A titanium carbonitride coating on the surface of 316L stainless steel and a preparation method thereof
The titanium carbonitride coating with equiaxed crystal structure is prepared by low-temperature chemical vapor deposition method, which solves the problems of low density and insufficient anti-corrosion and wear resistance of 316L stainless steel surface coating, achieving high density, low stress and good performance. The combination of bonding strength has significantly improved the anti-corrosion and wear resistance of 316L stainless steel for oil and gas field surface pipelines.
Patent Information
- Application Number
- CN202110603067.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-05-31
AI Technical Summary
The coating on the surface of 316L stainless steel has low density and insufficient anti-corrosion and wear resistance. The existing improvement methods have problems such as thermal expansion coefficient mismatch, large interface stress, low crystallization degree, high defect density and poor density.
The titanium carbonitride coating is prepared using a low-temperature chemical vapor deposition method. The nitrogen source, carbon source and titanium source are chemically reacted and deposited in a chemical reaction deposition furnace to form carbonitride with an equiaxed crystal structure and micron-sized massive grains. Titanium coating reduces the thermal expansion coefficient mismatch and interface stress between the coating and the steel matrix, and improves density and bonding strength.
Significantly improves the corrosion and wear protection performance of 316L stainless steel, enhances the density, bonding force and wear resistance of the coating, and extends the service life.
Smart Images

Figure CN115478258B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion and wear-resistant coatings of intermetallic compounds, and specifically relates to a titanium carbonitride coating on the surface of 316L stainless steel and a preparation method thereof. Background Art
[0002] 316L stainless steel is a pipe material commonly used in surface pipelines in oil and gas fields. Its corrosion and wear resistance mainly rely on its own corrosion resistance and external coating of epoxy anti-corrosion coatings. However, under long-term corrosion and wear conditions, the corrosion resistance of 316L stainless steel itself is still insufficient. Epoxy anti-corrosion coatings are currently one of the main means of surface corrosion protection for metal pipelines in oil and gas fields, and can be used for corrosion and wear protection of 316L stainless steel pipelines. However, epoxy anti-corrosion coatings have the disadvantages of poor wear resistance and low density. Corrosive media can still cause relatively serious corrosion to the 316L stainless steel pipe body, and long-term effective corrosion protection cannot be achieved. Therefore, the corrosion and wear protection capabilities of 316L stainless steel pipes used in surface pipelines in oil and gas fields need to be further enhanced.
[0003] Titanium carbonitride is an intermetallic compound, and the C and N atoms in its structure occupy the lattice points and lattice interstitial positions respectively. Titanium carbonitride coatings have the advantages of acid and alkali corrosion resistance, wear resistance, toughness and good chemical stability. They are often used as corrosion and wear resistant coatings on the surfaces of metals, ceramics, carbon-based composite materials to improve their mechanical properties and service life. However, titanium carbide coatings prepared by traditional methods usually have disadvantages such as mismatch with the thermal expansion coefficient of the substrate, large stress at the interface and inside the coating, low degree of crystallization, high defect density and poor density, which makes steel metal components prone to corrosion, peeling and cracking under corrosion and wear conditions, and their ability to protect steel from corrosion and wear is greatly limited.
[0004] In view of the above shortcomings, the current improvement methods are divided into two categories: (1) Introducing Al elements to prepare TiAlN coatings, forming a dense structure through a ternary compound system formed by Al elements, N elements, and Ti elements, as well as intermediate phases such as TiAl, TiN, and AlN, so as to improve the density and hardness of the coating and enhance the corrosion resistance and wear resistance of the coating; this method enhances the density and hardness of the coating to a certain extent, and improves the corrosion protection performance of the coating; however, the introduction of Al elements increases the lattice constant and the thermal expansion coefficient of the coating and the steel substrate, thereby increasing the internal stress of the coating and reducing the bonding force between the coating and the substrate, increasing the wear rate of the coating, and causing the wear resistance of the steel substrate to decrease and the service life to decrease. (2) Preparing TiCN-based composite coatings. Such as TiC / TiCN, TiN / TiCN, Ti / TiCN, TiC / TiCN / TiN composite coatings, etc. Although TiC / TiCN / TiN composite coatings have achieved good results in terms of density, film-based bonding and toughness. However, the corrosion and wear resistance of composite coatings are easily affected by the structure, interface bonding, phase composition and element distribution of each sub-coating. It is necessary to accurately control the coating preparation parameters to obtain a coating structure with good density and corrosion and wear resistance. In addition, the thickness of the composite coating is often significantly greater than that of a single coating, and the precision of its processing size is lower than that of a single coating. In addition, the preparation process is cumbersome and the production cost is high. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a titanium carbonitride coating on the surface of 316L stainless steel and a preparation method thereof, so as to solve the problems of low density and insufficient corrosion and wear resistance of the coating on the surface of 316L stainless steel in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a titanium carbonitride coating on a surface of 316L stainless steel comprises the following steps:
[0008] Step 1, pre-treating 316L stainless steel substrate;
[0009] Step 2, preheating the pretreated 316L stainless steel substrate with a first auxiliary gas in the chamber of a chemical vapor deposition furnace, introducing a nitrogen source, a carbon source and a titanium source after preheating to perform chemical reaction deposition on the 316L stainless steel substrate, wherein the nitrogen source and the carbon source are both in gaseous state, and the titanium source is loaded by a second auxiliary gas; the chemical reaction deposition temperature is 650-850°C, the time is 40-120min, and the deposition pressure is 0.01-0.08MPa; after chemical reaction deposition, a titanium carbonitride coating is formed on the surface of the 316L stainless steel substrate.
[0010] A further improvement of the present invention is:
[0011] Preferably, the pretreatment process is: cleaning, sandblasting, cleaning and drying are performed on the surface of the 316L stainless steel substrate in sequence.
[0012] Preferably, the first auxiliary gas is nitrogen and / or hydrogen, and the second auxiliary gas is nitrogen.
[0013] Preferably, the nitrogen source is ammonia, nitrogen, nitrogen dioxide, or a combination thereof; the carbon source is methane, ethane, propane, butane, ethylene, propylene, acetylene, or a combination thereof; the titanium source is titanium tetrachloride, titanium powder, butyl titanate, or a combination thereof.
[0014] Preferably, the flow rate of the nitrogen source is 500-800 sccm, and the flow rate of the carbon source is 600-1000 sccm.
[0015] Preferably, step 2 further includes a cooling step, wherein the cooling step is:
[0016] (3-1) First stage cooling process: stop introducing nitrogen source, carbon source, titanium source and the first auxiliary gas, adjust the flow rate of the second auxiliary gas to 100-200 sccm, and cool the temperature to 500-600°C at a cooling rate of 5-10°C / min.
[0017] (3-2) Second stage cooling process: When the temperature drops to 500-600°C, stop introducing the second and third auxiliary gases; when the temperature drops to 300-500°C, stop introducing all auxiliary gases, and then cool to room temperature.
[0018] A titanium carbonitride coating on the surface of 316L stainless steel prepared by the above preparation method, the coating is attached to the surface of 316L stainless steel, the coating is composed of titanium carbonitride micron grains, the micron grains are block-shaped, the average length of the micron grains is 1-3μm, the average width is 1-4μm, and the average thickness is 1-15μm.
[0019] Preferably, the average length of the micron grains is 1-2.5 μm, the average width is 1-2 μm, and the average thickness is 6-8 μm.
[0020] Preferably, based on the total number of atoms, the atomic percentage of nitrogen in the coating is 20-30%, the atomic percentage of carbon is 30-50%, the atomic percentage of titanium is 20-30%, and the sum of the atomic percentages of the three elements is ≤100%.
[0021] Preferably, the micron grains are equiaxed grains.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The invention discloses a method for preparing a titanium carbonitride coating on the surface of 316L stainless steel. The titanium carbonitride coating prepared by the preparation method of the invention through a low-temperature chemical vapor deposition method has the characteristics of high density, uniformity, high crystallinity and low defects; and the stress generated between the coating and a steel substrate due to thermal expansion coefficient mismatch is significantly reduced, and the metallurgical bonding strength with the metal pipeline substrate is enhanced, and the coating has a strong film-base bonding force, thereby significantly enhancing the corrosion and wear protection performance of 316L stainless steel for surface pipelines in oil and gas fields.
[0024] The present invention also discloses a titanium carbonitride coating on the surface of 316L stainless steel, the coating has an equiaxed crystal structure and a micron-sized block grain morphology, the structure can effectively improve the thermal expansion coefficient mismatch between the titanium carbonitride coating and the 316L stainless steel substrate, and reduce the interface stress between the coating and the substrate and the internal stress of the coating. The titanium carbonitride coating material with equiaxed crystals and micron-sized block grains can achieve high corrosion resistance, high wear resistance and low stress. The coating is metallurgically bonded with the metal substrate, and has the characteristics of high corrosion resistance, high wear resistance, good toughness and bonding strength. The coating of the present invention can effectively improve the corrosion resistance and wear resistance of 316L stainless steel materials for ground pipelines. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the XRD test diagram of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0026] Figure 2 This is a SEM test image of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0027] Figure 3 This is the EDS test picture of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline prepared in Example 1.
[0028] Figure 4 This is a cross-sectional SEM test image of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0029] Figure 5 This is the SEM image of the titanium carbonitride crystal coating on the surface of 316L stainless steel prepared in Comparative Example 1.
[0030] Figure 6This is a coating bonding test diagram of the titanium carbonitride crystal coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 (referred to as the coating prepared in Example 1).
[0031] Figure 7 This is a friction coefficient test graph of the titanium carbonitride crystal coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 (referred to as the coating prepared in Example 1).
[0032] Figure 8 This is a test graph of the average wear rate of the titanium carbonitride crystal coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the wear performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 (referred to as the coating prepared in Example 1).
[0033] Fig. 9 This is a test graph of uniform corrosion rate of the titanium carbonitride crystal coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the corrosion resistance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 (referred to as the coating prepared in Example 1). DETAILED DESCRIPTION
[0034] The object of the present invention is to provide a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines and a preparation method thereof.
[0035] A first aspect of the present invention provides a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines, wherein the coating contains titanium carbonitride formed by nitrogen, carbon and titanium.
[0036] In another preferred embodiment, the grains in the coating are equiaxed grains.
[0037] In another preferred embodiment, the grain size of the coating is in micrometer order.
[0038] In another preferred embodiment, the coating grain morphology is blocky.
[0039] In another preferred embodiment, the length of the micron-sized block grains is 1-3 μm, preferably 1-2.5 μm;
[0040] In another preferred embodiment, the width of the micron-sized block grains is 1-4 μm, preferably 1-2 μm.
[0041] In another preferred embodiment, the thickness of the coating is 1-15 μm, preferably 3-12 μm, and more preferably 6-8 μm.
[0042] In another preferred embodiment, the total content of N, C and Ti in the coating is ≥95%, preferably ≥98%, more preferably ≥99%, or ≥99.5%, and most preferably ≥99.9%, based on the total weight of the coating.
[0043] In another preferred embodiment, the ratio of the volume V1 of the equiaxed crystal structure to the volume V0 of the coating (V1 / V0) is ≥60%, preferably ≥80%, more preferably ≥90%, and most preferably ≥99%.
[0044] In another preferred embodiment, the atomic percentage of nitrogen in the coating is 20-30%, the atomic percentage of carbon is 30-50%, and the atomic percentage of titanium is 20-30%, calculated based on the total number of atoms in the coating.
[0045] In another preferred embodiment, the coating comprises one or more selected from the following group:
[0046] (1) The friction coefficient of the coating is 0.13-0.25;
[0047] (2) The average wear rate of the coating is 2.1×10 -7- 2.5×10 -7 mm 3 N -1 m -1 .
[0048] (3) The average bonding strength of the coating is 91N
[0049] (4) The uniform corrosion rate of the coating is 0.00012 mm / a.
[0050] In a second aspect, the present invention provides a method for preparing a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines as described in the first aspect of the present invention, wherein the method comprises the steps of:
[0051] (1) providing a substrate;
[0052] (2) A low-temperature chemical vapor deposition method is used to form a film by chemical reaction on the surface of the substrate in the presence of a nitrogen source, a carbon source and a titanium source, thereby forming the coating on the surface of the substrate.
[0053] In another preferred embodiment, the centralized procurement is 316L high-speed steel.
[0054] In another preferred embodiment, in the step (1), the substrate includes an untreated or pretreated substrate.
[0055] In another preferred embodiment, in the step (1), the substrate is a pretreated substrate, and the pretreatment comprises the steps of: (a) performing surface cleaning, sandblasting, surface cleaning and drying treatments on the surface of the substrate in sequence.
[0056] In another preferred embodiment, in the step (a), the following materials are selected for sandblasting: white corundum sand (aluminum oxide sand), brown corundum sand (aluminum oxide sand), quartz sand, or a combination thereof.
[0057] In another preferred embodiment, the particle size of the brown corundum sand is 300-500 mesh.
[0058] In another preferred embodiment, in the step (a), the surface cleaning is ultrasonic cleaning.
[0059] In another preferred embodiment, in step (a), the cleaning agent used for surface cleaning is selected from the following group: alcohol, acetone, water, or a combination thereof.
[0060] In another preferred embodiment, the water is selected from the following group: distilled water, deionized water, or a combination thereof.
[0061] In another preferred embodiment, the ultrasonic cleaning time is 20-30 minutes.
[0062] In another preferred embodiment, in the step (a), the drying temperature is 60-80°C.
[0063] In another preferred embodiment, in the step (a), the drying time is 4-8 hours.
[0064] In another preferred embodiment, the method further comprises the step of: (b) before performing the step (2), introducing a first auxiliary gas under vacuum conditions to preheat the substrate.
[0065] In another preferred embodiment, in the step (b), the vacuum degree under the vacuum conditions is ≤0.1 MPa, preferably 0.03-0.06 MPa.
[0066] In another preferred embodiment, in the step (b), the first auxiliary gas is selected from the following group: helium, argon, nitrogen, helium, hydrogen or a combination thereof.
[0067] In another preferred embodiment, in the step (b), the flow rate of the first auxiliary gas is 300-500 sccm.
[0068] In another preferred embodiment, in the step (b), the first auxiliary gas is nitrogen and hydrogen.
[0069] In another preferred embodiment, the flow rate of the nitrogen gas is 200-300 sccm.
[0070] In another preferred embodiment, the flow rate of hydrogen is 100-200 sccm.
[0071] In another preferred embodiment, the purity of the nitrogen is 99.9%.
[0072] In another preferred embodiment, the flow rate of hydrogen is 99.99% sccm
[0073] In another preferred embodiment, in the step (b), in the preheating step, the heating rate is 5-8°C / min.
[0074] In another preferred embodiment, in the step (b), the preheating temperature is 40-70°C.
[0075] In another preferred embodiment, in the step (2), the chemical vapor deposition method comprises the steps of: introducing a nitrogen source, a carbon source, a titanium source and a second auxiliary gas to deposit the coating on the surface of the substrate.
[0076] In another preferred embodiment, in the step (2), the nitrogen source is ammonia, nitrogen, nitrogen dioxide, or a combination thereof.
[0077] In another preferred embodiment, the flow rate of the nitrogen source gas is 500-800 sccm.
[0078] In another preferred embodiment, the nitrogen source is nitrogen gas.
[0079] In another preferred embodiment, the purity of the nitrogen is 99.9%.
[0080] In another preferred embodiment, in the step (2), the carbon source is selected from the group consisting of methane, ethane, propane, butane, ethylene, propylene, acetylene, or a combination thereof.
[0081] In another preferred embodiment, the carbon source is selected from the following group: methane, ethane, propylene, or a combination thereof.
[0082] In another preferred embodiment, the purity of the methane is 99.9%.
[0083] In another preferred example, the flow rate of methane is 600-1000 sccm.
[0084] In another preferred embodiment, in the step (2), the titanium source is selected from the following group: titanium tetrachloride, titanium trichloride, titanium dichloride, butyl titanate, titanium powder, titanium dioxide, or a combination thereof.
[0085] In another preferred embodiment, the titanium source is selected from the following group: titanium tetrachloride, titanium powder, butyl titanate, or a combination thereof.
[0086] In another preferred embodiment, the titanium source is titanium tetrachloride.
[0087] In another preferred embodiment, the purity of the titanium tetrachloride is 99.9%.
[0088] In another preferred embodiment, in the step (2), the titanium source is introduced using the second auxiliary gas as a carrier.
[0089] In another preferred embodiment, the second auxiliary gas is selected from the following group: argon, nitrogen, helium, hydrogen, or a combination thereof.
[0090] In another preferred embodiment, the flow rate of the second auxiliary gas is 500-800 sccm.
[0091] In another preferred example, the second auxiliary gas is nitrogen.
[0092] In another preferred embodiment, the heating rate is 5-8°C / min to the deposition temperature.
[0093] In another preferred embodiment, in the step (2), the deposition conditions include: the deposition temperature is 650-850°C.
[0094] In another preferred embodiment, in the step (2), the deposition conditions further include: the deposition time is 40-120 min, preferably 60-100 min, and more preferably 80-90 min.
[0095] In another preferred embodiment, in the step (2), the deposition conditions further include: the deposition pressure is 0.01-0.08 MPa, preferably, 0.02-0.07 MPa, and more preferably, 0.03-0.06 MPa.
[0096] In another preferred embodiment, the method further comprises step (3): cooling the coating obtained in step (2), wherein the cooling step comprises:
[0097] (3-1) First stage cooling process: stop introducing nitrogen source, carbon source, titanium source and the first auxiliary gas, adjust the flow rate of the second auxiliary gas to 100-200 sccm, and cool the temperature to 500-600°C at a cooling rate of 5-10°C / min.
[0098] (3-2) Second stage cooling process: when the temperature drops to 500-600°C, the flow rate of the second auxiliary gas is adjusted to 50-150 sccm; when the temperature drops to 300-500°C, the flow of the second auxiliary gas is stopped, and then cooled to room temperature.
[0099] The titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 was subjected to XRD, SEM and EDS tests. The test results are as follows: Figure 1-4 shown.
[0100] the term
[0101] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0102] As used herein, the terms "coating" and "titanium carbonitride corrosion and wear resistant coating" are interchangeable.
[0103] As used herein, the terms "include", "comprises", and "comprising" are interchangeable and include not only closed definitions, but also semi-closed and open definitions. In other words, the terms include "consisting of", "consisting essentially of".
[0104] As used herein, the term "316 stainless steel" refers to the American AISI standard grade, which is 316L steel. This grade of steel corresponds to the Chinese GB standard grade 022Cr17Ni12Mo2 (the national standard is the current version of GB / T 20878-2007), the German DIN standard grade 1.4404, the Japanese JIS standard grade SUS316L, and the British BS grade 316S12. "316L steel" and "316L stainless steel" can be used interchangeably.
[0105] As used herein, the term "CVD furnace" refers to a chemical vapor deposition furnace.
[0106] As used herein, the term "nitrogen source" refers to a raw material that provides nitrogen in a coating.
[0107] As used herein, the term "carbon source" refers to a raw material that provides carbon elements in a coating.
[0108] As used herein, the term "titanium source" refers to a raw material that provides the titanium element in the coating.
[0109] As used herein, the term "equiaxed crystal structure" refers to a structure in which grains in the coating are organized in such a way that the grains have relatively small differences in size in all directions within the coating.
[0110] As used herein, the term "micrometer-sized" means providing a coating having a grain size ranging from 1×10-6 m to 1×10-5 m.
[0111] As used herein, the term "blocky" refers to providing a linear profile characteristic of grains in the coating.
[0112] As used herein, the term "low temperature chemical vapor deposition" refers to providing a coating preparation temperature range of 500°C to 900°C.
[0113] As used herein, the term "sccm" is a unit of volume flow, ie, standard-state cubic centimeter per minute.
[0114] As used herein, the term "min" is a unit of time, namely, minute in English.
[0115] As used herein, the term "assistant gas" refers to a gas having a purity of 99.9%.
[0116] A titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines
[0117] The invention provides a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines. The coating contains titanium carbide formed by carbon and titanium elements, and the titanium carbonitride in the coating contains an equiaxed crystal structure and is composed of micron-sized block grains.
[0118] In the present invention, the term "equiaxed grains" refers to the phenomenon that the grain sizes in the coating are slightly different in all directions.
[0119] The term "micron-sized blocky grains" means that the outer contour of the grains in the coating is regular and the size ranges from 1×10-6m to 1×10-5m.
[0120] The term "low temperature chemical vapor deposition" refers to providing a coating preparation temperature range of 500°C to 900°C.
[0121] In a preferred embodiment of the present invention, the method for preparing the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines comprises the following steps:
[0122] 1. Place the substrate in a CVD device, evacuate the back to a vacuum of 0.3-3 Pa, and introduce the first auxiliary gas (such as a mixture of nitrogen and hydrogen, with a hydrogen flow rate of 100-200 sccm and an argon flow rate of 200-300 sccm). Start the gas system preheating program, with a preheating temperature of 60-80°C and a heating rate of 5-8°C / min;
[0123] 2. Continuously introduce the first auxiliary gas until it is heated to 650-850°C at a rate of 5-8°C / min, and introduce the nitrogen source, carbon source, titanium source and the second, wherein the titanium source is introduced with the second auxiliary gas as the carrier gas, and the flow rate of the second auxiliary gas is 500-800sccm; the flow rate of the nitrogen source is 500-800sccm, and the flow rate of the carbon source is 600-1000sccm; the deposition time is 80-90min, and the deposition pressure is 0.03-0.06MPa;
[0124] 3. After the deposition is completed, a controllable cooling program is entered, and the introduction of the titanium source, nitrogen source, carbon source and the first auxiliary gas is stopped. The flow rate of the second auxiliary gas is adjusted to 100-200 sccm, and the cooling rate is 5-10°C / min, and the temperature is cooled to 500-600°C; when the temperature is cooled to 500-600°C, the flow rate of the second auxiliary gas is adjusted to 50-150 sccm; when the temperature is cooled to 300-500°C, the introduction of the second auxiliary gas is stopped; then cooled to room temperature, a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines is obtained.
[0125] Example 1
[0126] Preparation of Titanium Carbonitride Anti-Corrosion and Wear-Resistant Coating on 316L Stainless Steel Surface for Oil and Gas Field Surface Pipelines
[0127] 1. Clean and polish the surface of 316L stainless steel substrate with a size of 20mm*10mm*5mm, remove impurities, sandblast the surface with brown corundum sand, clean it with alcohol ultrasonic wave for 20-30 minutes after polishing, dry it at 60-80℃ for 4-8 hours, and then place it in CVD device.
[0128] 2. The CVD device was evacuated to 0.3-3Pa, and nitrogen and hydrogen were filled in, with a nitrogen flow rate of 200sccm and a hydrogen flow rate of 100sccm. The gas system preheating program was started, and the preheating temperature was set to 50°C and the preheating rate was set to 5°C / min.
[0129] 3. Prepare the deposited coating by low-temperature chemical vapor deposition, including the steps of: starting the CVD system heating program, setting the heating temperature to 750°C, and the heating rate to 8°C / min. The CVD device is heated to 750°C to enter the deposition program, and nitrogen, methane, titanium tetrachloride, etc. are introduced in sequence; the nitrogen flow rate is 600sccm, and the methane flow rate is 800sccm; the deposition time is 90min, wherein titanium tetrachloride is loaded into the CVD device with the second auxiliary gas nitrogen as the carrier gas, and the second auxiliary gas flow rate is 800sccm.
[0130] 4. After the deposition is completed, the CVD device enters a controllable cooling mode, stops introducing the titanium source, nitrogen source, carbon source and the first auxiliary gas, adjusts the flow rate of the second auxiliary gas to 200 sccm, and cools to 500°C at a cooling rate of 10°C / min; when the temperature drops to 500°C, the flow rate of the second auxiliary gas is adjusted to 100 sccm; when the temperature drops to 300°C, stops introducing the second auxiliary gas; then cools to room temperature to obtain a titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines.
[0131] Determination
[0132] The titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 was subjected to XRD, SEM and EDS tests. The test results are as follows: Figure 1-4 shown.
[0133] Figure 1 This is the XRD test diagram of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1. Figure 1 It shows that the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 is composed of titanium carbonitride grains, the structure is a face-centered cubic structure, and the preferred growth orientation is the (111) plane.
[0134] Figure 2 This is a surface SEM test image of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1. Figure 2 It shows that the surface of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1 is dense and uniform, and the coating is composed of micron-sized block grains with an equiaxed crystal structure; the block grains are 1-2.5μm in length and 1-2μm in width.
[0135] Figure 3 This is the EDS test image of the surface of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1. Figure 2 It shows that the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1 is mainly composed of carbon, nitrogen and titanium, wherein the atomic percentage of carbon is 24.82%, the atomic percentage of nitrogen is 21.65%, and the atomic percentage of titanium is 53.53%.
[0136] Figure 4 This is a cross-sectional SEM test image of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines obtained in Example 1. Figure 4It shows that the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 is tightly bonded to the substrate, and the coating thickness is 22-23 μm.
[0137] Figure 5 This is a SEM test image of the titanium carbonitride crystal coating on the surface of 316L stainless steel obtained in Comparative Example 1. Figure 5 It is shown that the titanium carbonitride crystal coating on the surface of 316L stainless steel obtained in Comparative Example 1 mainly has flaky grains that are aggregated into a cellular structure, and the grain size is 200-300nm.
[0138] According to calculation, the elements of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 are nitrogen, carbon and titanium. The nitrogen content accounts for about 21.65% by mole, the carbon content accounts for about 24.82% by mole, and the titanium content accounts for about 53.53% by mole. The atomic percentages of nitrogen, carbon, titanium and are shown in Table 1.
[0139] Table 1 shows the atomic percentage of each element in the titanium carbonitride coating prepared in Example 1
[0140]
[0141] Performance test coating adhesion test
[0142] Method: The coating adhesion comparison test was performed on the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0143] Coating adhesion test method: CSM Revetest scratch tester is used to test the adhesion of the coating. Test mode: A diamond indenter material with a radius of 0.2 mm and a cone angle of 120° is used to perform a unidirectional scratch test on the sample at room temperature. The specific test parameters are: normal load 0-100N, scratch speed 1.5mm / min, test distance 3mm, each sample is tested 3 times, and the average value of the results is taken.
[0144] result:
[0145] The bonding strength of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 is 91N. Figure 6 shown.
[0146] Friction performance test
[0147] Method: The friction performance comparison test was conducted on the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0148] Friction performance test method: Rtec friction and wear tester was used to test the wear resistance of the sample. Test mode: 6mm SiC ball was used to perform XY bidirectional linear non-lubricated reciprocating friction on the sample at room temperature. The specific test parameters were: normal load 5-20N, friction speed 20mm / s, friction distance 5mm, time 20min, frequency 2Hz. Each sample was tested 3 times and the average value of the results was taken.
[0149] result:
[0150] The friction coefficient of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipeline obtained in Example 1 is 0.18. Figure 7 shown.
[0151] Wear performance test
[0152] Method: The wear performance comparison test was conducted on the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0153] Wear performance test method: Based on the friction performance test, firstly, the wear scar volume test is carried out by the surface profiler to obtain the wear scar volume data; secondly, the wear scar volume data is integrated and calculated by the analysis software to obtain the wear scar volume value; finally, the wear rate is calculated according to the wear rate calculation formula:
[0154]
[0155] in,
[0156] W: volume wear rate; V: wear volume; S: load size; L: total friction distance.
[0157] result:
[0158] The average wear rate of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 is 2.3×10 -7 mm 3 N -1 m -1 ,like Figure 8 shown.
[0159] Corrosion resistance test
[0160] Method: A corrosion performance comparison test was performed on the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.
[0161] Corrosion performance test method: Before the test, the sample weight is weighed using an electronic balance; then the sample anti-H2S corrosion performance is tested using a high-temperature autoclave device. The test parameters are: temperature: 60°C, H2 The S pressure is 0.1MPa, and the test time is 360 hours. After the test, the surface corrosion products are removed by ultrasonic cleaning with chemical cleaning solution (500mL hydrochloric acid + 3.5 hexamethylenetetramine + 500mL deionized water), and then the surface is cleaned with 10% NaOH solution, deionized water and anhydrous ethanol for 20 minutes in sequence, and then the surface is dried with cold air and weighed with an electronic balance.
[0162] The calculation formula for uniform corrosion is:
[0163]
[0164] in,
[0165] CR: uniform corrosion rate (mm / a); W: mass loss (mg); A: sample surface area (mm 2 ); D: coating density (mg / cm 3 ); t: experimental time (h)
[0166] result:
[0167] Example 1 Composite L360QS stainless steel surface anti-H 2 The uniform corrosion rate of the titanium nitride wear-resistant coating corroded by S is 0.00012mm / a. Fig. 9 shown.
[0168] Example 2
[0169] The method is the same as in Example 1, except that in step 1, the nitrogen flow rate is 1000 sccm
[0170] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 98%. The length of the micron-sized block grain is 1.5 μm and the width is 2.5 μm. The nitrogen atomic content in the coating is 22.43%, the carbon atomic content is 25.82%, and the titanium atomic content is 51.75%. The average bonding force of the coating is 75 N, the friction coefficient of the coating is 0.22, and the average wear rate is 3.5×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0003mm / a.
[0171] Example 3
[0172] The method is the same as that of Example 1, except that in step 3, the carbon source is propylene.
[0173] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 97%. The length of the micron-sized block grain is 1.3 μm and the width is 2.1 μm. The nitrogen atomic content in the coating is 26.65%, the carbon atomic content is 22.19%, and the titanium atomic content is 47.84%. The average bonding force of the coating is 82 N, the friction coefficient of the coating is 0.26, and the average wear rate is 3.3×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0003mm / a.
[0174] Example 4
[0175] The method is the same as that of Example 1, except that in step 3, the titanium source is titanium powder.
[0176] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology, and the ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 98%; the length of the micron-sized block grain is 1.6 μm and the width is 1.8 μm; the nitrogen atomic content in the coating is 25.24%, the carbon atomic content is 28.33%, and the titanium atomic content is 52.57%; the average bonding force of the coating is 80 N, the friction coefficient of the coating is 0.24, and the average wear rate is 3.1×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0002mm / a.
[0177] Example 5
[0178] The method is the same as that of Example 1, except that in step 3, the deposition temperature is 800°C.
[0179] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 97%. The length of the micron-sized block grain is 1.2 μm and the width is 1.6 μm. The nitrogen atomic content in the coating is 27.22%, the carbon atomic content is 24.55%, and the titanium atomic content is 48.24%. The average bonding force of the coating is 85 N, the friction coefficient of the coating is 0.22, and the average wear rate is 3.0×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0002mm / a.
[0180] Example 6
[0181] The method is the same as that of Example 1, except that the first auxiliary gas is hydrogen.
[0182] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 98%. The length of the micron-sized block grain is 1.4 μm and the width is 1.5 μm. The nitrogen atomic content in the coating is 21.76%, the carbon atomic content is 23.82%, and the titanium atomic content is 44.58%. The average bonding force of the coating is 86 N, the friction coefficient of the coating is 0.23, and the average wear rate is 2.9×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0002mm / a.
[0183] Example 7
[0184] The method is the same as that of Example 1, except that in step 3, the methane flow rate is 1000 sccm.
[0185] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 97%. The length of the micron-sized block grain is 1.8 μm and the width is 1.7 μm. The nitrogen atomic content in the coating is 28.54%, the carbon atomic content is 22.67%, and the titanium atomic content is 44.58%. The average bonding force of the coating is 85 N, the friction coefficient of the coating is 0.24, and the average wear rate is 3.2×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0003mm / a.
[0186] Example 8
[0187] The method is the same as that of Example 1, except that in step 3, the hydrogen flow rate is 1000 sccm.
[0188] The results show that the coating shows an equiaxed crystal structure and a micron-sized block grain morphology. The ratio of the equiaxed crystal structure V1 to the volume V0 of the coating (V1 / V0) is 98%. The length of the micron-sized block grain is 1.4 μm and the width is 1.5 μm. The nitrogen atomic content in the coating is 21.36%, the carbon atomic content is 23.82%, and the titanium atomic content is 44.18%. The average bonding force of the coating is 86 N, the friction coefficient of the coating is 0.23, and the average wear rate is 2.9×10 -7 mm 3 N -1 m, and the average corrosion rate of the coating is 0.0003mm / a.
[0189] Comparative Examples 1-6
[0190] Preparation of Titanium Carbonitride Crystal Coating Composited on 316 Stainless Steel Surface
[0191] The titanium carbide crystal coatings described in Comparative Examples 1-6 were prepared in a similar manner to Example 1, except that the parameters in the coating preparation process were changed as shown in Table 2, and the grain morphology, grain size, and element percentage of the coatings were characterized. At the same time, the same bonding performance test, corrosion resistance test, friction performance test, and wear performance test methods as those in Example 1 were used to measure performance data such as bonding strength, corrosion resistance, friction coefficient, and average wear rate.
[0192] Among them, the SEM image of the titanium carbonitride crystal coating composited on the surface of 316L stainless steel obtained in Comparative Example 1 is as follows Figure 5 As shown. Figure 5 It can be seen that the grains of the titanium carbonitride crystal coating prepared in Comparative Example 1 are flaky and aggregated into a cellular characteristic morphology, and the grain size is 200-300 nm.
[0193] Table 2 Characterization and performance test of titanium carbonitride crystal coating prepared in Comparative Examples 1-6
[0194]
[0195] Comparison of Examples 1-8 and Comparative Examples 1-6
[0196] The friction and wear properties of the coatings prepared in Example 1 and Comparative Examples 1-6 were compared. The comparison results are shown in Figure 7 and Figure 8 .
[0197] from Figure 7 and Figure 8 It can be seen that the average bonding force of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 is 91N, which is significantly greater than the titanium carbonitride crystal coating prepared in Comparative Examples 1-6 (such as the bonding force of Comparative Example 3 is 58N). The friction coefficient of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 is 0.18, which is significantly less than the titanium carbonitride crystal coating prepared in Comparative Examples 1-6 (such as the friction coefficient of Comparative Example 2 can reach 0.35). The average wear rate of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 is 2.3×10 -7 mm 3 N -1 m -1 , which is significantly smaller than that of Comparative Examples 1-6 (e.g., in Comparative Example 4, the average wear rate is 3.5×10 -6 mm 3 N -1m). The average corrosion rate of the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 is 0.00012 mm / a, which is significantly lower than that of Comparative Examples 1-6 (such as Comparative Example 2, the average corrosion rate is 0.0026 mm / a). Therefore, compared with Comparative Examples 1-6, the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1 of the present invention has excellent anti-corrosion and wear resistance.
[0198] The average corrosion rate, friction coefficient and average wear rate of Examples 1-8 are significantly lower than those of Comparative Examples 1-6, indicating that the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Examples 1-8 has excellent anti-corrosion and wear resistance.
[0199] Example 9
[0200] In this embodiment, the nitrogen source is ammonia, the carbon source is methane, the titanium source is titanium tetrachloride, and the other steps not involved are the same as those in Example 1.
[0201] Example 10
[0202] In this embodiment, the nitrogen source is nitrogen dioxide, the carbon source is ethane, the titanium source is titanium trichloride, and the other steps not involved are the same as those in Example 1.
[0203] Embodiment 11
[0204] In this embodiment, the nitrogen source is ammonia, the carbon source is propane, the titanium source is titanium dichloride, and the other steps not involved are the same as those in Example 1.
[0205] Example 12
[0206] In this embodiment, the nitrogen source is ammonia, the carbon source is methane, the titanium source is titanium tetrachloride, and the other steps not involved are the same as those in Example 1.
[0207] Embodiment 13
[0208] In this embodiment, the nitrogen source is ammonia, the carbon source is butane, the titanium source is butyl titanate, and the other steps not involved are the same as those in Example 1.
[0209] Embodiment 14
[0210] In this embodiment, the nitrogen source is ammonia, the carbon source is ethylene, the titanium source is titanium dioxide, and the other steps not involved are the same as those in Example 1.
[0211] Embodiment 15
[0212] In this embodiment, the nitrogen source is ammonia, the carbon source is acetylene, the titanium source is titanium tetrachloride, and the other steps not involved are the same as those in Example 1.
[0213] Example 16
[0214] In this embodiment, in step 3, the carbon source flow rate is 600 sccm, the nitrogen source flow rate is 500 sccm, the deposition time is 80 min, the deposition temperature is 700° C., and the deposition pressure is 0.03 MPa.
[0215] Embodiment 17
[0216] In this embodiment, in step 3, the carbon source flow rate is 800 sccm, the nitrogen source flow rate is 800 sccm, the deposition time is 85 min, the deposition temperature is 650° C., and the deposition pressure is 0.04 MPa.
[0217] Embodiment 18
[0218] In this embodiment, in step 3, the carbon source flow rate is 1000 sccm, the nitrogen source flow rate is 600 sccm, the deposition time is 90 min, the deposition temperature is 850° C., and the deposition pressure is 0.06 MPa.
[0219] Embodiment 19
[0220] In this embodiment, in step 3, the carbon source flow rate is 800 sccm, the nitrogen source flow rate is 800 sccm, the deposition time is 40 min, the deposition temperature is 650° C., and the deposition pressure is 0.01 MPa.
[0221] Embodiment 20
[0222] In this embodiment, in step 3, the carbon source flow rate is 1000 sccm, the nitrogen source flow rate is 600 sccm, the deposition time is 120 min, the deposition temperature is 850° C., and the deposition pressure is 0.08 MPa.
[0223] Embodiment 21
[0224] In this embodiment, in step 4, after the deposition is completed, the CVD device enters a controllable cooling mode, the introduction of the titanium source, the nitrogen source and the carbon source is stopped, and the flow rate of the second auxiliary gas is adjusted to 100 sccm; the cooling rate is 8°C / min, and the temperature is cooled to 550°C. When the temperature is cooled to 550°C, the introduction of the second auxiliary gas is stopped; when the temperature is cooled to 350°C, the introduction of all auxiliary gases is stopped.
[0225] Embodiment 22
[0226] In this embodiment, in step 4, after the deposition is completed, the CVD device enters a controllable cooling mode, the introduction of the titanium source, the nitrogen source and the carbon source is stopped, and the flow rate of the second auxiliary gas is adjusted to 150 sccm; the cooling rate is 6°C / min, and the temperature is cooled to 500°C. When the temperature is cooled to 500°C, the introduction of the second auxiliary gas is stopped; when the temperature is cooled to 300°C, the introduction of all auxiliary gases is stopped.
[0227] Embodiment 23
[0228] In this embodiment, in step 4, after the deposition is completed, the CVD device enters a controllable cooling mode, the introduction of the titanium source, the nitrogen source and the carbon source is stopped, and the flow rate of the second auxiliary gas is adjusted to 200 sccm; the cooling rate is 10°C / min, and the temperature is cooled to 600°C. When the temperature drops to 600°C, the introduction of the second auxiliary gas is stopped; when the temperature drops to 500°C, the introduction of all auxiliary gases is stopped.
[0229] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.
[0230] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a titanium carbonitride coating on the surface of 316L stainless steel, characterized in that: The following steps are involved: Step 1, pre-treating 316L stainless steel substrate; Step 2, preheating the pretreated 316L stainless steel substrate with a first auxiliary gas in the chamber of a chemical vapor deposition furnace, introducing a nitrogen source, a carbon source and a titanium source after preheating to perform chemical reaction deposition on the 316L stainless steel substrate, wherein the nitrogen source and the carbon source are both in gaseous state, and the titanium source is loaded by a second auxiliary gas; the chemical reaction deposition temperature is 650-850° C., the time is 40-120 min, and the deposition pressure is 0.01-0.08 MPa; after chemical reaction deposition, a titanium carbonitride coating is formed on the surface of the 316L stainless steel substrate; The nitrogen source is ammonia, nitrogen, nitrogen dioxide, or a combination thereof; the carbon source is methane, ethane, propane, butane, ethylene, propylene, acetylene, or a combination thereof; the titanium source is titanium tetrachloride, titanium powder, butyl titanate, or a combination thereof; The flow rate of the nitrogen source is 500-800 sccm, and the flow rate of the carbon source is 600-1000 sccm; The step 2 further includes a cooling step, wherein the cooling step is: (3-1) First stage cooling process: stop introducing nitrogen source, carbon source, titanium source and the first auxiliary gas, adjust the flow rate of the second auxiliary gas to 100-200 sccm, and cool down to 500-600°C at a cooling rate of 5-10°C / min; (3-2) Second stage cooling process: when the temperature drops to 500-600°C, stop introducing the second auxiliary gas; when the temperature drops to 300-500°C, stop introducing all auxiliary gases, and then cool to room temperature; The coating is attached to the surface of 316L stainless steel, and the coating is composed of titanium carbonitride micron grains, the micron grains are block-shaped, and the average length of the micron grains is 1-3 μm, the average width is 1-4 μm, and the average thickness is 1-15 μm; Calculated by the total number of atoms, the atomic percentage of nitrogen in the coating is 20-30%, the atomic percentage of carbon is 30-50%, the atomic percentage of titanium is 20-30%, and the sum of the atomic percentages of the three elements is ≤100%; In the coating, the total content of N, C and Ti is ≥ 95%; calculated based on the total weight of the coating; In the coating, a ratio of a volume V1 of the equiaxed crystal structure to a volume V0 of the coating (V1 / V0) is ≥ 60%.
2. The method for preparing a titanium carbonitride coating on a surface of 316L stainless steel according to claim 1, characterized in that: The pretreatment process is: cleaning, sandblasting, cleaning and drying are performed on the surface of the 316L stainless steel substrate in sequence.
3. The method for preparing a titanium carbonitride coating on a surface of 316L stainless steel according to claim 1, characterized in that: The first auxiliary gas is nitrogen and / or hydrogen, and the second auxiliary gas is nitrogen.
4. A titanium carbonitride coating on the surface of 316L stainless steel prepared by the preparation method according to claim 1, characterized in that: The coating is attached to the surface of 316L stainless steel, and is composed of titanium carbonitride micron grains, the micron grains are block-shaped, and the average length of the micron grains is 1-3 μm, the average width is 1-4 μm, and the average thickness is 1-15 μm.
5. The titanium carbonitride coating on the surface of 316L stainless steel according to claim 4, characterized in that: The micron grains have an average length of 1-2.5 μm, an average width of 1-2 μm, and an average thickness of 6-8 μm.
6. The titanium carbonitride coating on the surface of 316L stainless steel according to claim 4, characterized in that: Calculated by the total number of atoms, the atomic percentage of nitrogen in the coating is 20-30%, the atomic percentage of carbon is 30-50%, the atomic percentage of titanium is 20-30%, and the sum of the atomic percentages of the three elements is ≤100%.
7. The titanium carbonitride coating on the surface of 316L stainless steel according to claim 6, characterized in that: The micron grains are equiaxed grains.