A high-speed continuous casting process for producing 25Mn4 steel

By adjusting parameters such as crystallizer vibration frequency, electromagnetic stirring frequency, and cooling water volume in the high-speed continuous casting process of 25Mn4 steel, the problems of unstable production efficiency and product quality in the existing technology are solved, and high-speed continuous casting is achieved. efficiency improvement and quality assurance.

CN115502345BActive Publication Date: 2024-10-29NANJING IRON & STEEL CO LTD +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202210824267.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-10-29
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

The existing technology is difficult to improve the production efficiency of high-speed continuous casting of 25Mn4 steel while ensuring product quality, resulting in extended production cycles, increased equipment loss and energy consumption, and unstable product quality.

Method used

Using a high-speed continuous casting process including converter, refining furnace, crystallizer, tension leveler, secondary cooling and air cooling, the flow of molten steel is controlled by adjusting parameters such as the vibration frequency of the crystallizer, electromagnetic stirring frequency and cooling water volume. field and cooling methods to ensure the quality and production efficiency of the billet at high drawing speeds.

Benefits of technology

The drawing speed of 25Mn4 steel has been increased by more than 20%, the production efficiency has been improved, and the quality of the casting billet has been guaranteed, with no steel leakage accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003745783620000021
    Figure BDA0003745783620000021
Patent Text Reader

Abstract

The invention discloses a high-speed continuous casting process for producing 25Mn4 steel, which mainly comprises the following processes: the continuous casting speed is 2.4-3.0 m / min, the heat exchange of cooling water of a crystallizer is 1.0-3.0 MW; the specific water volume of a secondary cooling zone is 0.7-0.9 L / kg, the number of secondary cooling zones is 4-7, and the secondary cooling zones are composed of full water cooling and air-water cooling, and the outlet target temperatures of the zones are 1050° C. for a full roll zone, 1020° C. for a zone 1, 1000° C. for a zone 2, and 980° C. for a zone 3; the crystallizer vibrates, and the vibration frequency is 210-250 times / min; the stirring frequency of an electromagnetic stirrer in the crystallizer is 6-8 Hz; the electromagnetic stirring frequency at the end of solidification is 7-50 Hz; the pulling speed of 25Mn4 steel-related products produced according to the production process of the invention is increased by more than 20%, the production efficiency is improved, and the quality of the obtained ingot is qualified without steel leakage accidents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-speed continuous casting process for steel, in particular to a high-speed continuous casting process for producing 25Mn4 steel. Background Art

[0002] At present, with the advancement of the dual carbon policy, energy conservation and emission reduction in the steel industry have received unprecedented attention. Continuous casting is a link between steelmaking and steel rolling, which affects the production efficiency and energy consumption of steel products. The developed high-speed continuous casting technology has been widely used in ordinary steel, and has reached the level of saving or eliminating the energy consumption of heating furnaces.

[0003] For alloy steel, increasing the continuous casting speed can shorten the production cycle, reduce equipment loss and labor costs, reduce heat consumption and emissions, and improve product quality stability. However, how to ensure the product quality of alloy steel at high casting speed is still a technical difficulty.

[0004] Due to the improvement of steelmaking efficiency and the shortening of smelting cycle, the furnace and machine are not well matched during the production process, and the continuous casting production pressure is huge. At present, the drawing speed of 25Mn4 series pipe steel is 2.0-2.2m / min. Although the Chinese patent with application number 201911027407.2 discloses a continuous casting production process for preparing low-carbon, high-sulfur, high-oxygen free-cutting steel at a high drawing speed, this patent only provides a direct production solution for high-drawing speed continuous casting of low-carbon, high-sulfur, high-oxygen free-cutting steel. Different steel grades, different billet shapes and different products have different characteristics and production technical conditions. Therefore, it is necessary to provide a process suitable for the production of 25Mn4 and other series pipe steels according to the composition characteristics of 25Mn4 steel. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a high-speed continuous casting process for producing 25Mn4 steel, which can increase the continuous casting speed while ensuring production quality.

[0006] Technical solution: The high-speed continuous casting process for producing 25Mn4 steel described in the present invention includes a converter, a refining furnace, a ladle, a tundish, a crystallizer, a straightening machine, secondary cooling, air cooling and cutting. The specific process includes:

[0007] (1) The molten steel is produced by the converter and refined by the refining furnace. The molten steel is filled in the ladle and injected into the tundish through the long nozzle. The superheat of the molten steel in the tundish is controlled at 15-25°C. The molten steel is injected into the round billet crystallizer with a nominal diameter of 150-180 mm. Medium carbon steel high-speed casting crystallizer protection slag is used, and the thickness of the liquid slag layer is 13-15 mm.

[0008] (2) The continuous casting speed is 2.4-3.0 m / min; the slag consumption is 0.35-0.5 kg / t steel; the heat exchange of the cooling water of the crystallizer is 1.0-3.0 MW; the crystallizer is vibrated while the billet is drawn, the vibration frequency is 210-250 times / min, the amplitude is within ±4 mm, and the deflection rate does not exceed 0.2; and the stirring frequency of the electromagnetic stirrer in the crystallizer is 6-8 Hz and the current is 380-500 A;

[0009] (3) The specific water volume of the secondary cooling zone is 0.7-0.9L / kg, and the number of secondary cooling zones is 4-7, which are the full roll zone and secondary cooling zone 1, zone 2 and zone 3 from top to bottom. The full roll zone is fully water-cooled and the number is 1. The other zones are air-water cooled. The number of air-water cooled zones is 1-2. The cooling method is dynamic secondary cooling control based on the target temperature. The outlet target temperatures of each zone are 1050℃ for the full roll zone, 1020℃ for zone 1, 1000℃ for zone 2 and 980℃ for zone 3. The temperature of each zone is allowed to deviate by ±20℃.

[0010] (4) Electromagnetic stirring is performed at the end of solidification in the air cooling zone, and the stirring frequency of the electromagnetic stirrer is 7 to 50 Hz and the current is 550 to 850 A;

[0011] (5) After cutting, the continuous casting billet is slowly cooled for more than 24 hours.

[0012] Furthermore, the crystallizer uses an immersed water nozzle, and the water nozzle outlet can be in the form of 1 hole, 2 holes, 3 holes, 4 holes, 5 holes, etc., and the water nozzle insertion depth is 140-180mm; the deeper the water nozzle insertion depth is, the more the resistance of the molten steel to the upward flow stream is increased, so that the crystallizer liquid level fluctuation is more stable and the risk of slag rolling is reduced.

[0013] Furthermore, the crystallizer is 0.7-1.2 m long and made of pure copper, deoxidized phosphorus copper, or chromium zirconium copper. The inner surface is plated with Cr or Ni, and the inner cavity has a continuous inverted taper of 0.5-2.0% from top to bottom.

[0014] In one step, the cooling water volume of the crystallizer is 140-170m 3 / h, the water temperature difference is 5-9℃, the outer surface of the crystallizer is cooled by water, the water gap width is 3-4mm, and the water flow rate is not less than 6m / s; faster water flow rate and higher heat exchange efficiency can be achieved under the same total water volume.

[0015] Furthermore, the high-drawing speed protective slag is a protective slag with high melting rate, medium alkalinity, low viscosity and low melting temperature performance, which can achieve efficient and uniform heat transfer and lubrication.

[0016] Furthermore, the number of air-cooling zones in step (3) increases with the increase of the drawing speed. When the drawing speed is maximum, the secondary cooling zone is composed of one full-water-cooled full-roll zone and six air-water cooling zones, specifically two zones 1, two zones 2 and two zones 3. The increase in the number of secondary cooling zones is beneficial to the control of the surface temperature and solidification process of the ingot at high drawing speed, and the method of multiple groups of cooling zones + enhanced cooling is adopted to achieve efficient heat transfer at high drawing speed.

[0017] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the drawing speed of 25Mn4 steel and other related products produced according to the production process of the present invention is increased by more than 20%, the production efficiency is improved, and the quality of the resulting ingot is qualified without steel leakage accidents. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is further described below.

[0019] According to the steps of the above method, a specific example of producing 25Mn4 steel is provided below.

[0020] 25Mn4 steel composition, wt%, as shown in Table 1

[0021]

[0022] Table 1

[0023] The present invention mainly provides a high-speed continuous casting process for 25Mn4 steel. 25Mn4 steel belongs to medium-carbon alloy steel. The specific composition of molten steel is as described in Table 1, which can meet the production requirements of different round billet sections of 150-180 mm. The larger the diameter of the billet section, the corresponding drawing speed should be appropriately reduced within the range of 2.4 m / min-3.0 m / min to ensure the quality of the billet. The drawing speed of 150 mm round billet is 2.7-3.0 m / min, the drawing speed of 160 mm round billet is 2.7-2.9 m / min, the drawing speed of 170 mm round billet is 2.5-2.8 m / min, and the drawing speed of 180 mm round billet is 2.4-2.6 m / min. Among other parameters, the heat exchange value of crystallizer water and the total specific water volume of the secondary cooling zone are both positively correlated with the drawing speed. The parameter values ​​are appropriately adjusted as the drawing speed changes. In order to meet the requirements of 25Mn4 steel under high drawing speed, the drawing speed of 150 mm round billet is 2.7-3.0 m / min, the drawing speed of 160 mm round billet is 2.7-2.9 m / min, the drawing speed of 170 mm round billet is 2.5-2.8 m / min, and the drawing speed of 180 mm round billet is 2.4-2.6 m / min. 4. Solidification characteristics of steel. A larger electromagnetic stirring frequency and current are used at the end of solidification, which enhances the shrinkage compensation of the molten steel at the end and ensures the internal quality of the ingot. The larger the diameter of the ingot section, the higher the required end stirring frequency. In the present invention, the electromagnetic stirring frequency of the crystallizer is relatively large. At the crystallizer, combined with the deeper insertion depth of the immersion nozzle, a high-frequency electric stirring and a large current are used. This not only meets the equiaxed crystal rate requirements and uniform distribution of equiaxed crystals of different ingot sections of 150-180 mm, but also ensures the stability of the flow field of the molten steel in the crystallizer, achieving a better metallurgical effect. The stirring frequency in the crystallizer increases with the increase of the pulling speed. The vibration frequency is high and the amplitude is low. A shallower ingot vibration mark depth can be obtained under the condition of a higher pulling speed, and the control of the surface quality of the ingot is more accurate. The vibration frequency is also adjusted in a positive correlation with the pulling speed. The parameters of each process in the whole process cooperate with each other to ensure the production quality of 25Mn4 steel at a high pulling speed. Therefore, the following embodiments and comparative examples are provided for specific explanation.

[0024] Example 1

[0025] The process flow of producing 25Mn4 steel 150mm round billets by high-speed continuous casting is as follows: converter → refining furnace → ladle → tundish → crystallizer → straightening machine → secondary cooling → air cooling → cutting.

[0026] The first step is to check the accuracy of the equipment before production. The arc deviation of the crystallizer and the foot roller is controlled within ±1.0mm, the centering deviation of the crystallizer nozzle is within ±3mm, the nozzle patency rate is 100%, and the straightening machine and cutting machine are fault-free. The converter produces molten steel that meets the continuous casting requirements. The molten steel is refined by the refining furnace to ensure that the temperature, composition, deoxidation degree and purity of the molten steel meet the quality requirements. The molten steel is contained and transported by the ladle, and the ladle is placed on the turntable. The turntable receives the refined molten steel. The ladle rotates and starts to move above the crystallizer, and the molten steel is poured into the tundish through the long water nozzle. The tundish injects the molten steel into the crystallizer through the immersed water nozzle. The water nozzle outlet is 1 hole, the water nozzle insertion depth is 180mm, the cross-sectional diameter of the upper mouth of the crystallizer is 161mm, and the molten steel is injected into the round billet crystallizer with a nominal cross-sectional diameter of 150mm.

[0027] In the second step, when the molten steel level reaches two-thirds of the total height of the crystallizer, the straightening machine is started, and the vibration is turned on and protective slag is added. The protective slag is a protective slag with high melting rate, medium alkalinity, low viscosity and low melting temperature. The thickness of the liquid slag layer is 15mm, and the protective slag consumption is 0.35kg / t. Protective pouring is used throughout the process to prevent secondary oxidation of the molten steel. The initial pulling speed is set to 0.5-0.8m / min, and then the pulling speed is increased to the working pulling speed at a range of 0.6-1.2m / min per minute. The non-steady-state crystallizer liquid level fluctuation is controlled at ±6mm, and the steady-state fluctuation is controlled at ±3mm. After pouring, the molten steel in the crystallizer condenses with the ingot rod. Through the pulling and straightening machine, the ingot with the liquid core is continuously pulled out from the lower mouth of the crystallizer along with the ingot rod. The pulling speed is 3.0m / min, the inverted taper of the crystallizer is 1.1%, the length of the crystallizer is 1.0m, the crystallizer is cooled by water outside, the water temperature difference is 8.6℃, the water gap width is 4mm, the cooling water flow rate is 15m / s, and the heat exchange of the cooling water in the crystallizer is 1.2MW; the crystallizer is vibrated at the same time when the billet is drawn, and the vibration frequency of the crystallizer is set as a linear function that increases with the pulling speed, the vibration frequency is 243 times / min, the amplitude is ±3mm, and the deflection rate is 0.1; the electromagnetic stirring of the crystallizer is turned on at normal pulling speed, the stirring current intensity is 380A, and the frequency is 8Hz;

[0028] In the third step, the ingot exiting the lower mouth of the crystallizer is subjected to secondary cooling. The secondary cooling water volume is 0.9L / kg, and there are 7 secondary cooling zones, namely, full roll zone, secondary cooling zone 1, zone 2 and zone 3. The full roll zone is fully water-cooled, and the number is 1; the number of secondary cooling zones 1, 2 and 3 are two respectively, which are air-water cooling; the cooling method is dynamic secondary cooling control based on the target temperature, and the outlet target temperatures of each zone are 1050℃ for the full roll zone, 1020℃ for zone 1, 1000℃ for zone 2, 980℃ for zone 3, and a deviation of ±20℃ is allowed.

[0029] In the fourth step, the air cooling zone is subjected to terminal electromagnetic stirring, with a stirring current of 550A and a frequency of 7Hz;

[0030] The fifth step is that the ingot enters the cutting position and is flame cut. When cutting, the ingot is stacked and slowly cooled for 24 hours.

[0031] Quality inspection results: The continuous casting billet was corroded according to GBT 226-2015 "Acid Etching Test Method for Macrostructure and Defects of Steel" and rated according to YB / T 153-2015 "Grading Chart for Macrostructure Defects of High-quality Structural Steel Continuous Casting Billets". The internal center shrinkage rating was 0.5, the center segregation rating was 0.5, and there were no obvious defects on the surface.

[0032] Example 2

[0033] The 25Mn4 steel 160mm round billet was produced by high-speed continuous casting. The process flow was basically the same as that of Example 1, except that the casting speed was 2.8m / min, the thickness of the liquid slag layer was 14mm, the length of the crystallizer was 1.0m, the crystallizer was cooled by water outside, the water temperature difference was 7.8℃, the water gap width was 3.9mm, the cooling water flow rate was 12m / s, and the heat exchange of the crystallizer cooling water was 1.6MW; the casting was carried out simultaneously with The crystallizer was vibrated with a frequency of 232 times / min, an amplitude of ±3mm, and a deviation rate of 0.1; the crystallizer was electromagnetically stirred with a stirring current of 420A and a frequency of 7Hz; the protective slag consumption was 0.38kg / t; the secondary cooling water volume was 0.86L / kg, and the number of secondary cooling zones was 6, namely, the full roller zone, one zone 1, two zones 2, and two zones 3; the air cooling zone was subjected to terminal electromagnetic stirring with a stirring current of 620A and a frequency of 16Hz; the offline stack was slowly cooled for 36 hours during cutting.

[0034] Quality inspection results: the inspection standard is the same as that in Example 1, there are no obvious defects on the surface of the continuous casting billet, the internal center shrinkage rating is 1.0, and the center segregation rating is 1.0.

[0035] Example 3

[0036] The 25Mn4 steel 170mm round billet is produced by high-speed continuous casting. The process is basically the same as that in Example 1, except that the casting speed is 2.6m / min, the thickness of the liquid slag layer is 14mm, the length of the crystallizer is 0.9m, the crystallizer is cooled by water outside, the water temperature difference is 7.5℃, the water gap width is 3.6mm, the cooling water flow rate is 12.0m / s, and the heat exchange of the crystallizer cooling water is 2.4MW; while casting Crystallizer vibration was adopted with a vibration frequency of 223 times / min, an amplitude of ±3.2mm, and a deviation rate of 0.1; crystallizer electromagnetic stirring was adopted with a stirring current intensity of 450A and a frequency of 7Hz; protective slag consumption was 0.4kg / t; the secondary cooling water volume was 0.78L / kg, and the number of secondary cooling zones was 5, namely, a full roller zone, one zone 1, one zone 2, and two zones 3; terminal electromagnetic stirring was carried out in the air cooling zone with a stirring current of 760A and a frequency of 30Hz; the offline stacking was slow-cooled for 48h during cutting.

[0037] Quality inspection results: the inspection standard is the same as that in Example 1, there are no obvious defects on the surface of the continuous casting billet, the internal center shrinkage rating is 1.0, and the center segregation rating is 1.0.

[0038] Example 4

[0039] The 25Mn4 steel 180mm round billet is produced by high-speed continuous casting. The process is basically the same as that of Example 1, except that the casting speed is 2.4m / min, the thickness of the liquid slag layer is 13mm, the inverted taper of the crystallizer is 1.1%, the length of the crystallizer is 0.9m, the crystallizer is cooled by water outside, the water temperature difference is 7.5℃, the water gap width is 3.2mm, the cooling water flow rate is 10m / s, and the heat exchange of the crystallizer cooling water is 3.0MW. ; Crystallizer vibration is used during billet drawing, with a vibration frequency of 210 times / min, an amplitude of ±3.5mm, and a deviation rate of 0.1; crystallizer electromagnetic stirring is used, with a stirring current intensity of 500A and a frequency of 6Hz; protective slag consumption is 0.42kg / t; the secondary cooling water volume is 0.7L / kg, and the number of secondary cooling zones is 4, namely, the full roller zone, one zone 1, one zone 2 and one zone 3; terminal electromagnetic stirring is carried out in the air cooling zone, with a stirring current of 850A and a frequency of 50Hz; when cutting, the offline stack is slowly cooled for 72h.

[0040] Quality inspection results: the inspection standard is the same as that in Example 1, there are no obvious defects on the surface of the continuous casting billet, the internal center shrinkage rating is 1.5, and the center segregation rating is 1.5.

[0041] Comparative Example 1

[0042] 25Mn4 steel 150mm round billets are produced by high-speed continuous casting. The process production process is basically the same as that in Example 1, with the following parameters: the continuous casting speed is 3.5m / min, the heat exchange capacity of the crystallizer cooling water is 3.4MW, the crystallizer vibration frequency is 260 times / min, the amplitude is ±5mm, the crystallizer electromagnetic stirring frequency is 8Hz, the current is 380A, the secondary cooling water volume is 1.0L / kg, the end electromagnetic stirring frequency is 6Hz, and the current is 520A.

[0043] Quality inspection results: The inspection standard is the same as that in Example 1. Longitudinal cracks and transverse cracks appear on the surface of the continuous casting billet. The central shrinkage cavity rating is 2.5, and the central porosity rating is 3.0.

[0044] Comparative Example 2

[0045] The conventional casting speed continuous casting method is used to produce 25Mn4 steel 150mm round billets. The process flow is basically the same as that of Example 1, except that the continuous casting speed is 2.0m / min, the crystallizer cooling water volume is 120m 3 / h, the heat exchange rate of crystallizer cooling water is 0.8MW, the crystallizer vibration frequency is 280 times / min, the amplitude is ±3mm, the crystallizer electromagnetic stirring frequency is 3Hz, the current is 300A, the secondary cooling water volume is 0.6L / kg, the terminal electromagnetic stirring frequency is 5Hz, and the current is 340A.

[0046] Quality inspection results: the inspection standard is the same as that in Example 1, there are no obvious defects on the surface of the continuous casting billet, the central shrinkage rating is 1.5, and the central porosity rating is 1.0.

[0047] The drawing speed used in Comparative Example 2 is lower than that of Example 1. The quality test results thereof are slightly worse than those of Example 1. In addition, the drawing speed is slower, the production time is longer than that of Example 1, and the efficiency is lower.

Claims

1. A high-speed continuous casting process for producing 25Mn4 steel, the process flow is: converter → refining furnace → ladle → tundish → crystallizer → straightening machine → secondary cooling → air cooling → cutting, characterized in that: Specific processes include: (1) After the molten steel is produced by the converter and refined by the refining furnace, the molten steel is held in the ladle and injected into the tundish through the long nozzle. The superheat of the molten steel in the tundish is 15-25°C. The molten steel is injected into the round billet crystallizer with a nominal diameter of 150-180 mm. Medium carbon steel high-speed casting crystallizer protection slag is used; (2) The continuous casting speed is 2.4-3.0 m / min; the heat exchange capacity of the cooling water of the crystallizer is 1.0-3.0 MW; the crystallizer is vibrated while the billet is drawn, the vibration frequency is 210-250 times / min, the amplitude is within ±4 mm, and the deflection rate does not exceed 0.2; and the stirring frequency of the electromagnetic stirrer in the crystallizer is 6-8 Hz and the current is 380-500 A; (3) The specific water volume of the secondary cooling zone is 0.7-0.9L / kg, and the number of secondary cooling zones is 4-7, which are the foot roll zone and secondary cooling zones 1, 2 and 3 from top to bottom. The foot roll zone is fully water-cooled and the number is 1. The other zones are air-water cooled. The number of air-water cooled zones is 1-2. The cooling method is dynamic secondary cooling control based on the target temperature. The outlet target temperatures of each zone are 1050℃ for the foot roll zone, 1020℃ for zone 1, 1000℃ for zone 2 and 980℃ for zone 3. The temperature deviation of each zone is ±20℃. (4) Electromagnetic stirring is performed at the end of solidification in the air cooling zone, and the stirring frequency of the electromagnetic stirrer is 7 to 50 Hz and the current is 550 to 850 A; (5) After cutting, the continuous casting billet is slowly cooled for more than 24 hours.

2. The high-speed continuous casting process according to claim 1, characterized in that: The crystallizer uses an immersed water nozzle, the water nozzle outlet is 1 hole, 2 holes, 3 holes, 4 holes or 5 holes, and the water nozzle insertion depth is 140-180mm.

3. The high-speed continuous casting process according to claim 2, characterized in that: The crystallizer has a length of 0.7-1.2 m, is made of pure copper, deoxidized phosphorus copper, or chromium zirconium copper, has a Cr or Ni layer plated on the inner surface, and has a continuous inverted taper of 0.5-2.0% from top to bottom.

4. The high-speed continuous casting process according to claim 1, characterized in that: The cooling water volume of the crystallizer is 140-170m 3 / h, the water temperature difference is 5-9℃, the outer surface of the crystallizer is cooled by water, the water gap width is 3-4mm, and the water flow rate is not less than 6m / s.

5. The high-speed continuous casting process according to claim 1, characterized in that: The number of air-water cooling zones in step (3) increases as the pulling speed increases.

Citation Information

Patent Citations

  • Continuous casting production technology for high-casting-speed preparation of low-carbon high-sulfur high-oxygen free-cutting steel

    CN110722119A

  • Continuous casting columnar crystallizer small square blank and its columnar crystal control method

    CN101147966A

  • Electric furnace continuous casting short process production method of oil well pipe billets

    CN101653822A

  • Continuous casting production process for improving quality of free cutting steel casting blank

    CN102303108A

  • Continuous-cast P91-steel round pipe billet and production process thereof

    CN102527956A