Catalyst composition for decomposition of ammonia

By using cobalt-based catalysts, Co3O4/CeO2 composite oxides containing cobalt, cerium and barium, the problems of high cost of ruthenium-based catalysts and unstable carbon nanotube carriers in the existing technology are solved, and efficient and stable ammonia decomposition of hydrogen is achieved. production, reducing the risk of catalyst deactivation.

CN115485233BActive Publication Date: 2024-10-18SAUDI ARABIAN OIL CO +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180012415.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-03
Publication Date
2024-10-18
Estimated Expiration
2041-02-03

AI Technical Summary

Technical Problem

Among the existing methods of decomposing ammonia, the cost of ruthenium-based catalysts is high and the carbon nanotube carrier is unstable at high temperatures, leading to problems such as catalyst deactivation and methanation reactions, making it difficult to achieve efficient and economical hydrogen production from ammonia decomposition.

Method used

A cobalt-based catalyst is used, containing 15-70% cobalt, 5-45% cerium and 0.4-0.5% barium. It is prepared by coprecipitation and impregnation methods to form a Co3O4/CeO2 composite oxide catalyst and is activated above 500°C. Metal sites for catalyzing ammonia decomposition reactions.

Benefits of technology

Efficient and stable ammonia decomposition is achieved, the ammonia conversion rate is greater than 95%, catalyst deactivation is avoided, costs are reduced, and catalytic performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115485233B_ABST
    Figure CN115485233B_ABST
Patent Text Reader

Abstract

A method for decomposing ammonia to produce hydrogen, the method comprising the steps of introducing an ammonia stream into a reactor, wherein the ammonia stream comprises ammonia, wherein the reactor comprises a cobalt-based catalyst, wherein the cobalt-based catalyst comprises between 15 wt% and 70 wt% cobalt, between 5 wt% and 45 wt% cerium, and between 0.4 wt% and 0.5 wt% barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen; contacting the ammonia in the ammonia stream with the cobalt-based catalyst, wherein the cobalt-based catalyst is capable of catalyzing an ammonia decomposition reaction; catalyzing the ammonia decomposition reaction in the presence of the cobalt-based catalyst to decompose the ammonia to produce hydrogen; and removing a product stream from the reactor, the product stream comprising hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application discloses compositions and methods related to catalyst preparations. Specifically, compositions and methods of catalyst preparations for decomposing ammonia are disclosed. Background Art

[0002] Ammonia is a high-volume commercial chemical, with global production of 176 million tons in 2014. Due to the high volumetric energy density of ammonia (108 kg-H2 / m 3 NH3 and 8.6 bar) and gravimetric energy density (17.8 wt%), so it has become an efficient hydrogen carrier. In addition, ammonia is easy to store and transport. These advantages make ammonia suitable for on-site production of COx-free hydrogen by catalytic decomposition, which can be used in fuel cells or hydrogen-powered vehicles.

[0003] Current methods for decomposing ammonia include using ruthenium catalysts on carbon nanotube supports (Ru / CNTs). Ruthenium-based catalysts are too expensive for large-scale commercialization of such processes. In addition, CNTs as supports lack stability. Under the reaction conditions required for ammonia decomposition, such as temperatures of about 450 degrees Celsius (°C), methanation reactions may occur on carbon-based catalysts. Methanation reactions may involve hydrogenation of carbon in the carbon-based catalyst, resulting in deactivation of the catalyst. Summary of the invention

[0004] The present application discloses compositions and methods related to catalyst preparations. Specifically, compositions and methods of catalyst preparations for decomposing ammonia are disclosed.

[0005] In a first aspect, a method for decomposing ammonia to produce hydrogen is provided. The method comprises the steps of introducing an ammonia stream into a reactor, wherein the ammonia stream comprises ammonia, wherein the reactor comprises a cobalt-based catalyst, the cobalt-based catalyst comprising between 15% and 70% by weight of cobalt, between 5% and 45% by weight of cerium, and between 0.4% and 0.5% by weight of barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen. The method also comprises contacting the ammonia in the ammonia stream with the cobalt-based catalyst, wherein the cobalt-based catalyst is capable of catalyzing an ammonia decomposition reaction, catalyzing the ammonia decomposition reaction in the presence of the cobalt-based catalyst to cause the ammonia to decompose to produce hydrogen, and removing a product stream from the reactor, the product stream comprising hydrogen.

[0006] In certain aspects, the method further comprises the steps of introducing a hydrogen flow into the reactor, increasing the temperature in the reactor to 500°C at a rate of 2°C per minute, and maintaining the temperature in the reactor at 500°C for at least 3 hours to activate the metal sites on the cobalt-based catalyst, and then introducing an ammonia flow into the reactor.

[0007] In some aspects, the temperature in the reactor is in the range between 250° C. and 700° C. In some aspects, the pressure in the reactor is in the range between 1 bar and 40 bar. In some aspects, the product stream also includes nitrogen. In some aspects, the conversion of ammonia is greater than 95%.

[0008] In a second aspect, a method for preparing a cobalt-based catalyst is provided. The method comprises the steps of dissolving cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and cerium nitrate hexahydrate (Ce(NO3)2·6H2O) in distilled water, adding a sodium carbonate (Na2CO3) solution, maintaining the solution until cobalt carbonate and cerium carbonate precipitate out of the solution, filtering the cobalt carbonate and cerium carbonate at a pressure of about 0.4 bar, washing the filtered cobalt carbonate and cerium carbonate with cold distilled water until the pH is 7 to produce a washed precipitate, and drying the washed precipitate at a temperature of 100°C for at least 8 hours. to produce a dried precipitate, calcining the dried precipitate at a temperature of 550°C for at least 3 hours to produce a black powder, wherein the temperature of the calcination step is capable of burning out the carbonate to produce a black powder comprising a Co3O4 / CeO2 composite oxide, impregnating the black powder with an aqueous solution of barium nitrate (Ba(NO3)2) to produce a precursor, drying the precursor at a temperature of 120°C for at least 8 hours to produce a dried precursor, and calcining the dried precursor at a temperature of 550°C for at least 3 hours to produce a cobalt-based catalyst.

[0009] In certain aspects, the method further comprises the steps of: crushing the cobalt-based catalyst to produce cobalt-based catalyst particles, sieving the particles and collecting the cobalt-based catalyst particles having a diameter between 0.3 mm and 0.5 mm. In certain aspects, the cobalt-based catalyst comprises between 15 wt % and 70 wt % cobalt, between 5 wt % and 45 wt % cerium, and between 0.4 wt % and 0.5 wt % barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen.

[0010] In a third aspect, a cobalt-based catalyst composition is provided. The cobalt-based catalyst composition comprises between 15 wt% and 70 wt% cobalt, between 5 wt% and 45 wt% cerium, and between 0.4 wt% and 0.5 wt% barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen.

[0011] In some aspects, the cobalt-based catalyst composition comprises cobalt oxide. In some aspects, the cobalt-based catalyst composition comprises cerium oxide. In some aspects, cobalt is an active metal. In some aspects, cerium can be used as a carrier and promoter. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] These and other features, aspects and advantages of the scope of the present application will be better understood through the following specification, claims and drawings. However, it is to be noted that the drawings illustrate only several embodiments and are therefore not to be considered limiting of the scope as other equally effective embodiments may be admitted.

[0013] Figure 1 is a TEM image of cobalt-containing catalyst particles.

[0014] Figure 2 is a TEM image of cobalt-based catalyst particles.

[0015] Figure 3 is a graph comparing a commercially available 3%Ru-10%K / CaO catalyst and a 0.5%Ba / 80%Co-20%Ce cobalt-based catalyst at 1 bar and 40 bar.

[0016] Figure 4 is a graph showing the effect of promoters (Ca, Al, Ce) in cobalt-containing catalysts.

[0017] Figure 5 is a graph showing the effect of the first Co to Ce ratio.

[0018] Figure 6 is a graph showing the effect of secondary promoters (Ba, Cs, K, Na) in cobalt-containing catalysts.

[0019] Figure 7 is a graph showing the effect of the amount of barium in a cobalt-containing catalyst.

[0020] Figure 8 is a graph showing the effect of barium on 80% Co-20% Ce. DETAILED DESCRIPTION

[0021] Although the scope will be described using several embodiments, it should be understood that those of ordinary skill in the relevant art will understand that many examples, variations and modifications of the apparatus and methods described herein are within the scope of the present application. Therefore, the described embodiments are set forth without loss of generality and do not constitute limitations on the embodiments. Those skilled in the art understand that the scope includes all possible combinations and uses of the specific features described in the specification.

[0022] Described herein are compositions and methods relating to catalyst formulations for decomposing ammonia to produce nitrogen and hydrogen. The catalyst formulation is a cobalt-based catalyst. Advantageously, the cobalt-based catalyst can be used to produce hydrogen on demand from ammonia. Advantageously, the cobalt-based catalyst is stable, exhibits consistent catalytic performance, and no deactivation is observed over long periods of use.

[0023] As used throughout, "absent" means that a composition or method does not include, does not contain, does not have.

[0024] As used throughout, "promoter" refers to a component of a catalyst that improves the performance of the catalyst in a catalytic reaction but has little or no catalytic effect alone. Promoters can affect the structure and physical properties of the catalyst. Promoters can interact with the active components of the catalyst and change the chemical action of the active components on the catalytic substance.

[0025] The cobalt-based catalyst may comprise a cobalt component, a cerium component and a barium component. The cobalt-based catalyst is a composite oxide. The catalytic activity of the cobalt-based catalyst depends on the active metal sites, which are related to the dispersion of the active metal components.

[0026] The cobalt component is the active metal component of the cobalt-based catalyst. The ammonia decomposition reaction occurs on the cobalt component. The cobalt component can exist as cobalt metal or as the cobalt oxide in the form of Co3O4. The content of cobalt in the cobalt-based catalyst can be between about 15 wt % and 70 wt %, or between 25 wt % and 70 wt %, or between 30 wt % and 70 wt %, or between 35 wt % and 70 wt %, or between 40 wt % and 70 wt %. No matter the cobalt component exists as cobalt metal or as cobalt oxide, the amount of cobalt metal is the same. The particle size of the cobalt component can be in the range between 20 nanometers (nm) and 30nm.

[0027] The cerium component can serve the dual purpose of a promoter and a carrier. The cerium component prevents agglomeration of cobalt, thus increasing the dispersibility of the cobalt particles in the cobalt-based catalyst. The cobalt dispersion can be about 5%. The cerium component can be highly dispersed, which can reduce the size of the cobalt particles. Figure 1 and Figure 2 The dispersion of cerium can be observed in the transmission electron microscopy (TEM) images of MgO2, which show cerium agglomerates between and on top of the cobalt component particles. Figure 2 A single cerium atom on a particle of the cobalt component is shown. The cerium component may include cerium oxide in the form of CeO2. The cerium content of the cobalt-based catalyst may be in the range between 5 wt% and 45 wt%, or in the range between 7 wt% and 42 wt%.

[0028] The barium component can be used as a promoter. The cerium component can be doped with the barium component. The addition of the barium component can disperse additional cobalt, which improves the catalytic performance of the cobalt-based catalyst compared to a catalyst without barium. The barium component can improve the catalytic performance. At lower temperatures, the addition of the barium component can increase the conversion rate of ammonia. The barium component can include barium. The content of barium in the cobalt-based catalyst can be in the range of between 0.4 wt % and 0.5 wt %. When the content of barium in the catalyst is greater than 1 wt %, the activity of the ammonia decomposition reaction drops sharply. When the content of barium in the catalyst is greater than about 9 wt %, the barium will destroy the catalytic performance of the cobalt and prevent the occurrence of the ammonia decomposition reaction.

[0029] The cobalt-based catalyst may have a cobalt to cerium molar ratio in the range of 50 to 95. In at least one embodiment, the cobalt-based catalyst has a cobalt to cerium mass ratio of 63 / 67 and contains 0.5 wt% barium, the balance being oxygen. In at least one embodiment, the cobalt-based catalyst contains 41.4 wt% cobalt, 23.5 wt% cerium, 0.5 wt% barium, and the balance being oxygen. In at least one embodiment, the cobalt-based catalyst has a cobalt to cerium mass ratio of 67 / 37 and contains 0.5 wt% barium, the balance being oxygen.

[0030] Cobalt-based catalysts can be prepared by a combined method of coprecipitation and impregnation. Advantageously, the use of coprecipitation increases the cobalt loading and improves the physical and structural parameters of the final catalyst, which increases the activity of the final catalyst.

[0031] In the coprecipitation stage, cobalt carbonate and cerium carbonate are obtained by coprecipitation. In the first step, a certain amount of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and cerium nitrate hexahydrate (Ce(NO3)2·6H2O) are dissolved in distilled water and heated to produce a saline solution. The amount of cobalt nitrate hexahydrate can be selected based on the amount of water, the desired composition of the final catalyst, and the desired ratio of cobalt to cerium. The amount of cerium nitrate hexahydrate can be selected based on the amount of water, the desired composition of the cobalt-based catalyst, and the desired ratio of cobalt to cerium. Then a sodium carbonate (Na2CO3) solution is slowly added to the saline solution. The amount of sodium carbonate added is greater than the amount of cobalt nitrate hexahydrate and cerium nitrate hexahydrate, so that cobalt carbonate and cerium carbonate are precipitated. Sodium will not be incorporated into the catalyst. Cobalt carbonate and cerium carbonate are precipitated from the solution. The obtained cobalt carbonate and cerium carbonate are filtered under a reduced pressure of about 0.4 bar and washed with distilled water until the pH of the washing water is 7. Washing with distilled water can ensure the removal of sodium carbonate. In the drying step, the washed precipitate is dried at a temperature of 100°C for at least 8 hours to produce a dried precipitate. In the calcining step, the dried precipitate is then calcined at a temperature of 550°C for about 3 hours. The carbonates are burned out in the calcining step to produce a black powder containing the composite oxide Co3O4 / CeO2. In the impregnation stage, the black powder is impregnated with an aqueous solution of barium nitrate (Ba(NO3)2) to produce a precursor. The amount of barium nitrate can be selected to achieve the desired amount of barium. In the drying step, the precursor is dried at a temperature of 120°C for at least 8 hours to produce a dried precursor. In the calcining step, the dried precursor is calcined at a temperature of about 550°C for about 3 hours to produce a cobalt-based catalyst. The cobalt-based catalyst can be crushed and sieved. The size of the cobalt-based catalyst can be between 0.3 mm and 0.5 mm.

[0032] Prior to use in the ammonia decomposition reaction, the cobalt-based catalyst may be reduced in a reduction step. The temperature of the cobalt-based catalyst may be raised to a temperature of about 500° C. at a rate of 2° C. per minute over a period of about 3 hours under flowing hydrogen at atmospheric pressure. The flow rate of hydrogen may be about 25 milliliters per minute. The reduction step may produce active metal sites in the cobalt-based catalyst. The reduction step may be performed in a reactor containing the cobalt-based catalyst.

[0033] Cobalt-based catalysts can be used to catalyze the ammonia decomposition reaction occurring according to Formula 1.

[0034] 2NH3→N2+3H2 reaction 1

[0035] Cobalt-based catalysts can be used for the selective decomposition of ammonia in reaction 1.

[0036] The ammonia decomposition reaction is a balance-controlled reaction. The cobalt-based catalyst can be loaded in the reactor. The reactor can be any type of container that can accommodate the catalyst and support the operating conditions of the ammonia decomposition reaction. Examples of reactors include fixed reactors and fluidized bed reactors. An ammonia stream containing ammonia can be introduced into a reactor containing a cobalt-based catalyst. The ammonia decomposition reaction can be catalyzed on the cobalt-based catalyst. The ammonia decomposition reaction can produce hydrogen and nitrogen. The gas can be removed from the reactor as a product stream. The product stream can include nitrogen, hydrogen, ammonia and combinations thereof.

[0037] The conversion of ammonia over the cobalt-based catalyst may be greater than 95%, or greater than 97%, or greater than 99%. In at least one embodiment, the conversion may be 100%. In at least one embodiment where the conversion is 100%, ammonia may not be present in the product stream. The ammonia decomposition reaction may occur at a temperature between about 250° C. and 700° C., or between 250° C. and 550° C., or between 350° C. and 550° C. The ammonia decomposition reaction may occur at a pressure between 1 bar and 40 bar, or between 1 bar and 30 bar, or between 1 bar and 20 bar, or between 1 bar and 10 bar.

[0038] Cobalt-based catalysts do not contain precious metals. Cobalt-based catalysts do not contain manganese, nickel, copper, iron, ruthenium, palladium, platinum, magnesium, strontium, yttrium, lanthanum, neodymium, samarium, europium, gadolinium and erbium. Cobalt-based catalysts do not contain perovskite structures.

[0039] Example

[0040] Example 1. Cobalt-based catalysts were prepared by coprecipitation and impregnation methods.

[0041] In the coprecipitation stage, cobalt carbonate and cerium carbonate are obtained by coprecipitation. Sodium carbonate is used as a precipitant. Between 1.82 grams (g) and 3.46 g of Co(NO3)2·6H2O and between 0.27 g and 2.71 g of Ce(NO3)2·6H2O ( St. Louis, Missouri) was dissolved in distilled water and heated to 0.0125 mol of cobalt and cerium for each compound. Then, 2.65 g of Na2CO3 ( The coprecipitate obtained containing cobalt carbonate and cerium carbonate was filtered under a reduced pressure of about 0.4 bar and washed several times with cold distilled water until the pH of the collected washing water was equal to 7.

[0042] The washed precipitate was dried at 100° C. overnight and calcined at 550° C. for 3 hours to produce cobalt oxide or Co 3 O 4 / CeO 2 composite oxide as a black powder.

[0043] Then, a barium nitrate aqueous solution ( St. Louis, Missouri) was impregnated with black powder to achieve a nominal concentration of 0.5 wt % in the precursor.

[0044] The resulting precursor was then dried at 120°C overnight and thereafter calcined at 550°C for 3 hours to produce a cobalt-based catalyst.

[0045] The cobalt-based catalyst was crushed and sieved to obtain cobalt-based catalyst particles having a size of 0.3 mm to 0.5 mm.

[0046] The structural and chemical analysis of the cobalt-based catalysts was performed, and the catalytic performance was then evaluated. The structural parameters were determined by N2 and CO chemisorption, X-ray diffraction, XPS and HR-TEM. Figure 1 and Figure 2 The high resolution TEM images shown show that the cobalt and cerium are nanoparticle sized and well dispersed. Figure 1 Shown is a TEM image of a cobalt-based catalyst comprising 63% Co, 37% Ce after a reduction step. Figure 2 Shown is a TEM image of a cobalt based catalyst containing 0.5% Ba / 63% Co, 37% Ce after a reduction step. Figure 2 The barium also appeared to be well dispersed.The chemical composition was obtained using ICP.

[0047] Example 2. A cobalt-based catalyst prepared according to the method of claim 1 contains 0.5% Ba / 80% Co-20% Ce. The catalytic performance of the cobalt-based catalyst was tested in a fixed bed reactor (PID technology) at temperatures between 250°C and 550°C and pressures of 1 bar, 20 bar and 40 bar. For comparison, the catalytic performance of a commercial catalyst of 3% Ru-10% K / CaO was tested using the same method. The results can be found in Figure 3 The best catalytic performance is achieved at 1 bar and temperatures above 500 °C.

[0048] Example 3. Example 3 is a test of various cobalt-containing catalysts to show the efficacy of certain promoters compared to commercially available ruthenium-based catalysts. The catalysts were prepared according to the coprecipitation method described in Example 1, with salts of other promoter metals (such as aluminum and calcium) replacing cerium nitrate hexahydrate. Figure 4 A comparison of cobalt-containing catalysts with promoters including aluminum, calcium and cerium with cobalt catalysts and commercially available ruthenium-based catalysts is shown. The results show that the cobalt-containing catalyst with a cerium promoter has the best catalytic performance. Figure 5 Results for different cerium contents in cobalt are shown. The results show that catalysts containing 80% Co-20% Ce, 90% Co-10% Ce, and 95% Co-5% Ce behave similarly, outperforming 70% Co-30% Ce and 50% Co-50% Ce. Figure 6 A comparison of cobalt with cerium and other promoters including barium, cesium, potassium and sodium is shown. The results show that the catalyst containing barium as an additional promoter has the highest catalytic performance. Figure 7 The results show that the cobalt-based catalyst has the best catalytic performance. Figures 4 to 7 In each of the Figures, the best catalytic performance is observed at temperatures above 500°C. Figure 8 The catalytic performance results are shown for a cobalt-containing catalyst having 80% Co and 20% Ce, with and without Barium.

[0049] Although the embodiments herein have been described in detail, it should be understood that various changes, substitutions and alterations can be made thereto without departing from the spirit and scope of these embodiments. Therefore, the scope should be determined by the following claims and their appropriate legal equivalents.

[0050] Unless otherwise stated, various elements described herein may be used in combination with all other elements described herein.

[0051] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0052] Optional or alternatively means that the subsequently described event or circumstance may or may not occur. The description includes instances where the event or circumstance occurs and instances where it does not occur.

[0053] Ranges herein may be expressed as from about one particular value, and / or to about another particular value. When such a range is expressed, it is to be understood that another embodiment is from the one particular value and / or to the other particular value, and all combinations within the range.

[0054] Throughout this application, where patents or publications are cited, the disclosures of these references are intended to be incorporated by reference in their entireties into this application in order to more fully describe the state of the art to which the embodiments pertain, unless such citations are inconsistent with the statements herein.

[0055] As used herein and in the appended claims, the words "comprising," "having," and "including" and all grammatical variations thereof are each intended to have an open, non-limiting meaning that does not exclude additional elements or steps.

[0056] As used herein, terms such as "first" and "second" are arbitrarily designated and are intended only to distinguish between two or more components of a device. It should be understood that the words "first" and "second" are not used for other purposes and are not part of the component names or descriptions, nor do they necessarily define the relative positions or locations of the components. In addition, it should be understood that the mere use of the terms "first" and "second" does not require the existence of any "third" component, although such a possibility is contemplated within the scope of the present embodiment.

Claims

1. A method for decomposing ammonia to produce hydrogen, the method comprising the following steps: introducing a hydrogen gas stream into the reactor; The temperature in the reactor is raised to 500° C. at a rate of 2° C. per minute, wherein the reactor contains a cobalt-based catalyst comprising: between 15% and 70% by weight of cobalt, between 5% and 45% by weight of cerium, and between 0.4 wt % and 0.5 wt % barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen; maintaining the temperature in the reactor at 500° C. for at least 3 hours to activate metal sites on the cobalt-based catalyst; introducing an ammonia stream into a reactor, wherein the ammonia stream comprises ammonia; contacting ammonia in the ammonia stream with the cobalt-based catalyst to decompose ammonia when the temperature in the reactor is in the temperature range of 250° C. to 700° C., wherein the cobalt-based catalyst is capable of catalyzing an ammonia decomposition reaction; catalyzing the ammonia decomposition reaction in the presence of the cobalt-based catalyst to decompose ammonia to produce hydrogen; and A product stream is withdrawn from the reactor, said product stream comprising hydrogen.

2. The process according to claim 1, wherein the pressure in the reactor is in the range between 1 bar and 40 bar.

3. The method of claim 1, wherein the product stream further comprises nitrogen.

4. The process according to any one of claims 1 to 3, wherein the conversion of ammonia to hydrogen is greater than 95%.

5. A method for preparing a cobalt-based catalyst, the cobalt-based catalyst comprising: between 15% and 70% by weight cobalt; between 5 wt % and 45 wt % cerium; and between 0.4% and 0.5% by weight of barium, wherein the remainder of the weight of the cobalt-based catalyst is oxygen; The method comprises the following steps: Dissolve cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and cerium nitrate hexahydrate (Ce(NO3)2·6H2O) in distilled water; Add sodium carbonate (Na2CO3) solution; maintaining the solution until the cobalt carbonate and cerium carbonate precipitate from the solution; filtering cobalt carbonate and cerium carbonate at a pressure of 0.4 bar; washing the filtered cobalt carbonate and cerium carbonate with cold distilled water until the pH of the wash water is 7 to produce a washed precipitate; drying the washed precipitate at a temperature of 100° C. for at least 8 hours to produce a dried precipitate; calcining the dried precipitate at a temperature of 550° C. for at least 3 hours to produce a black powder, wherein the temperature of the calcining step is capable of burning out carbonates to produce a black powder comprising a Co3O4 / CeO2 composite oxide; impregnating the black powder with an aqueous solution of barium nitrate (Ba(NO3)2) to produce a precursor; drying the precursor at a temperature of 120° C. for at least 8 hours to produce a dried precursor; and The dried precursor was calcined at a temperature of 550° C. for at least 3 hours to produce a cobalt-based catalyst.

6. The method according to claim 5, further comprising the step of pulverizing the cobalt-based catalyst to produce cobalt-based catalyst particles; sieving the particles; and Cobalt-based catalyst particles with diameters between 0.3 mm and 0.5 mm were collected.

7. A cobalt-based catalyst composition prepared according to the method of claim 5 or 6.

8. The cobalt-based catalyst composition of claim 7, comprising cobalt oxide.

9. The cobalt-based catalyst composition of claim 7, comprising cerium oxide.

10. A cobalt-based catalyst composition according to claim 7 or claim 8, wherein the cobalt is the active metal.

11. A cobalt-based catalyst composition according to claim 7 or claim 9, wherein the cerium can function as a support and a promoter.

Citation Information

Patent Citations

  • Catalyst for ammonia decomposition, process for producing same, and method of treating ammonia

    CN102159314A

  • Catalyst for production of hydrogen and process for producing hydrogen using the catalyst, and catalyst for combustion of ammonia, process for producing the catalyst, and method for combustion of ammonia using the catalyst

    CN102348504A

  • Ni / CGO and Ni-Ru / CGO based pre-reforming catalysts formulation for methane rich gas production from diesel processing for fuel cell applications

    CN105377426A

  • Preparation of alkali metal or alkaline earth metal promoted Co-based catalysts for the water gas shift reaction

    KR1020180092831A

  • Catalyst for production of hydrogen and process for producing hydrogen using the catalyst, and catalyst for combustion of ammonia, process for producing the catalyst, and method for combustion of ammonia using the catalyst

    WO2010107065A1