A method for preparing a modified carbon nanotube film with low infrared emissivity

Through KOH solution activation and high-temperature heat treatment of the carbon nanotube film, defects are formed to reduce the infrared emissivity, solving the problem of high infrared emissivity of carbon materials, achieving multi-band low infrared emissivity, and improving infrared stealth performance.

CN115504459BActive Publication Date: 2024-10-01NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211345481.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-01
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The infrared emissivity of carbon materials is high, which limits its application in infrared stealth technology. The existing reduction methods are complex and inefficient.

Method used

By activating the carbon nanotube film in a KOH solution and performing heat treatment in an argon atmosphere, defects are formed to reduce the infrared emissivity. The specific steps include soaking, washing, vacuum drying and high-temperature calcination, resulting in the conductivity and dielectric properties of the carbon nanotubes. The electrical constant decreases, thereby reducing the infrared emissivity.

Benefits of technology

The infrared emissivity of the modified carbon nanotube film is significantly reduced, to 0.473 and 0.493 in the 3-5 μm and 8-14 μm bands respectively, achieving multi-band low infrared emissivity and improving the material's stealth performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115504459B_ABST
    Figure CN115504459B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a modified carbon nanotube film with low infrared emissivity, which comprises the following steps: first activating the carbon nanotube film with a KOH solution, and then heat treating the carbon nanotube film in an argon atmosphere after activation to obtain the modified carbon nanotube film. The infrared emissivity of the modified carbon nanotube film prepared by the present invention can be as low as 0.473 in the 3-5 μm band, and as low as 0.493 in the 8-14 μm band, which greatly reduces the infrared emissivity of the carbon nanotube film before modification, so that the carbon nanotube film has low infrared emissivity in multiple bands.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a modified carbon nanotube film with low infrared emissivity. Background Art

[0002] With the continuous development of military technology, infrared stealth is of vital importance in the military field, and the key to infrared stealth technology is to reduce the infrared radiation intensity of the target aircraft. According to Boltzmann's law, to reduce the intensity of infrared radiation, it is mainly necessary to reduce the surface temperature and infrared emissivity of the material. The method of reducing the surface temperature of the target usually requires the introduction of more equipment or materials, which is more complicated in actual situations. It can be seen that the use of low infrared emissivity materials to reduce the infrared emissivity of the target is the most effective method to achieve infrared stealth of the target. At present, due to its unique structure and physical and chemical properties, carbon materials generally have a high infrared emissivity, so there are relatively few studies on stealth, especially infrared stealth. Summary of the invention

[0003] Purpose of the invention: The purpose of the present invention is to provide a method for modifying a carbon nanotube film, which can significantly reduce the infrared emissivity of the modified carbon nanotube film.

[0004] Technical solution: The method for preparing the modified carbon nanotube film with low infrared emissivity described in the present invention is specifically as follows: the carbon nanotube film is first activated with a KOH solution, and then heat-treated in an argon atmosphere after activation to obtain a modified carbon nanotube film.

[0005] The thickness of the carbon nanotube film is 20 to 40 μm, and the carbon nanotubes in the carbon nanotube film are arranged in a three-dimensional network structure.

[0006] The activation by KOH solution specifically refers to: immersing the carbon nanotube film in a KOH solution, wherein the concentration of the KOH solution is 1.5-2 mol / L.

[0007] Among them, the soaking time is not less than 24h.

[0008] The immersed carbon nanotube film is taken out, washed with water until it becomes neutral, and then vacuum dried at 50-60°C.

[0009] The heat treatment temperature is 500-550°C, the heat treatment time is 3-4h, and the heating rate is 5-5.5°C / min.

[0010] The KOH on the carbon nanotubes begins to decompose into alkali metal oxides at 500-550 degrees. At this temperature, the alkali metal oxides react with carbon, causing the carbon to be released in the form of oxides, which etch the surface of the carbon to form defects. As the calcination temperature increases further, I D / IG As the value increases, the defects increase. The increase in defects will change the bond length of the valence bond between atoms and change the type of hybrid orbitals of some carbon atoms. The changes in bond length and orbital change the electrical properties of the defective area of ​​the carbon nanotube. The defects form electron wave scattering centers on the carbon surface. Such centers affect the transfer of electrons, and ultimately reduce the conductivity of the carbon nanotubes. At the same time, defects will also affect the dielectric constant. Too many defects will significantly reduce the dielectric constant. The imaginary part of the dielectric constant is positively correlated with the conductivity. As the imaginary part decreases, the conductivity decreases, thereby increasing the infrared emissivity.

[0011] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the infrared emissivity of the modified carbon nanotube film prepared by the present invention can be as low as 0.473 in the 3-5 μm band, and as low as 0.493 in the 8-14 μm band, which greatly reduces the infrared emissivity of the carbon nanotube film before modification, so that it has low infrared emissivity in multiple bands. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is the SEM image of carbon nanotube film;

[0013] Figure 2 The mechanical properties photo of the modified carbon nanotube film in Example 2;

[0014] Figure 3 1 is the Raman spectra of the carbon nanotube film before modification and the carbon nanotube film after modification in Example 2;

[0015] Figure 4 This is the Raman spectrum of the modified carbon nanotube film in Example 3;

[0016] Figure 5 This is the Raman spectrum of the modified carbon nanotube film in Example 4;

[0017] Figure 6 The Joule thermal performance of the modified carbon nanotube film in Example 2;

[0018] Figure 7 The shielding effectiveness of the modified carbon nanotube film in Example 2;

[0019] Figure 8 Comparison of infrared emissivity of different carbon nanotube films. DETAILED DESCRIPTION

[0020] Example 1

[0021] A method for activating carbon nanotubes comprises the following steps:

[0022] (1) A 50 mm*50 mm carbon nanotube film (thickness before modification was 24 μm) was immersed in a 2 mol / L KOH solution and stirred at room temperature for 24 h;

[0023] (2) The immersed carbon nanotube film was washed with deionized water for several times until it became neutral, and then dried at 50° C. for 24 h to obtain an activated carbon nanotube film with a thickness of 24 μm.

[0024] Example 2

[0025] The method for preparing the modified carbon nanotube film with low infrared emissivity of the present invention comprises the following steps:

[0026] (1) A 50 mm*50 mm carbon nanotube film (thickness before modification was 24 μm) was immersed in a 2 mol / L KOH solution and stirred at room temperature for 24 h;

[0027] (2) washing the immersed carbon nanotube film with deionized water several times until it becomes neutral, and then drying it at 50° C. for 24 h to obtain an activated carbon nanotube film;

[0028] (3) The activated carbon nanotube film was calcined in a tubular furnace at a calcination temperature of 500°C, a holding time of 4 h, and a heating rate of 5°C / min to obtain a carbon nanotube film -500 with a thickness of 28 μm.

[0029] Example 3

[0030] The method for preparing the modified carbon nanotube film with low infrared emissivity of the present invention comprises the following steps:

[0031] (1) A 50 mm*50 mm carbon nanotube film (thickness before modification was 24 μm) was immersed in a 2 mol / L KOH solution and stirred at room temperature for 24 h;

[0032] (2) washing the immersed carbon nanotube film with deionized water several times until it becomes neutral, and then drying it at 50° C. for 24 h to obtain an activated carbon nanotube film;

[0033] (3) The activated carbon nanotube film was calcined in a tubular furnace at a calcination temperature of 700°C, a holding time of 4 hours, and a heating rate of 5°C / min to obtain a carbon nanotube film -700 with a thickness of 28 μm.

[0034] Example 4

[0035] The method for preparing the modified carbon nanotube film with low infrared emissivity of the present invention comprises the following steps:

[0036] (1) A 50 mm*50 mm carbon nanotube film (thickness before modification was 24 μm) was immersed in a 2 mol / L KOH solution and stirred at room temperature for 24 h;

[0037] (2) washing the immersed carbon nanotube film with deionized water several times until it becomes neutral, and then drying it at 50° C. for 24 h to obtain an activated carbon nanotube film;

[0038] (3) The activated carbon nanotube film was calcined in a tubular furnace at a calcination temperature of 900°C, a holding time of 4 hours, and a heating rate of 5°C / min to obtain a carbon nanotube film -900 with a thickness of 37 μm.

[0039] When the carbon nanotube film is only activated by KOH solution, its thickness hardly changes, but when it is further calcined at high temperature, its thickness increases accordingly. This may be because the carbon nanotube film becomes fluffy due to high temperature calcination, resulting in a thicker thickness.

[0040] The microscopic morphology and performance of the carbon nanotube films prepared in Examples 1 to 4 were characterized:

[0041] Figure 1 The original carbon nanotube film (before modification) is at the 2 μm level ( Figure 1 a) and 500nm level ( Figure 1 b) SEM image from Figure 1 b It can be seen that the surface of the carbon nanotube is relatively smooth and the diameter of the carbon nanotube is about 100nm.

[0042] Figure 2 The mechanical properties of the carbon nanotube film-500 prepared in Example 2 are shown in FIG. Figure 2 It can be seen that the carbon nanotube film prepared in Example 2 can be curled, bent, and folded. The film is further cut into a size of 15mm*30mm. It can be found that the film can bear a weight of 500g without deformation or breakage, indicating that the carbon nanotube film prepared in Example 2 has good mechanical properties.

[0043] Figure 3 The Raman spectrum of the carbon nanotube film-500 prepared in Example 2 is as follows: Figure 3 As can be seen from b, the product I obtained in Example 2 D / I GThe value is significantly higher than that of the original carbon nanotube film, indicating that after activation-high temperature calcination, the defects of the carbon nanotube film are enhanced. When the heat treatment temperature is low (500-550°C), the defects can increase the refractive index and absorption coefficient of the film, thereby effectively reducing the emissivity of the film; but at a higher heat treatment temperature (700-900°C), the further increase of the defects will change the bond length of the valence bond between atoms, and at the same time change the type of hybrid orbits of some carbon atoms. The changes in the bond length and orbit change the electrical properties of the defective area of ​​the carbon nanotube, and the defects form electron wave scattering centers on the carbon surface. Such centers affect the transfer of electrons, and ultimately reduce the conductivity of the carbon nanotube. At this time, the increase of defects has a much greater impact on the conductivity than the refractive index and absorption coefficient. Therefore, the infrared emissivity of the carbon nanotube film prepared in Examples 3-4 is higher than that of the carbon nanotube film prepared in Example 2.

[0044] Figure 4 The Raman spectrum of the carbon nanotube film-700 prepared in Example 3 is as follows: Figure 4 It can be seen that the product I obtained in Example 3 D / I G The value is significantly higher than that of Example 2, indicating that after further high-temperature calcination, the defects on the surface of the carbon nanotube film are enhanced, so its conductivity decreases, resulting in an increase in infrared emissivity.

[0045] Figure 5 The Raman spectrum of the carbon nanotube film-900 prepared in Example 4 is as follows: Figure 5 It can be seen that the product I obtained in Example 4 D / I G The value is significantly higher than that of Example 3, indicating that with the further increase of the pyrolysis temperature, the defects on the surface of the carbon nanotube film are enhanced, so its conductivity decreases, resulting in an increase in infrared emissivity.

[0046] pass Figures 3 to 5 It can be seen that as the temperature increases, combined with Raman spectroscopy, the results are consistent with the theory, that is, as the temperature increases, I D / I G As the value increases, the defects increase, the conductivity of the carbon nanotube film decreases, and the infrared emissivity of the carbon nanotube film increases.

[0047] Figure 6 The Joule thermal performance of the carbon nanotube film-500 prepared in Example 2 is as follows: Figure 6 It can be seen that as the applied voltage increases, the surface temperature also increases accordingly. When the applied voltage is lower than 2.0V, the surface temperature does not change significantly; when the applied voltage is 3.5V, the surface temperature reaches 76.1℃, indicating that the prepared product has good Joule heat performance. This shows that the film has great potential in protecting the normal operation of electronic equipment in cold environments.

[0048] Figure 7 The shielding effectiveness of the carbon nanotube film-500 prepared in Example 2. Figure 7 It can be seen that in the X-band (8.2-12.4 GHz), when the pyrolysis temperature is 500°C, its shielding effectiveness reaches about 54.6 dB, which indicates that the film has a good shielding effect and can effectively suppress the interference of electromagnetic waves.

[0049] Figure 8 To test the infrared emissivity of the carbon nanotube films before modification and those prepared in Examples 1 to 4, Figure 7 It can be seen that compared with the carbon nanotube film before modification, only activated and obtained at a higher calcination temperature, the product prepared in Example 2 has a lower infrared emissivity in the 3-5μm band than in the 8-14μm band, indicating that effective treatment of the carbon nanotube film can reduce the infrared emissivity of the carbon nanotube film.

Claims

1. A method for preparing a modified carbon nanotube film with low infrared emissivity, characterized in that: Specifically, the carbon nanotube film is first activated with a KOH solution, and then heat-treated in an argon atmosphere to obtain a modified carbon nanotube film; wherein the heat treatment temperature is 500-550°C, the heat treatment time is 3-4h, and the heating rate is 5-5.5°C / min; the infrared emissivity of the modified carbon nanotube film is as low as 0.473 in the 3-5μm band, and as low as 0.493 in the 8-14μm band.

2. The method for preparing a modified carbon nanotube film with low infrared emissivity according to claim 1, characterized in that: The activation is performed using a KOH solution, specifically, the carbon nanotube film is immersed in a KOH solution, and the concentration of the KOH solution is 1.5-2 mol / L.

3. The method for preparing a modified carbon nanotube film with low infrared emissivity according to claim 2, characterized in that: The soaking time is not less than 24h.

4. The method for preparing a modified carbon nanotube film with low infrared emissivity according to claim 2, characterized in that: The immersed carbon nanotube film was taken out, washed with water until neutral, and then dried in vacuum at 50-60°C.