the smaller grade was used for both the front and back sides of the test sample.

[0226] Grade 5.0: No fuzzing.

[0227] Grade 4.0: The hair is fuzzy to the extent that 1 to 2 fibers are present or small pilling begins to appear in one place.

[0228] Level 3.5: The fiber is 3 to 5 or small pilling begins to appear in several places.

[0229] Level 3.0: Clear hair balls begin to appear, or multiple small hair balls are found.

[0230] Level 2.5: Large and clear hair balls are found, and fibers begin to float in many places.

[0231] Grade 2.0: Fibers are greatly peeled off to the extent that the test piece becomes thin.

[0232] Grade 1.0: Fibers are stripped off to the extent that the test piece is damaged.

[0233] (9) R / Ave value of the weight distribution per unit area of ​​2.5 cm square of the biaxially stretched sheet

[0234] The sample was cut into 12.5 cm squares and stretched to 20 cm in both MD / CD directions using a biaxial stretching device with a clamp interval of 8 cm, a stretching speed of 200 mm / min, and a temperature of 120°C to prepare a stretched sheet. The stretching ratio at this time was 2.5 times the length and 6.25 times the area ratio in each MD / CD direction. It should be noted that the sample was placed in a constant temperature chamber, and after 1 minute, the chamber temperature was confirmed to be 120°C, and the stretching was started.

[0235] A 10 cm square was drawn in the center of the produced stretched sheet, and a 2.5 cm square x 16 square grid was drawn in the middle. 16 pieces of the drawn 2.5 cm square grid were cut out and the weight was measured.

[0236] The value of R / Ave is a value defined by the following formula:

[0237] R (maximum value - minimum value of the weight of 16 pieces) / Ave (average value of the weight of 16 pieces).

[0238] (10) Formability

[0239] The biodegradable nonwoven fabric was installed in a molding machine, preheated at a hot air temperature of 100°C for 1 minute to make the nonwoven fabric temperature 60°C, and a cylindrical molding die (diameter 4.4 cm, height 1.3 cm and 3.2 cm) at 120°C was used for 2 seconds to perform press molding, and the appearance of the molded body at this time was observed and evaluated according to the following evaluation criteria. It should be noted that the molding index is a value defined by the following formula, which is obtained by dividing the surface area of ​​the molded body by the area of ​​the planar nonwoven fabric used in the molded body before molding (the opening area in the case of a container shape):

[0240] Forming index = (surface area of ​​the molded body cm 2 ) / (area of ​​nonwoven fabric before molding cm 2 )

[0241] ○: No cracks, good moldability, a molded body with a molding index of 1.9 or more was obtained in a mold with a height of 1.3 cm, and a molded body with a molding index of 3.4 or more was obtained in a mold with a height of 3.2 cm.

[0242] △: Although there is no cracking, there are problems such as unevenness on the surface of the molded article, uneven stretching, and significant fuzz.

[0243] ×: There are problems such as cracking, poor moldability, failure to obtain a molded body with a molding index of 1.9 or more in a mold with a height of 1.3 cm, and failure to obtain a molded body with a molding index of 3.4 or more in a mold with a height of 3.2 cm.

[0244] (11) Composting test

[0245] The state of the sample pieces after 4 weeks was observed visually using a stacking tester in a constant environment of 60°C and judged according to the following evaluation criteria:

[0246] ○: The sample piece was reduced in size.

[0247] ×: No change in the appearance of the sample was observed.

[0248] (12) Formability (uniform formability)

[0249] A long-fiber nonwoven fabric was installed in a molding machine having 10 rows of molding dies in the width direction, and the nonwoven fabric temperature was set to 100° C. by hot air. A cylindrical molding die (diameter 4.4 cm, height 3.2 cm) at 120° C. was used for 2 seconds for press molding, and 11 g of model particles with a particle size of 100 μm were filled. A PLA sheet was used as a cover and heat-sealed to produce 100 moldings.

[0250] The bottom of the obtained molded body was cut off by 1 cm each, and the weight was measured.

[0251] The value of R / Ave is a value defined by the following formula:

[0252] R (maximum value - minimum value of the weight of 100 pieces) / Ave (average value of the weight of 100 pieces).

[0253] (Evaluation of properties of molded product)

[0254] (1) Average fiber diameter (μm)

[0255] An appropriate number of fibers were collected from the side surface (the portion where the nonwoven fabric was stretched) of the nonwoven fabric molded body used in the beverage extraction container, and the fiber diameters were measured at 30 points under a microscope, and the average value of the measured values ​​was calculated.

[0256] (2) Conversion weight per unit area of ​​nonwoven fabric (g / m 2 )

[0257] The weight (g) of the nonwoven fabric molded body used in the beverage extraction container, the area of ​​the flat nonwoven fabric used in the nonwoven fabric molded body before molding (= the opening area in the case of the container shape) (m 2 ), convert it into unit mass to find out.

[0258] Nonwoven fabric conversion unit area weight (g / m 2 ) = weight of nonwoven fabric (g) / area of ​​flat nonwoven fabric before molding used in the molded article (m 2 )

[0259] (3) Weight per unit area of ​​the molded product (g / m 2 )

[0260] The weight (g) and area (m2) of the nonwoven fabric collected from the nonwoven fabric molded body used in the beverage extraction container were 2 When the nonwoven fabric has curvature, the nonwoven fabric is cut into small widths, smoothed, and the area of ​​the nonwoven fabric is measured using a microscope.

[0261] Weight per unit area of ​​the molded body (g / m 2 ) = weight of nonwoven fabric (g) / area before molding (m 2 )

[0262] (4) Birefringence (Δn)

[0263] The birefringence of the nonwoven fabric was similarly measured by the interference fringe method using BX53 manufactured by OLYMPUS Co., Ltd. The test piece was collected from the side surface (the point where the elongation was high) of the nonwoven fabric molded body.

[0264] (5) Crystallinity (%)

[0265] The crystallinity was measured using a differential scanning calorimeter DSC6000 manufactured by PerkinElmer by the same method as that for the nonwoven fabric.

[0266] (6) Dimensional change rate in MD direction

[0267] A sample with a width of 2 mm and a length of 25 mm was cut out from the side of the nonwoven fabric molded body used in the beverage extraction container (= the part with large elongation change in the container) in the MD direction of the nonwoven fabric, and a TMAQ400 (thermomechanical analysis (TMA)) manufactured by TA Instruments was used. The upper clamping device used a film / fiber clamping device and the lower clamping device used an aluminum ball manufactured by TA Instruments. The temperature was increased at a rate of 10°C / min and a grip length of 15 mm until the initial load was 0.05N and 30°C to 100°C. The dimensional change rate (%) was calculated by dimensional change (μm) / {grip length (mm)×1000}×100 at 30°C to 100°C, and the maximum value at 30°C to 100°C was calculated. The measurement was performed with N=5, and the average value was calculated. The positive sign of the dimensional change rate indicates elongation.

[0268] (7) Capacity change during immersion in boiling water

[0269] After the beverage extraction container (without content) is immersed in boiling water for 1 minute, it is air-dried, and the capacity change before and after the immersion in boiling water is calculated, and the average value of N = 5 is calculated. The capacity of the container is measured by the weight of the reference powder that can be filled in the container (the powder passing through the 150μm mesh by the sieve test is less than 0.05%).

[0270] Capacity change (%) = (reference powder filling amount before boiling water immersion (g) - reference powder filling amount after boiling water immersion) × 100 / reference powder filling amount before boiling water immersion (g)

[0271] (8) Surface fuzzing

[0272] The number of raised hairs on the surface of the beverage extraction container was measured visually, and the average value of N=10 was calculated.

[0273] (9) Extractability: Powder leakage

[0274] A beverage extraction container filled with coffee powder (the powder passing through a 150 μm mesh by a sieve test is 0.05% or less, and the filling amount is 11 g (the maximum filling amount is used when the container is small and cannot be added)) is set in a Keurig extractor. The coffee extracted with 170 ml of hot water is filtered using filter paper No. 2 manufactured by Advantec Co., Ltd., and dried for 6 hours in a dryer, and the amount of powder remaining on the filter paper is measured. The measurement is performed with N=10, and the average value is taken as the powder leakage amount.

[0275] (10) Extractability: Change in volume after extraction

[0276] For the beverage extraction container after extraction in (9), the volume change before and after extraction was calculated, and the average value of N = 5 was calculated. The volume of the container was measured by the weight of the reference powder (0.05% or less of the powder passed through a 150 μm mesh by a sieve test) that could be filled in the container.

[0277] Capacity change during extraction (%) = (reference powder filling amount before extraction (g) - reference powder filling amount after extraction) × 100 / reference powder filling amount before extraction (g)

[0278] (11) Extractability: Sealing of the lid

[0279] A beverage extractor container filled with reference powder (powder passing through a 150 μm mesh by a sieve test was 0.05% or less, and the filling amount was 11 g) was immersed in boiling water for 1 minute, and the presence or absence of cap peeling was visually determined according to the following evaluation criteria.

[0280] ○: No peeling (good sealing)

[0281] ×: There is peeling (poor sealing)

[0282] (12) Formability

[0283] The appearance of the nonwoven fabric molded body was observed and evaluated according to the following evaluation criteria. It should be noted that the molding index is a value obtained by dividing the surface area of ​​the molded body by the area of ​​the planar nonwoven fabric before molding used in the molded body (the opening area in the case of a container shape) using the following formula:

[0284] Forming index = (surface area of ​​the molded body cm 2 ) / (area of ​​nonwoven fabric before molding cm 2 ).

[0285] 4: Molding index is above 2.0 and there is no cracking.

[0286] 3: The molding index is 2.0 or more, and there is no cracking, but the surface of the molded product is uneven, there is uneven stretching, and there is noticeable fuzz.

[0287] 2: No cracking but the forming index is less than 2.0.

[0288] 1: There is a rupture.

[0289] (13) Biodegradability (composting test)

[0290] The state of the sample pieces after 4 weeks was observed visually using a stacking tester in a constant environment of 60°C and judged according to the following evaluation criteria:

[0291] ○: The sample piece was reduced in size.

[0292] ×: No change in the appearance of the sample was observed.

[0293] The following describes the contents of the evaluation of the properties of the nonwoven fabric.

[0294] [Example 1]

[0295] 10 wt% of polybutylene succinate (melting point 110°C) is added to polylactic acid having an MFR value of 44 g / 10 min at a temperature of 230°C, and the mixture is melted and kneaded using a single-screw extruder. The filaments are extruded onto a moving collecting surface using a spunbond method with an ejection amount of 0.9 g / min·Hole, a spinning temperature of 220°C, and a spinning speed of 1011 m / min to produce a biodegradable long fiber web (circular cross section).

[0296] Then, a pair of embossing rolls with a concave-convex pattern on the surface were used for preliminary pressing. The pressing area ratio of the embossing rolls used was 14%, and the preliminary pressing was performed at a roller line pressure of 300 N / cm at an upper and lower roller temperature of 45°C.

[0297] Next, the pre-pressed web was stored at 30°C for 72 hours and then heat-treated by felt roll calendering (roller diameter 2500 mm, temperature 135°C, processing speed 10 m / min) to obtain a biodegradable long fiber nonwoven fabric (weight per unit area 250 g / m 2 , fiber diameter 30μm).

[0298] The biodegradable long-fiber nonwoven fabric was installed in a molding machine, preheated at a hot air temperature of 100° C., and press-molded for 2 seconds using a 120° C. cylindrical molding die (diameter 4.4 cm, height 1.3 cm and 3.2 cm) to produce a molded body.

[0299] [Examples 2 and 3]

[0300] The weight per unit area of ​​the biodegradable long fiber nonwoven fabric is 90 and 25 g / m 2 , except for the above, a biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 1.

[0301] [Example 4]

[0302] The weight per unit area of ​​the biodegradable long fiber nonwoven fabric is 15 g / m 2 A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 1 except that the fiber diameter was 12 μm and the ejection rate was 0.7 g / min·Hole.

[0303] [Example 5]

[0304] The weight per unit area of ​​the biodegradable long fiber nonwoven fabric is 150 g / m2 A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 4 except that the ejection rate was 0.7 g / min·Hole.

[0305] [Example 6]

[0306] The calendering temperature of the felt roll is 125°C and the weight per unit area of ​​the biodegradable long fiber nonwoven fabric is 310 g / m 2 A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 1 except that the fiber diameter was 38 μm.

[0307] [Examples 7 and 8]

[0308] A biodegradable long-fiber nonwoven fabric and a molded product were produced in the same manner as in Example 2 except that the amount of polybutylene succinate added was changed to 5% by weight and 25% by weight.

[0309] [Example 9]

[0310] The addition amount of polybutylene succinate was 35 wt % and the weight per unit area of ​​the biodegradable long-fiber nonwoven fabric was 150 g / m 2 , except for the above, a biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 2.

[0311] [Example 10]

[0312] The weight per unit area of ​​the biodegradable long fiber nonwoven fabric is 150 g / m 2 , except for the above, a biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 2.

[0313] [Example 11]

[0314] A biodegradable long-fiber nonwoven fabric and a molded product were produced in the same manner as in Example 10 except that the spinning speed was 805 m / min and the fiber diameter was 34 μm.

[0315] [Example 12]

[0316] A biodegradable long-fiber nonwoven fabric and a molded product were produced in the same manner as in Example 10 except that the spinning speed was 1160 m / min and the fiber diameter was 28 μm.

[0317] [Example 13]

[0318] A biodegradable long-fiber nonwoven fabric and a molded product were produced in the same manner as in Example 10 except that the spinning speed was changed to 2519 m / min.

[0319] [Example 14]

[0320] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the spinning temperature was set to 210°C, the spinning speed was set to 1345 m / min, and the fiber was stored at 30°C for 1 hour and then heat-treated by calendering with a felt roll to adjust the fiber diameter to 26 μm.

[0321] [Example 15]

[0322] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the calendering temperature of the felt roll was set to 90°C.

[0323] [Example 16]

[0324] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the calendering temperature of the felt roll was 160°C.

[0325] [Example 17]

[0326] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the heat treatment was performed by felt roll calendering after storage at 50°C for 720 hours.

[0327] [Example 18]

[0328] Make the unit area weight 15g / m 2 , except for the above, a long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 1.

[0329] [Example 19]

[0330] A biodegradable long-fiber nonwoven fabric and a molded product were produced in the same manner as in Example 2 except that the amount of polybutylene succinate added was 2.5% by weight.

[0331] [Example 20]

[0332] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the calendering temperature of the felt roll was set to 110°C.

[0333] [Example 21]

[0334] Make the unit area weight 50g / m 2 , except for the above, a biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 20.

[0335] [Comparative Example 1]

[0336] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10, except that the heat treatment was not performed by felt roll calendering. The dimensional change rate was large and the moldability was poor.

[0337] [Comparative Example 2]

[0338] A biodegradable long-fiber nonwoven fabric and a molded body were produced in the same manner as in Example 10 except that the fabric was heat-treated by felt roll calendering after storage at 30°C for 1 hour. The dimensional change rate was large and the moldability was poor.

[0339] [Comparative Example 3]

[0340] A known spunbond method was used to spin polylactic acid having an MFR value of 44 g / 10 minutes at a temperature of 230°C at a discharge rate of 0.9 g / min·Hole and a spinning temperature of 220°C to obtain a polylactic acid-based fiber having a weight per unit area of ​​135 g / m 2 , thickness 0.49mm (measured by the method specified in JIS L-1913, load 100g / cm 2 A nonwoven fabric (Tm: 172°C, Tc: 83°C, Tg: 63°C) having a thickness of 28 μm, a fiber diameter of 28 μm, and a pressure-bonded area ratio of 18% was produced in the same manner as in Example 1. The dimensional change rate was large and the moldability was poor.

[0341] [Comparative Example 4]

[0342] A known spunbond method was used to spin polylactic acid having an MFR value of 44 g / 10 minutes at a temperature of 230°C at a discharge rate of 0.9 g / min·Hole and a spinning temperature of 220°C to obtain a polylactic acid-based fiber having a weight per unit area of ​​17.3 g / m 2 , thickness 0.09mm (measured by the method specified in JIS L-1913, load 100g / cm 2 A nonwoven fabric having a thickness of 15 μm, a fiber diameter of 15 μm, and a pressure-bonded area ratio of 21% was produced in the same manner as in Example 1. The elongation was low and the moldability was poor.

[0343] [Comparative Example 5]

[0344] Polyethylene terephthalate (PET) with an MFR value of 25 g / 10 minutes at a temperature of 300°C was spunbonded to extrude filaments at a discharge rate of 0.9 g / min·Hole and a spinning temperature of 290°C onto a moving collecting surface to produce a filament with a unit area weight of 100 g / m 2 A polyethylene terephthalate fiber web (melting point 260° C., spinning speed 1716 m / min, average fiber diameter 22 μm, circular cross section).

[0345] Then, a pair of embossing rolls with concave-convex patterns on the surface were used for partial hot pressing. The embossing rolls used had a pressing area ratio of 14%, and the partial hot pressing was performed at a roller line pressure of 400 N / cm under the condition of upper and lower roller temperatures of 65°C.

[0346] Next, the partially bonded web was stored at 30°C for 1 hour and then heat treated by felt roll calendering (roller diameter 2500 mm, temperature 130°C, processing speed 15 m / min) to obtain a polyethylene terephthalate long fiber nonwoven fabric.

[0347] The biodegradable long-fiber nonwoven fabric was installed in a molding machine, preheated at a hot air temperature of 100° C., and press-molded for 2 seconds using a 120° C. cylindrical molding die (diameter 4.4 cm, height 1.3 cm and 3.2 cm) to produce a molded body.

[0348] The obtained polyethylene terephthalate nonwoven fabric was subjected to a piling treatment, but no change in appearance was observed.

[0349] [Comparative Example 6]

[0350] Make the unit area weight 70g / m 2 , except for the above, a long-fiber nonwoven fabric and a molded body were produced in the same manner as in Comparative Example 4.

[0351] [Comparative Example 7]

[0352] A long-fiber nonwoven fabric and a molded product were produced in the same manner as in Comparative Example 1 except that the spinning speed was 1455 m / min.

[0353] [Comparative Example 8]

[0354] A long-fiber nonwoven fabric and a molded body were produced in the same manner as in Comparative Example 6 except that the spinning speed was 1455 m / min.

[0355] The results of Examples 1 to 21 and Comparative Examples 1 to 8 are shown in the following Table 1 (Table 1-1, Table 1-2).

[0356] [Table 1-1]

[0357]

[0358] [Table 1-2]

[0359]

[0360] The results of the dynamic viscoelasticity measurements in Example 10 and Comparative Example 1 are as follows: Figure 3 shown.

[0361] The results of evaluating the properties of the molded product will be described below.

[0362] [Example 22]

[0363] A biodegradable nonwoven fabric was obtained by the same method as in Example 10. The obtained nonwoven fabric was installed in a molding machine, preheated to 75°C using hot air, and pressed using a cylindrical molding die (diameter 4.4 cm, height 3.2 cm) at 80°C for 2 seconds (including a heat setting time of 0.2 seconds), and cooled to below the Tg of polylactic acid using a room temperature mold to obtain a beverage extraction container (total unit area weight 150 g / m 2 , fiber diameter of the stretched part 25μm). The lid of the container is heat-sealed with a polylactic acid resin film. The results of the maximum value of the dimensional change rate in the MD direction when a load of 0.05N / 2mm is applied to the nonwoven fabric constituting the container at 30 to 100°C, the capacity change when immersed in boiling water, the powder amount, the capacity change before and after extraction, surface fuzzing, the sealing property of the lid, the shape retention during extraction, and the biodegradability test for the beverage extraction container are shown in Table 2 below.

[0364] [Examples 23, 24, 25]

[0365] A nonwoven fabric molded body was obtained in the same manner as in Example 22 except that the mold temperature during molding was changed to 105, 125, and 145°C, respectively.

[0366] [Example 26]

[0367] A nonwoven fabric molded body and a beverage extraction container were obtained in the same manner as in Example 23 except that the fabric temperature of the nonwoven fabric during molding was 105°C.

[0368] [Example 27]

[0369] A nonwoven fabric molded body and a beverage extraction container were obtained in the same manner as in Example 24 except that the fabric temperature of the nonwoven fabric during molding was 125°C.

[0370] [Example 28]

[0371] A nonwoven fabric molded body and a beverage extraction container were obtained in the same manner as in Example 22 except that the mold temperature during molding was 90°C and the fabric temperature of the nonwoven fabric was 150°C.

[0372] [Examples 29 and 30]

[0373] A nonwoven fabric molded body and a beverage extraction container were obtained in the same manner as in Example 24 except that the heat setting time during molding was changed to 60 seconds or 300 seconds.

[0374] [Example 31]

[0375] A nonwoven fabric molded body and a beverage extraction container were obtained in the same manner as in Example 23 except that a room temperature mold was not used during molding.

[0376] [Example 32]

[0377] The polylactic acid long-fiber nonwoven fabric used was the same as in Example 2, and the molding method was the same as in Example 26, to obtain a nonwoven fabric molded body and a beverage extraction container.

[0378] [Example 33]

[0379] The polylactic acid long-fiber nonwoven fabric used was the same as in Example 1, and the molding method was the same as in Example 26, to obtain a nonwoven fabric molded body and a beverage extraction container.

[0380] [Example 34]

[0381] The polylactic acid long-fiber nonwoven fabric used was the same as in Example 13, and the molding method was the same as in Example 24, to obtain a nonwoven fabric molded body and a beverage extraction container.

[0382] [Example 35]

[0383] The polylactic acid long-fiber nonwoven fabric used was the same as in Example 6, and the molding method was the same as in Example 24, thereby performing thermoforming to obtain a nonwoven fabric molded body and a beverage extraction container.

[0384] [Examples 36 and 37]

[0385] A polylactic acid long-fiber nonwoven fabric was prepared by the same method as in Comparative Example 1. The mold temperatures during molding were 120°C and 140°C, respectively. A normal temperature mold was not used during molding. Apart from this, thermoforming was performed by the same method as in Example 22, thereby obtaining a nonwoven fabric molded body and a beverage extraction container.

[0386] [Example 38]

[0387] The polylactic acid fibers obtained by the known melt spinning method with a spinning speed of 1150 m / min and a fiber diameter of 30 μm were cut to obtain short fibers with a fiber length of 10 cm. The obtained short fibers were integrated by needle punching to form a short fiber nonwoven fabric (weight per unit area 150 g / m 2 ), and prepare a nonwoven fabric molding and a beverage extraction container in the same manner as in Example 23.

[0388] [Comparative Example 9]

[0389] A nonwoven fabric molded body and a beverage extraction container were produced in the same manner as in Example 22 except that the mold temperature during molding was 30° C. The bag was broken during molding and could not be used as a beverage extraction container.

[0390] [Comparative Example 10]

[0391] A nonwoven fabric molded body and a beverage extraction container were prepared by thermoforming in the same manner as in Example 24 except that the temperature of the nonwoven fabric before molding was 40° C. The bag was broken during molding and could not be used as a beverage extraction container.

[0392] [Comparative Example 11]

[0393] A nonwoven fabric was prepared in the same manner as in Example 15, and thermoformed in the same manner as in Example 22 to produce a nonwoven fabric molded body and a beverage extraction container. Oriented crystallization was difficult to proceed, and thermal stability during extraction was poor.

[0394] [Comparative Example 12]

[0395] A nonwoven fabric was prepared by the same method as in Example 3, and thermoformed by the same method as in Example 26 to produce a nonwoven fabric molded body and a beverage extraction container. The stretched portion of the beverage extraction container had a low basis weight and poor shape stability during beverage extraction.

[0396] [Comparative Example 13]

[0397] The nonwoven fabric used has a unit area weight of 500 g / m 2 , except for the above, a nonwoven fabric molded body and a beverage extraction container were prepared in the same manner as in Example 26.

[0398] [Comparative Example 14]

[0399] A PET nonwoven fabric was prepared in the same manner as in Comparative Example 5, except that the mold temperature during molding was 150° C., and a nonwoven fabric molded body and a beverage extraction container were prepared in the same manner as in Example 22. The obtained beverage extraction container was not biodegradable.

[0400] [Comparative Example 15]

[0401] A biodegradable nonwoven fabric was prepared by the same method as in Comparative Example 3, and molded by the same method as in Example 22 to produce a nonwoven fabric molded body and a beverage extraction container. The shape retention during extraction was poor.

[0402] [Comparative Example 16]

[0403] The polylactic acid fibers obtained by the known melt spinning method with a spinning speed of 1500 m / min and a fiber diameter of 25 μm were cut to obtain short fibers with a fiber length of 10 cm. The obtained short fibers were integrated by needle punching to form a short fiber nonwoven fabric (weight per unit area 150 g / m 2 ), a nonwoven fabric molded body and a beverage extraction container were prepared in the same manner as in Example 23. The container surface had a lot of fuzz and the quality was deteriorated.

[0404] The results of Examples 22 to 38 and Comparative Examples 9 to 16 are shown in Table 2 below.

[0405] [Table 2]

[0406]

[0407] Industrial Applicability

[0408] The biodegradable nonwoven fabric of the present invention has excellent formability while being biodegradable, and can be suitably used in a wide range of fields such as containers for daily materials, containers for industrial materials, vehicle interior and exterior materials, sound insulation materials, sound absorbing materials, parts transport trays, fruit and vegetable trays, food containers, seedling pods, filters, etc. In addition, the biodegradable nonwoven fabric of the present invention has high elongation and can be formed into containers of complex shapes, so it can also be suitably used in fields requiring good appearance as a container.

Claims

1. A biodegradable long-fiber nonwoven fabric for thermoforming, comprising fibers containing a polylactic acid polymer and having a unit area weight of 20 to 350 g / m 2 , the elongation in the MD direction at 120°C is 50% or more, and the dimensional change rate in the MD direction at 80°C to 140°C obtained by thermomechanical analysis is ±4% or less, and the birefringence of the long fibers constituting the nonwoven fabric sampled from the nonwoven fabric is 0.014 to 0.10, The nonwoven fabric is stored or aged before being heat-set to a fixed length.

2. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1, wherein: The elongation in the MD direction at 120°C is 100% to 400%, and the dimensional change rate in the MD direction at 80°C to 140°C obtained by thermomechanical analysis is ±2% or less.

3. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The nonwoven fabric has a storage modulus of 10 to 500 MPa in a temperature range of 90° C. to 150° C. in a temperature dependency test for dynamic viscoelasticity evaluation.

4. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The value obtained by dividing the warp tear strength of the nonwoven fabric by the unit area weight is 0.002 to 0.5 N / (g / m 2 ).

5. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The fibers containing a polylactic acid-based polymer in the nonwoven fabric further contain, in addition to the polylactic acid-based polymer, an aliphatic ester copolymer in an amount of 0.5 to 30% by weight based on the weight of the entire resin.

6. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 5, wherein: The fibers containing a polylactic acid-based polymer in the nonwoven fabric further contain, in addition to the polylactic acid-based polymer, an aliphatic ester copolymer in an amount of 0.5 to 27% by weight based on the weight of the entire resin.

7. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The nonwoven fabric has an average fiber diameter of 1 to 40 μm, and is composed of long fibers.

8. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The nonwoven fabric has a maximum loss tangent value (tan δ) of 0.5 or less in a temperature dependency test for evaluating dynamic viscoelasticity.

9. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The storage modulus of the nonwoven fabric at 10 to 70° C. in a temperature dependency test for evaluating dynamic viscoelasticity is 200 MPa or more.

10. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The R / Ave value of the 2.5 cm square unit area weight of a stretched sheet obtained by simultaneously stretching the nonwoven fabric in MD / CD directions at a temperature of 120° C. to an area ratio of 6.25 times was within 1.

0.

11. The biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, wherein: The nonwoven fabric has a unit area weight of 20 to 300 g / m 2 .

12. The method for producing a biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, comprising the step of heat-setting at a fixed length within a range of 50°C to 160°C.

13. The method for producing a biodegradable long-fiber nonwoven fabric for thermoforming according to claim 12, comprising: The step of heating and melting the polylactic acid polymer and ejecting it from a spinning nozzle to obtain a filament; The step of cooling the filament; The silk strips are deposited on a collecting surface to form a net; The mesh is pre-crimped to obtain a pre-crimped mesh; The pre-compressed mesh is subjected to the above-mentioned fixed-length heat setting process.

14. The method for producing a biodegradable long-fiber nonwoven fabric for thermoforming according to claim 12, wherein: The fixed-length heat setting treatment is at least one selected from the group consisting of hot air drying, pin chain tenter drying, hot plate, calendering, felt roll calendering and hot air processing.

15. The method for producing a biodegradable long-fiber nonwoven fabric for thermoforming according to claim 12, wherein: The fixed-length heat setting treatment is a felt roller calendering process.

16. The method for producing a biodegradable long-fiber nonwoven fabric for thermoforming according to claim 12, wherein: Prior to the fixed-length heat setting step, a storage or aging step is included.

17. A method for producing a molded article, comprising the step of integrally processing the biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2 by thermoforming.

18. The method according to claim 17, comprising the step of preheating the nonwoven fabric to 55°C to 160°C.

19. A molded product, comprising the biodegradable long-fiber nonwoven fabric for thermoforming according to claim 1 or 2, and having a molding index of 1.1 or more.

20. A formed body group, which is composed of the biodegradable long-fiber non-woven fabric for thermoforming according to claim 1 or 2, has a forming index of 1.1 to 20 times, and the R / Ave value of the unit area weight of the fabric pieces collected from the same position on the bottom of at least 10 or more formed bodies formed by continuous non-woven fabric using the same forming machine is within 0.

5.

21. A biodegradable beverage extraction container, which is the molded article according to claim 19, characterized in that: The elongation change rate in the MD direction when a load of 0.05 N / 2 mm is applied to the molded body sheet constituting the container by thermomechanical analysis (TMA) at 30 to 100° C. is 4% or less.

22. The beverage extraction container according to claim 21, wherein: The capacity change when immersed in boiling water is 20% to 90%.

23. The beverage extraction container according to claim 21 or 22, characterized in that: The orientation degree of the formed nonwoven fabric is 0.010 or more.

24. The beverage extraction container according to claim 21 or 22, wherein: The crystallinity of the nonwoven fabric formed body is 30 to 70%.