Polyester release film and preparation method thereof

By forming an aqueous coating composition release layer of polyester resin and polyolefin wax on the polyester base layer, the problems of uniform thickness and static electricity in the preparation of polarizing plates are solved, and the polyester separation is achieved The excellent peeling performance and low friction electric power of the type film are suitable for the preparation of thin polarizing plates.

CN115443302BActive Publication Date: 2024-11-19MIKEVO GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180029378.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-28
Filing Date
2021-05-31
Publication Date
2024-11-19
Estimated Expiration
2041-05-31

AI Technical Summary

Technical Problem

When using a low-surface energy silicone-based release film as the base layer, it is difficult to form a barrier coating of uniform thickness, and electrostatic problems may occur, affecting the preparation process of the polarizer.

Method used

An aqueous coating composition using polyester resin and polyolefin wax is used to form a release layer on the polyester base layer, and a polyester release film with excellent peeling performance and low friction electricity is prepared by online coating and heat treatment technology.

Benefits of technology

It realizes excellent peeling performance and low friction electricity of the polyester release film, prevents static pollution, and is suitable for use as a base film for peeling in the preparation of thin polarizing plates.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure relates to a polyester release film and a method for preparing the same. According to the present disclosure, there are provided: a polyester release film made of a non-silicone material and having excellent peeling performance and low triboelectricity; and a method for preparing the polyester release film. The polyester release film can be appropriately used as a peeling base film in preparing a thin polarizing plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyester release film and a preparation method thereof. Background Art

[0002] As display units in image display devices tend to be larger and thinner, there is an increasing demand for thinner polarizing plates.

[0003] One method of reducing the thickness of the polarizing plate is to thin the conventional polarizing plate protective material such as polyethylene terephthalate (PET) or triacetyl cellulose (TAC). Another method of reducing the thickness of the polarizing plate is to replace the polarizing plate protective material with a coating having barrier properties (hereinafter referred to as "barrier coating").

[0004] To form the barrier coating layer, the composition for forming the barrier coating layer is uniformly coated on any substrate layer, cured, and then peeled off.

[0005] In order to obtain a good quality barrier coating, the cured barrier coating should be easily peeled off from the substrate.

[0006] However, when a siloxane-based release film having low surface energy is used as a base layer, it is difficult to form a barrier coating layer having a uniform thickness, and static electricity problems may occur due to siloxane. Summary of the invention

[0007] Technical issues

[0008] In the present disclosure, a polyester release film having excellent peeling performance and low triboelectricity is provided.

[0009] In addition, a method for preparing the polyester release film is provided.

[0010] Technical Solution

[0011] According to one embodiment of the present disclosure, a polyester release film is provided, comprising: a polyester base layer and a release layer formed on at least one surface of the base layer,

[0012] The release layer comprises: an adhesive comprising a polyester resin and a polyolefin wax dispersed on the adhesive, and

[0013] The release layer has a peel strength of less than 10 gf / inch and a triboelectricity of less than 500V.

[0014] According to another embodiment of the present disclosure, there is provided a polyester release film for a thin polarizing plate, comprising: a polyester base layer having a thickness of 20 nm to 200 nm; and a release layer having a thickness of 20 nm to 200 nm, the release layer being formed by in-line coating on the base layer,

[0015] The release layer comprises: an adhesive comprising a polyester resin; and a polyolefin wax dispersed on the adhesive, and

[0016] The release layer has a peel strength of 10 gf / inch or less and a triboelectricity of less than 500V.

[0017] According to another embodiment of the present disclosure, a method for preparing the polyester release film is provided, comprising the following steps:

[0018] (i) preparing a polyester base layer stretched in the machine direction (MD);

[0019] (ii) forming a release layer by applying an aqueous coating composition to at least one surface of the polyester base layer, the aqueous coating composition comprising: a binder comprising a polyester resin; and a polyolefin wax dispersed on the binder; and

[0020] (iii) heat-treating the laminate including the polyester base layer and the release layer formed on the polyester base layer while stretching the laminate in the transverse direction (TD),

[0021] wherein step (iii) is performed while the laminate passes through a heat treatment device, wherein a total heat amount of air supplied to a passing area of ​​the heat treatment device is 222,000 kcal / min to 229,000 kcal / min.

[0022] Hereinafter, a polyester release film and a method for preparing the same according to an embodiment of the present invention will be described in more detail.

[0023] The terminology is used to refer to particular embodiments only, and is not intended to be limiting of the disclosure unless expressly stated.

[0024] Unless differently expressed in the context, a singular expression of the present disclosure may include a plural expression.

[0025] The terms "include", "comprising", etc. in the present disclosure are used to specify specific features, regions, integers, steps, operations, elements and / or components, and these do not exclude the existence or addition of other specific features, regions, integers, steps, operations, elements and / or components.

[0026] I. Polyester release film

[0027] According to one embodiment of the present disclosure, a polyester release film is provided, comprising: a polyester base layer; and a release layer formed on at least one surface of the base layer,

[0028] The release layer comprises: an adhesive comprising a polyester resin; and a polyolefin wax dispersed on the adhesive, and

[0029] The release layer has a peel strength of 10 gf / inch or less and a triboelectricity of less than 500V.

[0030] As a result of the continuous research of the present inventors, it has been confirmed that when an aqueous coating composition comprising a polyester resin and a polyolefin wax is coated on a uniaxially stretched base layer by an online coating method to form a release layer in a peeling base film used in the preparation of a thin polarizing plate, a polyester release film having excellent coating processing performance and peel strength can be provided.

[0031] The polyester release film using the same may exhibit excellent peeling properties in post-processing (eg, a process of forming a barrier coating on the release film, etc.), and may have low triboelectricity, thereby preventing contamination due to static electricity.

[0032] The polyester release film includes a polyester base layer and a release layer formed on at least one surface of the base layer.

[0033] The polyester base layer is made of polyester resin. As the polyester base layer, conventional materials in the field to which the present invention belongs can be used without particular limitation. For example, the polyester base layer can be made of polyethylene terephthalate, polyethylene naphthalate, etc. As a non-limiting example, in terms of achieving weather resistance and hydrolysis resistance, the polyester base layer can be made of polyethylene terephthalate having an intrinsic viscosity of 0.6 dl / g to 0.8 dl / g.

[0034] The release layer is formed on one surface or both surfaces of the polyester base layer. Preferably, the release layer is formed on one surface of the polyester base layer.

[0035] The release layer comprises an adhesive containing a polyester resin and a polyolefin wax dispersed on the adhesive.

[0036] The polyester resin contained in the adhesive is a resin obtained by polycondensation of an acid component containing a dicarboxylic acid as a main component and a diol component containing an alkylene glycol as a main component. As the acid component, terephthalic acid or its alkyl ester or phenyl ester can be mainly used, and a part thereof can be substituted by isophthalic acid, oxyethoxybenzoic acid, adipic acid, sebacic acid, 5-sodium sulfoisophthalic acid, sulfoterephthalic acid, etc. As the diol component, ethylene glycol or diethylene glycol can be mainly used, and a part thereof can be substituted by propylene glycol, trimethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-dioxyethoxybenzene, bisphenol, polyethylene glycol, etc.

[0037] As a non-limiting example, the polyester resin may be obtained by polycondensation of 50 mol % of a diol component including diethylene glycol and ethylene glycol in a molar ratio of 5:5 and 50 mol % of an acid component including terephthalic acid and sulfoterephthalic acid in a molar ratio of 8.5:1.5.

[0038] When the weight average molecular weight of the polyester resin is 2000 g / mol to 25,000 g / mol, it is beneficial for the release layer to have appropriate solvent resistance. Preferably, the weight average molecular weight of the polyester resin may be 2000 g / mol to 25,000 g / mol, 2000 g / mol to 20,000 g / mol, 3000 g / mol to 20,000 g / mol, or 3000 g / mol to 15,000 g / mol.

[0039] In the present disclosure, the weight average molecular weight refers to the weight average molecular weight in terms of polystyrene measured by GPC. In the measurement process of the weight average molecular weight in terms of polystyrene measured by GPC, a known analytical device, a detector such as a refractive index detector, and an analytical chromatographic column can be used, and commonly used temperature conditions, solvents, flow rates, etc. can be applied.

[0040] As a specific example of measurement conditions, a polymer resin such as a polyurethane resin is dissolved in tetrahydrofuran (THF) at a concentration of 1.0 (w / w)% in THF (solid content of about 0.5 (w / w)%), and then filtered using a syringe filter with a pore size of 0.45 μm, and then 20 μl is injected into the GPC. The mobile phase of the GPC is tetrahydrofuran (THF) and flows at a flow rate of 1.0 mL / min. A chromatographic column in which one Agilent PLgel 5μm Guard (7.5×50 mm) and two Agilent PLgel 5μm Mixed D (7.5×300 mm) are connected in series is used, and the measurement is performed at 40°C using an Agilent 1260 InfinityⅡ system and an RI detector.

[0041] Polystyrene standard samples (STD A, B, C, D) obtained by dissolving polystyrene having various molecular weights in tetrahydrofuran at a concentration of 0.1 (w / w)% were filtered through a syringe filter with a pore size of 0.45 μm and then injected into GPC to obtain the weight average molecular weight (Mw) of the polymer using the calibration curve thus formed.

[0042] STD A(Mp):791,000 / 27,810 / 945

[0043] STD B(Mp):282,000 / 10,700 / 580

[0044] STD C(Mp):126,000 / 4430 / 370

[0045] STD D(Mp):51,200 / 1920 / 162

[0046] The release layer may further include acrylic resin as an adhesive.

[0047] For example, the adhesive may include the polyester resin and the acrylic resin in a weight ratio of 1:0.5 to 1:1.5, preferably 1:1, based on solid content.

[0048] Preferably, the acrylic resin may contain a free radical polymerizable unsaturated monomer having a glycidyl group as a comonomer, and the content is 20 mol% to 80 mol% of all monomer components. The free radical polymerizable unsaturated monomer having a glycidyl group improves the strength of the release layer through a cross-linking reaction and prevents leakage of oligomers. The free radical polymerizable unsaturated monomer having a glycidyl group may include glyceryl acrylate, glyceryl methacrylate, aryl glycidyl ether, etc.

[0049] Examples of the free radical polymerizable unsaturated monomer copolymerizable with the free radical polymerizable unsaturated monomer having a glycidyl group may include vinyl esters, unsaturated carboxylates, unsaturated carboxylic acid amides, unsaturated nitriles, unsaturated carboxylic acids, allyl compounds, nitrogen-containing vinyl monomers, hydrocarbon vinyl monomers, and vinyl silane compounds. As the vinyl ester, vinyl propionate, vinyl stearate, vinyl chloride, etc. may be used.

[0050] As unsaturated carboxylic acid esters, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, ethyl methacrylate, butyl methacrylate, butyl maleate, octyl maleate, butyl fumarate, octyl fumarate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, etc. can be used. As unsaturated carboxylic acid amides, acrylamide, methacrylamide, hydroxymethyl acrylamide, butoxyhydroxymethyl acrylamide, etc. can be used. As unsaturated nitrile, acrylonitrile, etc. can be used.

[0051] As unsaturated carboxylic acids, acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, maleic acid esters, fumaric acid esters, itaconic acid esters, etc. can be used. As allyl compounds, allyl acetate, allyl methacrylate, allyl acrylate, allyl itaconic acid, diallylitaconic acid, etc. can be used. As nitrogen-containing vinyl monomers, vinyl pyridine, vinyl imidazole, etc. can be used.

[0052] As the hydrocarbon vinyl monomer, ethylene, propylene, hexene, octene, styrene, vinyltoluene, butadiene, etc. can be used. As the vinylsilane compound, dimethylvinylmethoxysilane, dimethylvinylethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyldimethoxysilane, etc. can be used.

[0053] As a non-limiting example, the acrylic resin may be a copolymer of 40 mol % to 60 mol % of glyceryl ether acrylate and 40 mol % to 60 mol % of propionic acid.

[0054] The weight average molecular weight of the acrylic resin may preferably be 20,000 g / mol to 70,000 g / mol. More preferably, the weight average molecular weight of the polyester resin may be 20,000 g / mol to 60,000 g / mol, 30,000 g / mol to 60,000 g / mol, 40,000 g / mol to 60,000 g / mol, or 45,000 g / mol to 55,000 g / mol.

[0055] The release layer includes a polyolefin wax dispersed on the adhesive.

[0056] The specific kind of the polyolefin wax is not particularly limited, but at least one selected from polyethylene wax and polypropylene wax may be preferably used.

[0057] Based on the adhesive of 100 parts by weight, the content of polyolefin wax can be 10 parts by weight to 40 parts by weight. In order to make the release layer show suitable peel strength, based on the adhesive of 100 parts by weight, the content of polyolefin wax is preferably more than 10 parts by weight. However, if polyolefin wax is added to the release layer with too much amount, reverse transfer (back transfer) problem and processing coating performance reduction will be caused. Therefore, based on the adhesive of 100 parts by weight, the content of polyolefin wax is preferably less than 40 parts by weight.

[0058] For example, based on 100 parts by weight of the adhesive, the content of the polyolefin wax may be 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, or 25 parts by weight or more, and 40 parts by weight or less, 35 parts by weight or less, or 30 parts by weight or less. Specifically, based on 100 parts by weight of the adhesive, the content of the polyolefin wax may be 10 to 40 parts by weight, 15 to 40 parts by weight, 15 to 35 parts by weight, 20 to 35 parts by weight, 20 to 30 parts by weight, or 25 to 30 parts by weight.

[0059] The thickness of the polyester base layer and the release layer is not particularly limited and can be adjusted according to the specific application field of the polyester release film. For example, the thickness of the polyester base layer can be 10 μm to 100 μm, and the thickness of the release layer can be 20 nm to 200 nm.

[0060] In the polyester release film, the polyester base layer may be biaxially stretched in the machine direction (MD) and the transverse direction (TD), and the release layer may be uniaxially stretched in the transverse direction (TD).

[0061] When the above characteristics are met, the polyester release film may have excellent peeling performance and low triboelectricity.

[0062] For example, the polyester release film may have an excellent peel strength of 10 gf / inch or less, 2 gf / inch to 10 gf / inch, 5 gf / inch to 10 gf / inch, or 5 gf / inch to 8 gf / inch.

[0063] In the present disclosure, the peel strength can be measured according to the standard test method of ASTM D903. Specifically, the peel strength can be measured by the following steps: preparing a first sample in which a cured UV resin layer with a thickness of 10 μm is formed on a release layer of a polyester release film; preparing a second sample by reciprocatingly rubbing a TESA tape on the cured UV resin layer of the first sample twice using a 2 kg rubber roller and then cutting it into a size of 2.5 mm×15 cm; and applying 70 g / cm 2 The TESA tape was peeled off at 180° using a peel tester at a peel rate of 300 mm / min.

[0064] Additionally, the polyester release film may have a low triboelectricity of less than 500V, 150V to 450V, 200V to 450V, 200V to 400V, 250V to 400V, or 250V to 350V.

[0065] In the present disclosure, triboelectricity is measured according to the standard test method of KS K 0555. Specifically, triboelectricity can be obtained by measuring static electricity of a polyester release film using a conventional rotary static tester. At this time, static electricity is generated by rubbing the A side (one side of the release layer in the polyester release film) and the B side (one side of the polyester base layer sample on which the release layer is not formed) at 300 rpm for 180 seconds.

[0066] In addition, the polyester release film can exhibit excellent processing and coating properties while having low haze.

[0067] For example, the haze of the polyester release film may be 3.90% or less. Preferably, the haze of the polyester release film may be 3.90% or less, 3.50% to 3.90%, 3.60% to 3.90%, 3.60% to 3.85%, 3.70% to 3.85% or 3.75% to 3.85%.

[0068] In addition, the polyester release film may have excellent processing and coating properties satisfying the following Formula 1:

[0069] [Formula 1]

[0070] N H =0

[0071] In formula 1,

[0072] N H When UV resin is applied to the release layer of the polyester release film to a thickness of 10 μm and cured, the 2 The number of pinholes generated.

[0073] That is, in any manufacturing process using a polyester release film as a base layer, when any resin layer is formed on the release layer, substantially no pinholes are formed on the release layer, thereby exhibiting excellent processing coating properties.

[0074] In addition, the polyester release film may have a total light transmittance of 90% to 95%, a water contact angle of 85° to 90°, a diiodomethane contact angle of 50° to 60°, and a surface energy of 30 mN / m to 35 mN / m.

[0075] According to another embodiment of the present disclosure, there is provided a polyester release film for a thin polarizing plate, comprising: a polyester base layer having a thickness of 20 nm to 200 nm; and a release layer having a thickness of 20 nm to 200 nm, the release layer being formed by in-line coating on the base layer,

[0076] Wherein, the release layer comprises: an adhesive containing a polyester resin and a polyolefin wax dispersed on the adhesive, and

[0077] The release layer has a peel strength of 10 gf / inch or less and a triboelectricity of less than 500V.

[0078] In the polyester release film, the specific details of the polyester base layer and the release layer are the same as described above.

[0079] In particular, in the polyester release film, the release layer is formed by online coating on the polyester base layer. The release layer can be formed by coating an aqueous coating composition containing an adhesive and a polyolefin wax on the polyester base layer using an online coating method.

[0080] Since the release layer is formed by an in-line coating method, it has excellent adhesion to the polyester base layer while having a thin coating thickness, and can exhibit excellent moisture resistance and solvent resistance.

[0081] Since the polyester release film has excellent peeling performance and low triboelectricity, it can be suitably used as a release base film in the preparation of a thin polarizing plate.

[0082] As a non-limiting example, when preparing a thin polarizing plate, a barrier coating layer; a polyvinyl alcohol resin layer; an adhesive layer; and a resin layer such as polyethylene terephthalate (PET), triacetyl cellulose (TAC) or polymethyl methacrylate (PMMA) may be sequentially laminated on a base layer of a polyester release film to form a laminate. Also, the polyester release film may be removed from the laminate.

[0083] II. Preparation method of polyester release film

[0084] According to another embodiment of the present disclosure, a method for preparing the polyester release film is provided, comprising the following steps:

[0085] (i) preparing a polyester base layer stretched in the machine direction (MD);

[0086] (ii) forming a release layer by coating an aqueous coating composition on at least one surface of the polyester base layer, the aqueous coating composition comprising a binder containing a polyester resin and a polyolefin wax dispersed on the binder; and

[0087] (iii) heat-treating the laminate including the polyester base layer and the release layer formed on the polyester base layer while stretching the laminate in the transverse direction (TD),

[0088] wherein step (iii) is performed while the laminate passes through a heat treatment device, wherein a total heat amount of air supplied to a passing area of ​​the heat treatment device is 222,000 kcal / min to 229,000 kcal / min.

[0089] (i) A step of preparing a polyester base layer stretched in the machine direction (MD) is performed.

[0090] The polyester base layer is made of polyester resin. As the polyester base layer, conventional materials in the field to which the present invention pertains may be used without particular limitation.

[0091] The polyester base layer is prepared by stretching in the machine direction (MD, or length direction). Preferably, the polyester base layer can be stretched 2 to 5 times in the machine direction (MD).

[0092] The thickness of the polyester-based substrate is preferably 10 μm to 300 μm.

[0093] Subsequently, (ii) a step of forming a release layer by coating an aqueous coating composition on at least one surface of the polyester-based substrate is carried out. The aqueous coating composition contains an adhesive containing a polyester resin and a polyolefin wax dispersed on the adhesive.

[0094] The aqueous coating composition is used to form a release layer on the polyester-based substrate.

[0095] The aqueous coating composition contains an adhesive and a polyolefin wax dispersed on the adhesive.

[0096] The adhesive contains a polyester resin. The adhesive may also contain an acrylic resin.

[0097] The specific details of the polyester resin, acrylic resin, and polyolefin wax are the same as those described in <I. Polyester Release Film>.

[0098] For example, based on the solid content, the adhesive may preferably contain a polyester resin and an acrylic resin in a weight ratio of 1:0.5 to 1:1.5.

[0099] In addition, based on 100 parts by weight of the adhesive, the aqueous coating composition preferably contains 10 parts by weight to 40 parts by weight of the polyolefin wax.

[0100] Based on the solid content, the total amount of the adhesive and the polyolefin wax contained in the aqueous coating composition may be 4.5 wt% to 6.4 wt%, 4.5 wt% to 6.0 wt%, 4.5 wt% to 5.8 wt%, 5.0 wt% to 5.8 wt%, or 5.1 wt% to 5.8 wt%.

[0101] Based on the solid content, if the total amount of the adhesive and the polyolefin wax contained in the aqueous coating composition is too small, the transfer performance and peeling performance will deteriorate, and the triboelectricity will increase. In addition, if the total amount based on the solid content is too high, the processing coating performance will deteriorate. For example, fine pinholes will appear during the preparation of the polyester release film.

[0102] In the aqueous coating composition, additives such as silicone-based wetting agents, fluorine-based wetting agents, curing agents, acid catalysts, slip agents, defoamers, wetting agents, surfactants, thickeners, plasticizers, antioxidants, ultraviolet absorbers, preservatives, and crosslinking agents may also be added as needed. The additives can be selectively used within the limit of not impairing the physical properties of the aqueous coating composition and the release layer.

[0103] The aqueous coating composition may be prepared by uniformly mixing the above components with water. For the efficiency of the coating process, the solid content of the aqueous coating composition may be 20 wt % to 60 wt %.

[0104] The aqueous coating composition can be used to form a release layer on at least one surface of a polyester base layer by an online coating method. Since the release layer is formed by an online coating method, it has excellent adhesion to the polyester base layer while having a thin coating thickness, and can exhibit excellent water resistance and solvent resistance.

[0105] The in-line coating process can be carried out using conventional equipment.

[0106] When in-line coating is performed, the aqueous coating composition may be applied to a thickness of 20 nm to 200 nm after final stretching and drying of the release layer.

[0107] The release layer is formed by coating the aqueous coating composition on the polyester base layer, and then removing water from the aqueous coating composition, followed by curing.

[0108] Subsequently, (iii) a step of heat-treating the laminate while stretching the laminate including the polyester base layer and the release layer formed on the polyester base layer in the transverse direction (TD, or width direction) is performed.

[0109] The laminate may be stretched 2 to 5 times in the transverse direction (TD).

[0110] For example, a release layer is formed on a polyester base layer uniaxially stretched in the machine direction (MD) and then stretched in the transverse direction (TD). Through this stretching process, the polyester base layer is biaxially stretched in the machine direction and the transverse direction, and the release layer is uniaxially stretched in the transverse direction.

[0111] Step (iii) can be performed using a conventional heat treatment apparatus such as a tenter. In step (iii), the laminate is continuously passed through the tenter.

[0112] The laminate is preheated while passing through the front area of ​​the tenter, stretched in the transverse direction (TD) while passing through the middle area of ​​the tenter, and heat-treated while passing through the rear area of ​​the tenter. Heat-treatment refers to heating while maintaining tension applied to the laminate during stretching in the transverse direction.

[0113] Preferably, step (iii) can be performed while the laminate passes through a heat treatment device in which the total heat of air supplied to the passing area is 222,000 kcal / min to 229,000 kcal / min. The laminate passing through the heat treatment device is transversely stretched and heat-treated while being exposed to the above total heat.

[0114] For example, step (iii) can be carried out while the laminate passes through a heat treatment device, in which the total heat of the air supplied to the entire pass area is 222,000 kcal / min or more, 225,000 kcal / min or more, or 226,000 kcal / min or more, and is 229,000 kcal / min or less, 228,000 kcal / min or less, or 227,000 kcal / min or less.

[0115] Specifically, step (iii) can be carried out while the laminate passes through a heat treatment device, in which the total heat of the air supplied to the entire passing area is 222,000 kcal / min to 229,000 kcal / min, 225,000 kcal / min to 229,000 kcal / min, 226,000 kcal / min to 229,000 kcal / min, 226,000 kcal / min to 228,000 kcal / min or 226,000 kcal / min to 227,000 kcal / min.

[0116] The total heat (kcal) of the air supplied to the entire area through which the laminate passes in step (iii) can be calculated based on data such as the temperature (°C) of the area, the mass (kg / min) of the air supplied to the heat treatment device, and the specific heat (kcal / kg°C) of the air. The mass (kg / min) of the air can be calculated from the volume flow rate (Nm 3 / min) and the density of air (kg / Nm 3 )get.

[0117] For example, when the density of air supplied to any area of ​​the heat treatment device is 1.286 kg / Nm 3 , the specific heat of air is 0.24kcal / kg℃, and the volume flow rate of air is 380Nm 3 / min, the initial temperature of the air is 20°C, and the set temperature of the zone is 220°C, the total heat (kcal) of the air supplied to the zone obtained by the following equations 1 and 2 can be 23,456.64 kcal / min.

[0118] [Equation 1]

[0119] Air mass (kg / min) = air volume flow rate (Nm 3 / min)×density of air (kg / Nm 3 )

[0120] [Equation 2]

[0121] Heat of air (kcal / min) = mass of air (kg / min) × specific heat of air (kcal / kg℃) × temperature change (℃)

[0122] In addition, when the passing length of the zone is 3 m and the laminate passes through the zone at 100 m / min, the amount of heat to which the laminate is exposed in the zone can be calculated as 7037 kcal / zone by the following Equation 3.

[0123] [Equation 3]

[0124] Heat exposure of laminate (kcal / area) = Heat of air (kcal / min) × Passage length of area (m / area) × Speed ​​of laminate (m / min)

[0125] According to one embodiment of the present disclosure, the method may be carried out in the following manner, including: a process of preheating the laminate while the laminate passes through a region supplied with heat of 44,000 kcal / min to 46,000 kcal / min; a process of stretching the laminate in the transverse direction (TD) while the preheated laminate passes through a region supplied with heat of 62,000 kcal / min to 64,000 kcal / min; and a process of heat-treating the laminate while the stretched laminate passes through a region supplied with heat of 114,000 kcal / min to 120,000 kcal / min.

[0126] Preferably, the preheating process may be performed while the laminate passes through a region in which heat of 45,000 kcal / min to 46,000 kcal / min is supplied.

[0127] Preferably, the transverse stretching process may be performed while the preheated laminate passes through a zone in which heat of 63,000 kcal / min to 64,000 kcal / min is supplied.

[0128] In addition, preferably, the heat treatment process can be performed while the stretched laminate passes through a zone where heat of 115,000 kcal / min to 120,000 kcal / min, 115,000 kcal / min to 119,000 kcal / min, 116,000 kcal / min to 119,000 kcal / min, 117,000 kcal / min to 118,500 kcal / min or 118,000 kcal / min to 118,500 kcal / min is supplied.

[0129] In step (iii), the preheating process, the transverse stretching process and the heat treatment process may be performed in two or more zones where the amount of heat supplied varies within the above range, as necessary.

[0130] As a non-limiting example, in step (iii), transverse stretching and heat treatment may be performed while the laminate sequentially passes through two preheating zones, three stretching zones, and five heat treatment zones.

[0131] If the total amount of heat supplied to the passing area (particularly, the heat treatment area after transverse stretching) in step (iii) is too low, the peeling performance and transfer performance of the polyester release film will deteriorate, and the triboelectricity will increase. In addition, if the total amount of heat supplied to the passing area (particularly, the heat treatment area after transverse stretching) in step (iii) is too high, the surface energy of the polyester release film will decrease, thereby reducing the processing and coating performance.

[0132] In addition, in step (iii), the laminate preferably passes through the heat treatment device at a speed of 80 m / min to 120 m / min, 90 m / min to 110 m / min, or 90 m / min to 100 m / min.

[0133] When performing step (iii), the laminate is preferably passed through a heat treatment device within the above-mentioned speed range so that the laminate is exposed to appropriate heat in various regions and the transverse stretching and heat treatment are sufficiently performed.

[0134] Step (iii) may be performed at 120°C to 245°C.

[0135] For example, step (iii) may be performed by preheating the laminate at 120 to 150°C; stretching the preheated laminate in the transverse direction at 130 to 150°C; and heat-treating the stretched laminate at 215 to 245°C.

[0136] Specifically, the heat treatment process of the stretched laminate can be performed at 215°C or more, 220°C or more, 225°C or more, or 230°C or more; and below 245°C, below 240°C, or below 235°C. Specifically, the heat treatment process of the stretched laminate can be performed at 215°C to 245°C, 220°C to 245°C, 220°C to 240°C, 225°C to 240°C, 225°C to 235°C, or 230°C to 235°C.

[0137] If the temperature of the heat treatment process of the stretched laminate is too low, the peeling performance of the polyester release film will deteriorate and the friction electricity will increase. In addition, if the temperature of the heat treatment process is too high, the processing and coating performance will deteriorate, for example, fine pinholes will appear during the preparation of the polyester release film.

[0138] After performing step (iii), a process of relaxing the film at 150° C. to 200° C. by 2% to 10% in the longitudinal and transverse directions, respectively, may be performed.

[0139] The final thickness of the polyester release film obtained through the above process may be 20 μm to 100 μm, 30 μm to 80 μm, or 30 μm to 50 μm.

[0140] Beneficial Effects

[0141] According to the present disclosure, a polyester release film made of a non-silicone material and having excellent peeling performance and low triboelectricity and a preparation method thereof are provided. The polyester release film can be suitably used as a peeling base film in the preparation of a thin polarizing plate. DETAILED DESCRIPTION

[0142] Hereinafter, preferred embodiments are provided to help understand the present invention. However, the following embodiments are only used to illustrate the present invention and do not limit the present invention.

[0143] Preparation Example 1

[0144] The first polyester resin (weight average molecular weight: 10,000 g / mol) was obtained by polycondensation of 50 mol % of a diol component including diethylene glycol and ethylene glycol in a molar ratio of 5:5 and 50 mol % of an acid component including terephthalic acid and sulfoterephthalic acid in a molar ratio of 8.5:1.5.

[0145] 100 parts by weight of the first polyester resin and 25 parts by weight of polyethylene wax were added to distilled water and stirred for 30 minutes to prepare a first resin composition (solid content: 20% by weight).

[0146] Preparation Example 2

[0147] The second polyester resin (weight average molecular weight: 3000 g / mol) was obtained by polycondensation of 50 mol % of a diol component including diethylene glycol and ethylene glycol in a molar ratio of 5:5 and 50 mol % of an acid component including terephthalic acid and sulfoterephthalic acid in a molar ratio of 8.5:1.5.

[0148] 60 mol % of glyceryl ether acrylate and 40 mol % of vinyl propionate were copolymerized to obtain an acrylic resin (weight average molecular weight: 50,000 g / mol).

[0149] 50 parts by weight of the second polyester resin, 50 parts by weight of an acrylic resin, and 25 parts by weight of a polyethylene wax were added to distilled water and stirred for 30 minutes to prepare a second resin composition (solid content: 20% by weight).

[0150] Example 1

[0151] (i) A polyethylene terephthalate (PET) substrate layer stretched 3.5 times in the machine direction (MD) was prepared. Specifically, PET chips from which moisture was removed to 100 ppm or less were injected into a melt extruder and melted, and then rapidly cooled and solidified with a casting drum having a surface temperature of 20° C. while being extruded through a T-die to prepare a PET sheet. The prepared PET sheet was stretched 3.5 times in the machine direction at 110° C. and then cooled to room temperature to obtain a PET substrate layer.

[0152] (ii) 14.3 wt % (solid content: 20 wt %) of the first resin composition according to Preparation Example 1, 14.3 wt % (solid content: 20 wt %) of the second resin composition according to Preparation Example 2, 0.2 wt % of a siloxane-based wetting agent (manufactured by Dow Corning, Q2-5212, solid content: 90 wt %), 0.2 wt % of a fluorine-based wetting agent (manufactured by Dupont, FS-31, solid content: 25 wt %) and 71 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0153] The aqueous coating composition was applied onto the PET base layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate.

[0154] (iii) Subsequently, a step of heat-treating the laminate while stretching the laminate 4 times in the transverse direction (TD) in a tenter divided into a preheating zone, a stretching zone, and a heat treatment zone was performed.

[0155] Step (iii) was performed while passing the laminate (initial width: 5.12 m, initial thickness: 152 μm) through a tenter having a total length of 33 m sequentially including a preheating zone, a stretching zone, and a heat treatment zone at a moving speed of 100 m / min.

[0156] Step (iii) was performed while passing the laminate through a tenter having a total heat of 226,400 kcal / min of air supplied to the passing area.

[0157] In step (iii), the density of the air supplied to the tenter was 1.286 kg / Nm 3 , confirm that the specific heat of air is 0.24kcal / kg℃, and adjust the volume flow rate of air to 270Nm 3 / min to 680Nm 3 / min range.

[0158] Specifically, the laminate was passed through a preheating zone (channel length: 7.5 m) supplied with 45,000 kcal / min of heat at a temperature of about 120° C. to 130° C. Subsequently, the preheated laminate was stretched 4 times in the transverse direction at a temperature of about 130° C. to 140° C. while passing through a stretching zone (channel length: 10.5 m) supplied with 63,200 kcal / min of heat. Subsequently, the stretched laminate was heat treated at a temperature of 230° C. to 235° C. while passing through a heat treatment zone (channel length: 15 m) supplied with 118,200 kcal / min of heat.

[0159] After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing at 200° C. by 10% in the longitudinal and transverse directions, respectively.

[0160] Example 2

[0161] In the same manner as in Example 1, a PET base layer stretched 3.5 times in the machine direction (MD) was prepared.

[0162] 25.75 wt % of the first resin composition according to Preparation Example 1 (solid content: 20 wt %), 0.81 wt % of a melamine curing agent (manufactured by DIC, J-101LF, solid content: 70 wt %), 0.48 wt % of an acid catalyst (manufactured by KING INDUSTRY, Nacure 8924, solid content: 25 wt %), 0.2 wt % of a siloxane wetting agent (manufactured by Dow Corning, Q2-5212, solid content: 90 wt %) and 72.8 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0163] The aqueous coating composition was coated onto the PET substrate layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate. Then, transverse (TD) stretching and heat treatment were performed in the same manner as in Example 1. After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing 10% in the longitudinal and transverse directions at 200°C, respectively.

[0164] Comparative Example 1

[0165] In the same manner as in Example 1, a PET base layer stretched 3.5 times in the machine direction (MD) was prepared.

[0166] 10.75 wt % (solid content: 20 wt %) of the first resin composition according to Preparation Example 1, 10.75 wt % (solid content: 20 wt %) of the second resin composition according to Preparation Example 2, 0.2 wt % of a siloxane-based wetting agent (manufactured by Dow Corning, Q2-5212, solid content: 90 wt %), 0.2 wt % of a fluorine-based wetting agent (manufactured by DuPont, FS-31, solid content: 25 wt %) and 78.1 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0167] The aqueous coating composition was coated onto the PET substrate layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate. Then, transverse (TD) stretching and heat treatment were performed in the same manner as in Example 1. After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing 10% in the longitudinal and transverse directions at 200°C, respectively.

[0168] Comparative Example 2

[0169] In the same manner as in Example 1, a PET base layer stretched 3.5 times in the machine direction (MD) was prepared.

[0170] 17.9 wt % (solid content: 20 wt %) of the first resin composition according to Preparation Example 1, 17.9 wt % (solid content: 20 wt %) of the second resin composition according to Preparation Example 2, 0.2 wt % of a siloxane-based wetting agent (manufactured by Dow Corning, Q2-5212, solid content: 90 wt %), 0.2 wt % of a fluorine-based wetting agent (manufactured by DuPont, FS-31, solid content: 25 wt %) and 63.8 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0171] The aqueous coating composition was coated onto the PET substrate layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate. Then, transverse (TD) stretching and heat treatment were performed in the same manner as in Example 1. After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing 10% in the longitudinal and transverse directions at 200°C, respectively.

[0172] Comparative Example 3

[0173] In the same manner as in Example 1, a PET base layer stretched 3.5 times in the machine direction (MD) was prepared.

[0174] 19.3 wt % of the first resin composition according to Preparation Example 1 (solid content: 20 wt %), 0.61 wt % of a melamine curing agent (manufactured by DIC, J-101LF, solid content: 70 wt %), 0.36 wt % of an acid catalyst (manufactured by KING INDUSTRY, Nacure 8924, solid content: 25 wt %), 0.2 wt % of a siloxane wetting agent (manufactured by Dow Corning, solid content: 90 wt %) and 79.5 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0175] The aqueous coating composition was coated onto the PET substrate layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate. Then, transverse (TD) stretching and heat treatment were performed in the same manner as in Example 1. After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing 10% in the longitudinal and transverse directions at 200°C, respectively.

[0176] Comparative Example 4

[0177] In the same manner as in Example 1, a PET base layer stretched 3.5 times in the machine direction (MD) was prepared.

[0178] 32.2 wt % of the first resin composition according to Preparation Example 1 (solid content: 20 wt %), 1.03 wt % of a melamine curing agent (manufactured by DIC, J-101LF, solid content: 70 wt %), 0.56 wt % of an acid catalyst (manufactured by KING INDUSTRY, Nacure 8924, solid content: 25 wt %), 0.2 wt % of a siloxane wetting agent (manufactured by Dow Corning, Q2-5212, solid content: 90 wt %) and 66 wt % of distilled water were mixed to prepare an aqueous coating composition.

[0179] The aqueous coating composition was coated onto the PET substrate layer using a gravure coater to a final thickness of 70 nm after drying to form a laminate. Then, transverse (TD) stretching and heat treatment were performed in the same manner as in Example 1. After the heat treatment step, a polyester release film having a total thickness of 38 μm was prepared by heat setting by relaxing 10% in the longitudinal and transverse directions at 200°C, respectively.

[0180] Comparative Example 5

[0181] A polyester release film having a thickness of 38 μm was prepared in the same manner as in Example 1, except that the total heat supplied to the passing zone of the tenter in step (iii) was 221,400 kcal / min.

[0182] Specifically, the laminate was passed through a preheating zone (channel length: 7.5 m) supplied with 45,000 kcal / min of heat at a temperature of about 120° C. to 130° C. Subsequently, the preheated laminate was stretched 4 times in the transverse direction at a temperature of about 130° C. to 140° C. while passing through a stretching zone (channel length: 10.5 m) supplied with 63,200 kcal / min of heat. Subsequently, the stretched laminate was heat treated at a temperature of 230° C. to 235° C. while passing through a heat treatment zone (channel length: 15 m) supplied with 113,200 kcal / min of heat.

[0183] Comparative Example 6

[0184] A polyester release film having a thickness of 38 μm was prepared in the same manner as in Example 1, except that the total heat supplied to the passing zone of the tenter in step (iii) was 229,200 kcal / min.

[0185] Specifically, the laminate was passed through a preheating zone (channel length: 7.5 m) supplied with 45,000 kcal / min of heat at a temperature of about 120° C. to 130° C. Subsequently, the preheated laminate was stretched 4 times in the transverse direction at a temperature of about 130° C. to 140° C. while passing through a stretching zone (channel length: 10.5 m) supplied with 63,200 kcal / min of heat. Subsequently, the stretched laminate was heat treated at a temperature of 230° C. to 235° C. while passing through a heat treatment zone (channel length: 15 m) supplied with 121,000 kcal / min of heat.

[0186] Comparative Example 7

[0187] A polyester release film having a thickness of 38 μm was prepared in the same manner as in Example 2, except that the total heat supplied to the passing zone of the tenter in step (iii) was 221,400 kcal / min.

[0188] Specifically, the laminate was passed through a preheating zone (channel length: 7.5 m) supplied with 45,000 kcal / min of heat at a temperature of about 120° C. to 130° C. Subsequently, the preheated laminate was stretched 4 times in the transverse direction at a temperature of about 130° C. to 140° C. while passing through a stretching zone (channel length: 10.5 m) supplied with 63,200 kcal / min of heat. Subsequently, the stretched laminate was heat treated at a temperature of 230° C. to 235° C. while passing through a heat treatment zone (channel length: 15 m) supplied with 113,200 kcal / min of heat.

[0189] Comparative Example 8

[0190] A polyester release film having a thickness of 38 μm was prepared in the same manner as in Example 2, except that the total heat supplied to the passing zone of the tenter in step (iii) was 229,200 kcal / min.

[0191] Specifically, the laminate was passed through a preheating zone (channel length: 7.5 m) supplied with 45,000 kcal / min of heat at a temperature of about 120° C. to 130° C. Subsequently, the preheated laminate was stretched 4 times in the transverse direction at a temperature of about 130° C. to 140° C. while passing through a stretching zone (channel length: 10.5 m) supplied with 63,200 kcal / min of heat. Subsequently, the stretched laminate was heat treated at a temperature of 230° C. to 235° C. while passing through a heat treatment zone (channel length: 15 m) supplied with 121,000 kcal / min of heat.

[0192] Test example

[0193] (1) Optical properties:

[0194] The haze and total light transmittance (TT) of the films of Examples and Comparative Examples were measured using a haze meter (Nippon Denshoku, NDH 5000).

[0195] (2) Transfer performance (transfer test):

[0196] After laminating an untreated PET base film on the release layer of the polyester release film, a load of 50 gf / inch was applied and placed in an oven at 45°C for 24 hours. If the difference in the water contact angle is △2° or more, it indicates transfer (or O), and if there is no difference in the water contact angle, it indicates no transfer (or X).

[0197] (3) Water contact angle:

[0198] The contact angle measurement device ( DSA 100) measures the water contact angle of the release layer relative to the film. 3 μl of pure water (S1, volume mode) is dropped on the film sample, and the average water contact angle at 15 seconds is measured. A total of 5 measurements are made, and the average values ​​are listed below.

[0199] (4) Diiodomethane contact angle:

[0200] Use a contact angle measurement device ( DSA 100) measures the diiodomethane contact angle relative to the release layer of the film. 3 μl of diiodomethane (S1, volume mode) is dropped on the film sample, and the average diiodomethane contact angle at 15 seconds is measured. A total of 5 measurements are made, and the average values ​​are listed below.

[0201] (5) Surface energy:

[0202] The surface energy of the release layer of the film was calculated from the measurement results of the water contact angle and the diiodomethane contact angle using the Owens-Wendt method.

[0203] (6) Processing and coating performance:

[0204] The UV curing sample was prepared by coating a UV resin (Miwon Specialty Chemical Co., MIRAMER M1130) on the release layer of the film to a thickness of 10 μm. The processing coating properties of the sample were evaluated according to the following criteria.

[0205] *Level 1 - per unit area (m 2 )No pinhole

[0206] *Level 2-per unit area (m 2 ) Less than 2 pinholes

[0207] *Level 3 - per unit area (m 2 ) Less than 5 pinholes

[0208] *Level 4 - per unit area (m 2 ) Less than 10 pinholes

[0209] *Level 5 - per unit area (m 2 ) greater than 10 pinholes

[0210] (7) Peel strength:

[0211] The peel strength was measured according to the standard test method of ASTM D903, comprising the following steps: preparing a first sample in which a UV-cured layer was formed by coating a UV resin (Miwon Specialty Chemical Co., MIRAMER M1130) on the release layer of the film to a thickness of 10 μm; preparing a second sample by reciprocatingly rubbing a TESA tape on the cured UV resin layer of the first sample twice using a 2 kg rubber roller and then cutting it into a size of 2.5 mm×15 cm; and applying 70 g / cm 2 The TESA tape was peeled off at 180° at a peeling rate of 300 mm / min using a peel tester (manufactured by Chem Instrument, AR-1000).

[0212] (8) Triboelectricity:

[0213] The triboelectricity of the polyester release film was measured using a rotary static tester (Daei Kagaku Seiki MFG, RST-300a). Side A (the side of the release layer in the polyester release film) was adhered to a rotating drum, and side B (the side of the polyester base layer sample that did not form a release layer) was fixed to a friction table. While rotating side A at a speed of 300 rpm under mechanical control, side B was rubbed against the friction table for 180 seconds, and then the charge was measured.

[0214] [Table 1]

[0215] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 5 Comparative Example 6 S*(wt%) 5.72 4.30 7.16 5.72 5.72 T*(℃) 235 235 235 210 250 H*(kcal) 7545 7545 7545 7390 7625 A*(%) 3.85 3.10 3.99 4.13 3.98 B*(%) 90.34 90.01 90.38 90.30 90.23 C*(°) 87.0 87.0 90.8 79.5 79.5 D*(°) 53.4 45.7 49.3 54.0 54.0 E*(mN / m) 35 39 36 37 37 F*(level) 1 1 3 1 2 G*(gf / inch) 7 16 3 11 8 H* X O X O X I*(V) 274 770 243 503 387

[0216] [Table 2]

[0217] Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 7 Comparative Example 8 S*(wt%) 5.15 3.86 6.44 5.15 5.15 T*(℃) 235 235 235 210 250 H*(kcal) 7545 7545 7545 7390 7625 A*(%) 3.76 3.70 3.79 4.02 3.80 B*(%) 90.51 90.35 90.52 90.45 90.44 C*(°) 85.4 83.0 89.1 80.3 85.4 D*(°) 57.3 49.2 49.7 61.9 57.3 E*(mN / m) 34 38 36 34 34 F*(level) 1 1 2 1 2 G*(gf / inch) 8 12 7 12 8 H* X X X O X I*(V) 310 672 699 513 423

[0218] S*: Total amount of binder and polyolefin wax contained in the aqueous coating composition (based on solid content)

[0219] T*: Heat treatment temperature in the tenter frame (°C)

[0220] H*: Total heat in the stenter (kcal)

[0221] A*: Haze (%)

[0222] B*: Total light transmittance (%)

[0223] C*: Water contact angle (°)

[0224] D*: Diiodomethane contact angle (°)

[0225] E*: surface energy (mN / m)

[0226] F*: Processing and coating performance (level)

[0227] G*: Peel strength (gf / inch)

[0228] H*: Transfer performance

[0229] I*: Triboelectricity (V)

[0230] With reference to Table 1 and Table 2, it can be confirmed that the polyester release film of the example has excellent peeling performance and low triboelectricity, and also has excellent transfer performance and processing and coating performance compared with the release film of the comparative example.

Claims

1. A method for preparing a polyester release film, The following steps are involved: (i) preparing a polyester base layer stretched in the machine direction MD; (ii) forming a release layer by applying an aqueous coating composition to at least one surface of the polyester base layer, the aqueous coating composition comprising a binder containing a polyester resin and a polyolefin wax dispersed on the binder; and (iii) while stretching the laminate including the polyester base layer and the release layer formed on the polyester base layer in the transverse direction TD, heat-treating the laminate at the same time, wherein step (iii) is performed while the laminate passes through a heat treatment device, wherein the total heat of air supplied to the passing area of ​​the heat treatment device is 222,000 kcal / min to 229,000 kcal / min, Wherein, based on 100 parts by weight of the binder, the aqueous coating composition comprises 10 parts by weight to 40 parts by weight of a polyolefin wax, wherein the total amount of the binder and the polyolefin wax contained in the aqueous coating composition is 4.5 wt % to 6.4 wt % based on solid content, and The polyester release film comprises a polyester base layer and a release layer formed on at least one surface of the base layer. The release layer comprises: an adhesive comprising a polyester resin and a polyolefin wax dispersed on the adhesive, The polyester resin contained in the adhesive has a weight average molecular weight of 3000 g / mol to 15,000 g / mol. Wherein, based on 100 parts by weight of the adhesive, the release layer comprises 20 parts by weight to 30 parts by weight of the polyolefin wax, The polyester release film has a peel strength of 5 gf / inch to 8 gf / inch, a triboelectricity of 250 V to 350 V, and a processing and coating performance satisfying the following formula 1: [Formula 1] N H =0 In formula 1, N H When UV resin is applied to the release layer of the polyester release film to a thickness of 10 μm and cured, the 2 The number of pinholes generated.

2. The method for preparing a polyester release film according to claim 1, in, The aqueous coating composition further comprises an acrylic resin as the binder.

3. The method for preparing the polyester release film according to claim 2, in, The adhesive includes the polyester resin and the acrylic resin in a weight ratio of 1:0.5 to 1:1.5 based on solid content.

4. The method for preparing a polyester release film according to claim 1, in, The release layer is formed on at least one surface of the polyester base layer by an in-line coating method using the aqueous coating composition.

5. The method for preparing the polyester release film according to claim 1, in, The stretching in the machine direction MD and the stretching in the transverse direction TD are each performed by stretching 2 to 5 times.

6. The method for preparing the polyester release film according to claim 1, in, In step (iii), the laminate passes through the heat treatment device at 80 m / min to 120 m / min.

7. The method for preparing a polyester release film according to claim 1, in, Step (iii) comprises: Passing the laminate through a zone supplied with heat at 44,000 kcal / min to 46,000 kcal / min to preheat the laminate; A process of stretching the preheated laminate in the transverse direction TD while passing the preheated laminate through a zone supplied with heat of 62,000 kcal / min to 64,000 kcal / min; and A process of heat-treating the stretched laminate while passing the stretched laminate through a zone supplied with heat at 114,000 kcal / min to 120,000 kcal / min.