A polyamide / polyolefin mixed matrix nanofiltration membrane and preparation method thereof
By using reverse diffusion to grow UIO-66 nanoparticles in situ in polyamide/polyolefin mixed matrix nanofiltration membranes, the 'trade-off' effect between water permeability and salt rejection of traditional nanofiltration membranes is solved. The problem of membrane fouling is eliminated, the effect of high flux and high rejection rate is achieved, the preparation process is simplified, and the cost is reduced.
Patent Information
- Application Number
- CN202211213941.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-30
AI Technical Summary
Traditional polyamide nanofiltration membranes have a 'trade-off' effect between water permeability and salt rejection, and are prone to membrane fouling problems during use, and their preparation is complex and costly.
A polyamide/polyolefin mixed matrix nanofiltration membrane based on in-situ growth of UIO-66 by reverse diffusion is used to load metal zirconium ions on the polyolefin porous support layer to form a dense polyamide active layer, and in the organic ligand machine solvent In-situ synthesis of UIO-66 nanoparticles was carried out through reverse diffusion to prepare high-performance nanofiltration membranes.
Nanofiltration membranes that achieve high flux and high rejection rates simplify the preparation process, reduce costs, and have huge application potential in wastewater treatment, hard water softening, seawater desalination, etc.
Smart Images

Figure HDA0003875584290000011 
Figure HDA0003875584290000012 
Figure HDA0003875584290000021
Abstract
Description
(I) Technical field
[0001] The invention relates to a polyamide / polyolefin mixed matrix nanofiltration membrane based on reverse diffusion in-situ growth of UIO-66 and a preparation method thereof. (II) Background technology
[0002] With the rapid development of human science and technology and the rapid increase in industrial production, the living standards of human beings have been greatly improved. However, it has also brought about various problems such as environmental pollution and water shortage. Membrane technology has the advantages of high separation efficiency, simple operation and no pollution, and has great application potential in wastewater treatment, hard water softening, seawater desalination, etc. Nanofiltration membrane, as one of the membrane classifications, is popular because of its selectivity for monovalent and polyvalent ions, low operating pressure and relatively low cost.
[0003] At present, polyamide (PA) nanofiltration membrane has become the mainstream of nanofiltration membrane development due to its polyamide active layer, which has good water permeability and salt retention. Traditional polyamide nanofiltration membrane is composed of a bottom membrane support layer and a polyamide active layer. The nanofiltration membrane support layer usually adopts an ultrafiltration membrane, which is made of polyester non-woven fabric and ultrafiltration layers such as polysulfone, polyethersulfone, and polyvinylidene fluoride. The current ultrafiltration membrane is heavily dependent on foreign imports, and the preparation is complicated and the cost is high. Domestic polyolefin (PE) has been widely used as a lithium battery separator. Its thickness (5-50um) and pore size (10-70nm) make it very suitable for nanofiltration membrane to replace the traditional two-layer ultrafiltration membrane as a support layer, and it is cheap and easy to obtain, which is conducive to large-scale continuous production. However, PA nanofiltration membrane still faces many difficulties in the application process, such as the "trade-off" effect between water permeability and salt retention and the problem of membrane pollution during use. Therefore, in order to further improve the performance of PA nanofiltration membrane, the modification and optimization of nanofiltration membrane has become the focus of current research. Among them, the introduction of MOFs nanoparticles into the polyamide active layer can greatly improve the water permeability and selectivity of the membrane. However, the traditional MOFs mixed matrix nanofiltration membrane is prone to problems such as nanoparticle agglomeration and phase interface defects during the preparation process. (III) Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of existing nanofiltration membranes and provide a polyamide / polyolefin mixed matrix nanofiltration membrane based on reverse diffusion in-situ growth of UIO-66 and a preparation method thereof.
[0005] The technical solution adopted by the present invention is:
[0006] A polyamide / polyolefin mixed matrix nanofiltration membrane comprises a polyolefin porous support layer, a polyamide active layer and in-situ grown and attached UIO-66 nanoparticles, and is prepared by the following method: firstly, metal zirconium ions are loaded on the polyolefin porous support layer, then interfacial polymerization is performed to generate a dense polyamide active layer, and finally, the membrane is immersed in an organic ligand organic solvent to in-situ synthesize UIO-66 nanoparticles by reverse diffusion to obtain the polyamide / polyolefin mixed matrix nanofiltration membrane.
[0007] The UIO-66 nanoparticles are prepared by self-assembly of metal zirconium ion monomers and organic ligand monomers, wherein the metal zirconium ion monomers are one or more of zirconium chloride, zirconium sulfate, and zirconium nitrate, and the organic ligand monomers are one or more of terephthalic acid, 2-aminoterephthalic acid, 2,5-dihydroxyterephthalic acid, 2,5-dimercaptoterephthalic acid, 2-hydroxyterephthalic acid, and 1,3,5-tricarboxylic acid.
[0008] The polyolefin porous support layer is made of one or more of polyethylene and polypropylene.
[0009] The present invention also relates to a method for preparing the polyamide / polyolefin mixed matrix nanofiltration membrane, the method comprising:
[0010] (1) immersing the polyolefin porous support layer in a solution containing a metal zirconium ion monomer to attach metal salt ions on the surface of the polyolefin porous support layer; the metal zirconium ion monomer is one or more of zirconium chloride, zirconium sulfate, and zirconium nitrate;
[0011] (2) immersing the membrane formed in step (1) in an organic phase solution of an acyl chloride monomer to form an organic phase liquid layer on the surface of the membrane; the acyl chloride monomer is one or more of isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, trimesoyl chloride, and polyvalent aromatic sulfonyl chloride;
[0012] (3) contacting the membrane formed in step (2) with an aqueous solution containing amine monomers, and forming a polyamide active layer on the surface of the PE support layer through an interfacial polymerization reaction, thereby obtaining an initial nanofiltration membrane doped with metal salt ions; the amine monomers are one or more of piperazine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, ethylenediamine, hexamethylenediamine, 1,4-butylenediamine, 4,4-diaminodiphenyl ether, 4,4-diaminodiphenylmethane, o-benzylamine, 1,2-propylenediamine, 1,3-propylenediamine, 2,4-diaminotoluene, 1,2-cyclohexanediamine, 4,5-dichloro-o-phenylenediamine, diethylenetriamine, and mesitylenetriamine;
[0013] (4) In situ growth of UIO-66 on the initial nanofiltration membrane doped with metal salt ions formed in step (3) in a solution containing organic ligands is performed, and the membrane is cleaned to obtain the polyamide / polyolefin mixed matrix nanofiltration membrane; the organic ligand monomer is one or more of terephthalic acid, 2-aminoterephthalic acid, 2,5-dihydroxyterephthalic acid, 2,5-dimercaptoterephthalic acid, 2-hydroxyterephthalic acid, and 1,3,5-tricarboxylic acid.
[0014] Specifically, the step (1) is: pouring an organic phase solution containing metal zirconium ion monomers onto the surface of the polyolefin porous support layer for a contact time of 0.1 to 15 minutes, then pouring it out and air-drying it; the mass fraction of metal zirconium ion monomers in the organic phase solution is 0.005 to 0.1%, and the solvent is one or more of water, ether, acetone, dimethylformamide, ethanol, and acetonitrile.
[0015] Specifically, the step (2) is: covering the surface of the membrane obtained in step (1) with a layer of organic phase solution of acyl chloride monomer, which is continued for 0.1 to 15 minutes and then poured out, wherein the mass fraction of acyl chloride monomer in the organic phase solution is 0.01 to 1%, and the solvent is one or more of n-hexane, cyclohexane, toluene, benzene, and ethyl acetate.
[0016] Specifically, the step (3) comprises: covering the surface of the membrane obtained in step (2) with a layer of aqueous solution containing amine monomers, which is applied for 0.1 to 15 minutes and then poured out, heat-treated at 40 to 80° C. for 5 to 30 minutes, and then washed with an organic solvent; the mass fraction of the amine monomers in the aqueous solution is 0.01 to 1%.
[0017] In the step (4), the mass fraction of the organic ligand monomer in the organic ligand solution is 0.005-0.1%, and the solvent is one or more of acetone, ethanol, acetonitrile, and N,N-dimethylformamide.
[0018] Preferably, the reaction temperature of step (4) is in the range of 25 to 50° C. (more preferably 25° C.), and the reaction time is 12 to 48 hours.
[0019] Preferably, the cleaning solvent in step (4) is acetone.
[0020] The beneficial effects of the present invention are mainly reflected in: the polyamide / polyolefin mixed matrix nanofiltration membrane of the present invention has high flux and high retention rate, and the preparation method is simple and feasible with low cost, and has great application potential in wastewater treatment, hard water softening, seawater desalination, etc. (IV) Description of the drawings
[0021] Figure 1 It is the separation performance diagram of nanofiltration membrane (water flux and Na2SO4 retention rate);
[0022] Figure 2 This is a scanning electron microscopy image of the PA / PE mixed matrix nanofiltration membrane based on reverse diffusion in situ growth of UIO-66;
[0023] Figure 3 It is the principle diagram and device diagram of the membrane performance evaluation device. (V) Specific implementation methods
[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:
[0025] The preparation environment of all the initial nanofiltration membranes in the examples is: temperature of 25° C., humidity of 40%, and normal pressure.
[0026] A PA / PE mixed matrix nanofiltration membrane based on reverse diffusion in-situ growth of UIO-66 is composed of a PE membrane as a support layer and a polyamide layer containing UIO-66 nanoparticles as a functional layer. The specific steps of the preparation method are as follows:
[0027] (1) Pour a metal salt monomer solution on the surface of the PE film support layer for 4 minutes, then pour out the solution and air dry it. The metal salt monomer is zirconium chloride, the solvent is acetone, and the concentration of zirconium chloride is 0.00625wt%.
[0028] (2) Covering the surface of the PE film support layer obtained in step (1) with a layer of organic phase solution for 4 minutes, and then discarding it. The monomer is trimesoyl chloride, the organic phase solvent is n-hexane, and the concentration of trimesoyl chloride is 0.075wt%;
[0029] (3) Pour the aqueous phase solution on the surface of the PE membrane support layer for 1 minute, then pour off the solution, and heat treat at 60°C for 15 minutes to obtain an initial nanofiltration membrane; wherein the monomer is piperazine. The mass fraction of the aqueous phase monomer is 0.1wt%, and the pH of the aqueous phase solution is 10.
[0030] (4) The membrane obtained in step (3) is cleaned with acetone and then modified with a solution containing an organic ligand at 25°C / 50°C for 24h / 48h to in-situ grow UIO-66. After cleaning, a nanofiltration membrane grown in situ by UIO-66 is obtained; wherein the organic ligand is 2-aminoterephthalic acid with a mass fraction of 0.00625wt%, the solvent is acetone, and the polyamide nanofiltration membrane is a circle with a diameter of 6cm.
[0031] Embodiment 1:
[0032] (1) The PE film support layer (Shanghai Enjie New Materials Technology Co., Ltd.) was immersed in a zirconium chloride acetone solution (0.00625 wt%) for 4 min, the solution was poured out, and the film was dried.
[0033] (2) immersing the obtained membrane in a 0.075 wt % benzyl chloride n-hexane solution for 4 min;
[0034] (3) subjecting the obtained membrane to interfacial polymerization with a 0.1 wt % piperazine aqueous solution for 1 min to form a polyamide layer doped with zirconium ions on the surface of the PE membrane support layer, heat-treating for 15 min, and washing with an acetone solution;
[0035] (4) The obtained membrane was placed in a 2-aminoterephthalic acid acetone solution for 24 hours at 25°C to in situ grow UIO-66, and then cleaned with acetone to obtain a nanofiltration membrane based on in situ grown UIO-66 nanoparticles.
[0036] The nanofiltration membrane obtained in Example 1 was analyzed and tested:
[0037] The nanofiltration membrane prepared in this example was loaded into a membrane performance evaluation device (Hangzhou Saifei Membrane Separation Technology Co., Ltd., SA model). Figure 3 , Experimental conditions: room temperature, 0.6MPa, pre-pressure 1h, 1g / L Na2SO4 salt solution; Experimental results: water flux: 6.6Lm -2 h -1 bar -1 , Na2SO4 retention rate: 75%.
[0038] Embodiment 2:
[0039] (1) immersing the PE membrane support layer in a zirconium chloride acetone solution (0.00625 wt%) for 4 min, then pouring out the solution and air-drying the membrane;
[0040] (2) immersing the obtained membrane in a 0.075 wt % benzyl chloride n-hexane solution for 4 min, then pouring out the solution to form an organic phase liquid layer on the surface;
[0041] (3) subjecting the obtained membrane to interfacial polymerization with a 0.1 wt % piperazine aqueous solution for 1 min to form a polyamide layer doped with zirconium ions on the surface of the PE membrane support layer, heat-treating for 15 min, and washing with an acetone solution;
[0042] (4) The obtained membrane was placed in a 2-aminoterephthalic acid acetone solution for 48 hours at 25°C to in-situ grow UIO-66, and then cleaned with acetone to obtain a nanofiltration membrane based on in-situ grown UIO-66 nanoparticles. The scanning electron microscopy image is shown in Figure 2 From the figure, we can see the nodular structure of polyamide, and we can also see obvious particles on the surface of the membrane.
[0043] The nanofiltration membrane obtained in Example 2 was analyzed and tested:
[0044] The performance test method of the membrane is the same as that of Example 1. The experimental results are as follows: Water flux: 6.8 Lm -2 h -1 bar -1 , Na2SO4 retention rate: 77%.
[0045] Embodiment 3:
[0046] (1) immersing the PE membrane support layer in a zirconium chloride acetone solution (0.00625 wt%) for 4 min, then pouring out the solution and air-drying the membrane;
[0047] (2) immersing the obtained membrane in a 0.075 wt % benzyl chloride n-hexane solution for 4 min, then pouring out the solution to form an organic phase liquid layer on the surface;
[0048] (3) subjecting the obtained membrane to interfacial polymerization with a 0.1 wt % piperazine aqueous solution for 1 min to form a polyamide layer doped with zirconium ions on the surface of the PE membrane support layer, heat-treating for 15 min, and washing with an acetone solution;
[0049] (4) The obtained membrane was placed in a 2-aminoterephthalic acid acetone solution at 50°C for 24 hours to in-situ grow UIO-66, and then cleaned with acetone to obtain a nanofiltration membrane based on in-situ grown UIO-66 nanoparticles.
[0050] The nanofiltration membrane obtained in Example 3 was analyzed and tested:
[0051] The performance test method of the membrane is the same as that of Example 1. The experimental results are as follows: Water flux: 7.8 Lm -2 h -1 bar -1 , Na2SO4 retention rate: 47%.
[0052] Embodiment 4 (comparative example):
[0053] (1) immersing a polysulfone (PSF) membrane support layer in a 0.2 wt % piperazine aqueous solution for 4 min, then pouring out the solution to form an aqueous phase layer on the surface;
[0054] (2) The organic phase liquid layer and 0.1 wt % benzyl chloride n-hexane solution were subjected to interfacial polymerization for 1 min to form a polyamide layer on the surface of the polysulfone ultrafiltration membrane support layer, which was heat treated for 15 min and then stored in deionized water.
[0055] The performance test method of the membrane is the same as that of Example 1. The experimental results are as follows: Water flux: 3.3 Lm -2 h -1 bar -1, Na2SO4 retention rate: 97%.
[0056] The separation performance diagrams (water flux and Na2SO4 retention rate) of the nanofiltration membranes of Examples 1-4 are shown in Figure 1 , see Table 1 for specific data:
[0057] Table 1: Water flux and Na2SO4 retention rate of nanofiltration membrane in the embodiment of the present invention
[0058] Example <![CDATA[Pure water flux (Lm -2 h -1 bar -1 )]]> <![CDATA[Na2SO4 rejection rate (%)]]> Example 1 6.6 75 Example 2 6.8 77 Example 3 7.8 47 Example 4 3.3 97
[0059] It can be seen that compared with the traditional polyamide nanofiltration membrane with a polysulfone ultrafiltration membrane as the support layer (Example 4), the water flux of the polyamide / polyolefin mixed matrix nanofiltration membrane (Examples 1, 2, 3) prepared in the present invention is significantly increased (2 times), and the salt retention rate is slightly reduced.
Claims
1. A method for preparing a polyamide / polyolefin mixed matrix nanofiltration membrane, the method comprising: (1) immersing the polyolefin porous support layer in a solution containing metal zirconium ion monomers to attach metal salt ions on the surface of the support layer; The metal zirconium ion monomer is one or more of zirconium chloride, zirconium sulfate, and zirconium nitrate; (2) immersing the membrane formed in step (1) in an organic phase solution of an acyl chloride monomer to form an organic phase liquid layer on the surface thereof; the acyl chloride monomer is one or more of isophthaloyl chloride, terephthaloyl chloride, phthaloyl chloride, trimesoyl chloride, and polyaromatic sulfonyl chloride; (3) contacting the membrane formed in step (2) with an aqueous solution containing amine monomers, and forming a polyamide active layer on the surface of the PE support layer through an interfacial polymerization reaction, thereby obtaining an initial nanofiltration membrane doped with metal salt ions; the amine monomers are one or more of piperazine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, ethylenediamine, hexamethylenediamine, 1,4-butylenediamine, 4,4-diaminodiphenyl ether, 4,4-diaminodiphenylmethane, o-benzylamine, 1,2-propylenediamine, 1,3-propylenediamine, 2,4-diaminotoluene, 1,2-cyclohexanediamine, 4,5-dichloro-o-phenylenediamine, diethylenetriamine, and mesitylenetriamine; (4) In situ growth of UIO-66 on the initial nanofiltration membrane doped with metal salt ions formed in step (3) in a solution containing organic ligands, and cleaning to obtain the polyamide / polyolefin mixed matrix nanofiltration membrane; the organic ligand monomer is one or more of terephthalic acid, 2-aminoterephthalic acid, 2,5-dihydroxyterephthalic acid, 2,5-dimercaptoterephthalic acid, 2-hydroxyterephthalic acid, and 1,3,5-tricarboxylic acid.
2. The method according to claim 1, characterized in that The step (1) comprises: pouring an organic phase solution containing metal zirconium ion monomers onto the surface of the polyolefin porous support layer for a contact time of 0.1 to 15 minutes, then pouring it out and air-drying it; the mass fraction of metal zirconium ion monomers in the organic phase solution is 0.005 to 0.1%, and the solvent is one or more of water, ether, acetone, dimethylformamide, ethanol, and acetonitrile.
3. The method according to claim 1, characterized in that The step (2) comprises: covering the surface of the membrane obtained in the step (1) with a layer of organic phase solution of acyl chloride monomer, which is continued for 0.1 to 15 minutes and then poured out, wherein the mass fraction of acyl chloride monomer in the organic phase solution is 0.01 to 1%, and the solvent is one or more of n-hexane, cyclohexane, toluene, benzene, and ethyl acetate.
4. The method according to claim 1, characterized in that The step (3) comprises: covering the surface of the membrane obtained in the step (2) with a layer of aqueous solution containing amine monomers, which is kept for 0.1 to 15 minutes and then poured out, heat-treated at 40 to 80° C. for 5 to 30 minutes, and then washed with an organic solvent; the mass fraction of the amine monomers in the aqueous solution is 0.01 to 1%.
5. The method according to claim 1, characterized in that In the step (4), the mass fraction of the organic ligand monomer in the organic ligand solution is 0.005-0.1%, and the solvent is one or more of acetone, ethanol, acetonitrile, and N,N-dimethylformamide.
6. The method according to claim 1, characterized in that The reaction temperature of step (4) is in the range of 25 to 50° C., and the reaction time is in the range of 12 to 48 hours.