A method for preparing battery-grade single crystal iron phosphate
By controlling the reaction conditions and raw material ratios, high-purity octahedral single-crystal iron phosphate was prepared, solving the problems of high cost and low compaction density in existing lithium iron phosphate production, and realizing the preparation of efficient and low-cost lithium iron phosphate materials.
Patent Information
- Application Number
- CN202211012399.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Existing lithium iron phosphate production processes suffer from high costs, numerous impurities, and low compaction density. In particular, when using ferrous sulfate, a byproduct of titanium dioxide slag, as a raw material, the sulfate extraction process is complex and wasteful of water resources, resulting in poor electrochemical performance.
High-purity hydrated hydroxy ferric phosphate was prepared by controlling reaction conditions using iron source, phosphoric acid, hydrogen peroxide and 1,2-propanediol as raw materials to form octahedral single crystal ferric phosphate. The closed-loop reaction system reduced the use of precipitant, simplified the process and reduced costs.
The preparation of high-purity iron phosphate with an octahedral single crystal morphology and high compaction density has been achieved, which is suitable for the preparation of high-performance lithium iron phosphate, reducing production costs and achieving zero wastewater discharge, and simplifying the process flow.
Smart Images

Figure CN115506006B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a method for preparing battery-grade single crystal iron phosphate. Background Art
[0002] With the rapid development of the global economy, the existing resources of mankind are becoming increasingly scarce, and the development of new energy has become the direction of the current society. As a new type of lithium-ion battery positive electrode material, lithium iron phosphate (LiFePO4) is very popular in the new energy market for its excellent cycle stability and high temperature resistance, but its low temperature performance and energy density are poorer than those of ternary batteries. The compaction density of lithium iron phosphate materials is affected by sintering temperature, crushing particle size and precursors. Among them, sintering temperature and crushing particle size have limited room for improvement in their compaction density. Improving the compaction density of lithium iron phosphate materials by increasing the compaction density of precursors is the most effective and significant method.
[0003] Ferrous phosphate is one of the important materials for the industrial production of lithium iron phosphate. Among the many methods for synthesizing iron phosphate, the cost of synthesizing iron phosphate using ferrous sulfate, a byproduct of titanium dioxide slag, as raw material is high. However, the steps for extracting ferrous sulfate in this synthesis process are complicated, and the subsequent preparation requires a large amount of pure water to wash away the excessive sulfate (SO4 2- ), wasting water resources and increasing production costs. In addition, the iron phosphate produced by this process has many impurities and low compaction density, resulting in poor electrochemical performance of the lithium iron phosphate produced subsequently. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing battery-grade single crystal iron phosphate.
[0005] The present invention provides a method for preparing battery-grade single crystal iron phosphate, comprising the following steps:
[0006] S1, adding an iron source into a phosphoric acid solution and fully dissolving it to obtain an iron-phosphorus solution;
[0007] S2. Add hydrogen peroxide and 1,2-propylene glycol to the iron-phosphorus liquid, first stir and react at room temperature for 10-30 minutes, then heat and stir and react at 70-100° C. for 3-6 hours, and after the reaction is completed, let it stand for aging and filter, wash the obtained filter cake, dry it, and then sinter it at high temperature to obtain the product.
[0008] In S2, the filter cake obtained is hydrated hydroxyferric phosphate. The reaction mechanism of the present invention to obtain hydrated hydroxyferric phosphate is: 10Fe 2+ +5H2O2+8HPO4 2- ——2Fe5(PO4)4(OH)3·2H2O+4H + .
[0009] Preferably, the iron source is industrial waste containing elemental iron, preferably at least one of iron flakes, iron filings and iron slag.
[0010] Preferably, the carbon content in the iron sheets, iron filings and iron slag is ≤3%.
[0011] Preferably, the mass fraction of the phosphoric acid solution is 30-60wt%.
[0012] Preferably, the mass ratio of the iron source to the phosphoric acid solution is 1:(3-6).
[0013] Preferably, the ratio of the iron source to the hydrogen peroxide is 1 g: (1-2) mL, and the mass fraction of the hydrogen peroxide is 20-30 wt %.
[0014] Preferably, the mass ratio of the iron source to 1,2-propylene glycol is 1:(0.05-0.1).
[0015] In S1, complete dissolution means that no obvious bubbles are generated; preferably, in S1, the dissolution temperature is 50-70°C and the dissolution time is 20-30h.
[0016] In S1, after the iron source is added to the phosphoric acid solution and fully dissolved, a conventional filtering and impurity removal step may also be included, and the filtrate is collected after filtering, which is the iron-phosphorus solution.
[0017] Preferably, in S2, the stirring speed is 200-500 rpm.
[0018] Preferably, in S2, the standing aging time is 10-30 min.
[0019] Preferably, in S2, the high temperature sintering temperature is 600-800°C and the time is 5-10h.
[0020] A battery-grade single crystal iron phosphate is prepared by the preparation method.
[0021] The beneficial effects of the present invention are as follows:
[0022] The preparation method of iron phosphate provided by the present invention can use industrial waste iron pieces, iron filings, and iron slag as raw materials, and by controlling the raw material concentration ratio, temperature, stirring speed, reaction time and other conditions, it is possible to prepare high-purity iron phosphate without adjusting pH and other precipitants during the preparation of iron phosphate; at the same time, the phosphoric acid generated by the reaction can be recycled to continue to dissolve iron, achieving a closed cycle and zero discharge of wastewater, simplifying the process flow, and reducing production costs, impurity removal costs, and wastewater treatment costs. The method uses 1,2-propylene glycol as a surfactant, and the prepared iron phosphate has an octahedral single crystal morphology, high purity, and is suitable for preparing lithium iron phosphate with a high compaction density. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the iron phosphate prepared in Example 1 of the present invention.
[0024] Figure 2 This is a SEM image of the iron phosphate prepared in Comparative Example 1 of the present invention.
[0025] Figure 3 This is a SEM image of the iron phosphate prepared in Comparative Example 2 of the present invention.
[0026] Figure 4 This is a SEM image of the iron phosphate prepared in Comparative Example 3 of the present invention.
[0027] Figure 5 This is a SEM image of the iron phosphate prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is described in detail below through specific embodiments.
[0029] In the following examples and comparative examples, the scrap iron sheets used had a carbon content of 2 wt%.
[0030] Example 1
[0031] S1. Add 60 g of scrap iron into 293.1 g of 60 wt% phosphoric acid solution, and place in a 60° C. water bath for 24 h to dissolve the solution, then filter and collect the filtrate to obtain an iron-phosphorus solution.
[0032] S2. Add 4.93 g of 1,2-propylene glycol and 80 mL of 30 wt% hydrogen peroxide to the iron-phosphorus liquid, stir and react at 300 rpm at room temperature for 10 min, then heat to 80°C, stir and react at 300 rpm for 4 h, let stand for 10 min and then filter, wash the filter cake with deionized water 3 times, then dry at 100°C for 12 h, and then sinter at 600°C for 5 h to obtain battery-grade single crystal iron phosphate.
[0033] Example 2
[0034] The only difference between Example 2 and Example 1 is that the mass concentration of the phosphoric acid solution is 52 wt %.
[0035] Example 3
[0036] The only difference between Example 2 and Example 1 is that the mass concentration of the phosphoric acid solution is 42 wt %.
[0037] Example 4
[0038] S1. Add 60 g of scrap iron into 349.2 g of 35 wt% phosphoric acid solution, place in a 50° C. water bath for 30 h to dissolve, then filter and collect the filtrate to obtain an iron-phosphorus solution;
[0039] S2. Add 6 g of 1,2-propylene glycol and 120 mL of 30 wt% hydrogen peroxide to the iron-phosphorus liquid, stir and react at 200 rpm at room temperature for 20 min, then heat to 70°C, stir and react at 200 rpm for 6 h, let stand for 20 min and then filter, wash the filter cake with deionized water 3 times, then dry at 100°C for 12 h, and then sinter at 700°C for 8 h to obtain battery-grade single crystal iron phosphate.
[0040] Example 5
[0041] S1. Add 60 g of scrap iron into 232.2 g of a 42 wt% phosphoric acid solution, place in a 70° C. water bath to dissolve for 20 h, then filter and collect the filtrate to obtain an iron-phosphorus solution;
[0042] S2. Add 3g of 1,2-propylene glycol and 60mL of 30wt% hydrogen peroxide to the iron-phosphorus liquid, stir and react at 500rpm for 30min at room temperature, then heat to 95°C, stir and react at 200rpm for 4h, let stand for 10min and then filter, wash the filter cake with deionized water 3 times, dry at 100°C for 12h, and then sinter at 800°C for 5h to obtain battery-grade single crystal iron phosphate.
[0043] Comparative Example 1
[0044] The only difference between Comparative Example 1 and Example 1 is that polyethylene glycol is used instead of 1,2-propylene glycol.
[0045] Comparative Example 2
[0046] The only difference between Comparative Example 2 and Example 1 is that sodium aluminate is used instead of 1,2-propylene glycol.
[0047] Comparative Example 3
[0048] The only difference between Comparative Example 3 and Example 1 is that sodium dodecylbenzene sulfonate is used instead of 1,2-propylene glycol.
[0049] Comparative Example 4
[0050] The only difference between Comparative Example 1 and Example 1 is that 1,2-propylene glycol is not added.
[0051] Test example
[0052] The SEM images of the iron phosphate prepared in Example 1 and Comparative Examples 1-3 are as follows: Figure 1-4As shown. It can be seen that Figure 1 The morphology is a large octahedral single crystal, which is due to the participation of the surfactant 1,2-propylene glycol, Fe 3+ The hexacoordinated geometry (i.e., octahedron) configuration of the 1,2-propylene glycol coordinated ion can be functionalized to form a single crystal octahedron of hydrated hydroxyferric phosphate, which is dehydrated at high temperature to form anhydrous single crystal octahedral ferric phosphate with a grain diameter of 1-3 μm. Comparative Examples 1-3 use other surfactants, and Comparative Example 4 does not use a surfactant. The formed ferric phosphate is in the form of fine flakes with a thickness of 20-40 nm. Compared with Comparative Example 4, the formation effect of the final morphology of ferric phosphate in Comparative Examples 1-3 is improved.
[0053] The iron phosphate of Examples 1-3 and Comparative Examples 1-4 is used to prepare lithium iron phosphide according to a conventional method, comprising the following steps:
[0054] S01: iron phosphate, lithium carbonate and glucose were prepared in a molar ratio of 1:1.02:0.2, premixed for 12 hours, sand-milled and sprayed to obtain a dry material;
[0055] S02: Under nitrogen protection, place the dried material in an atmosphere furnace and keep it at 750°C for 10 hours to obtain lithium iron phosphate.
[0056] The lithium iron phosphate prepared from the iron phosphate of the above Examples 1-3 and Comparative Examples 1-4 was subjected to performance tests, and the results are shown in Table 1:
[0057] Table 1
[0058]
[0059] Comparing the data of Examples 1-3 in Table 1, it can be seen that as the concentration of phosphoric acid increases, the compaction density of lithium iron phosphate prepared from the iron phosphate formed therefrom also increases.
[0060] Comparison of the data of Example 1 and Comparative Examples 1-4 in Table 1 shows that the present invention uses 1,2-propylene glycol as a surfactant, and the lithium iron phosphate prepared by the large single crystal octahedral morphology of iron phosphate formed has the highest compaction density, which is 2.58 g / cm 3 In summary, the preparation method of the present invention can be used to prepare single-crystal octahedral iron phosphate, and the product has strong performance stability and higher compaction density.
[0061] It can be seen that the preparation method of the present invention does not add a precipitant during the entire process, the raw material cost used is low, the entire solution system can be recycled, and the preparation cost is reduced. The product is high-purity single-crystalline iron phosphate, which has an octahedral single crystal morphology without impurities, high purity, small particle size, and high compaction density, and can be used to prepare high-compacted lithium iron phosphate.
[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing battery-grade single crystal iron phosphate, characterized in that: The following steps are involved: S1. Add an iron source into a phosphoric acid solution and fully dissolve it to obtain an iron-phosphorus solution; the mass fraction of the phosphoric acid solution is 30-60wt%; the mass ratio of the iron source to the phosphoric acid solution is 1:(3-6); the iron source is at least one of iron flakes, iron filings, and iron slag; the carbon content of the iron flakes, iron filings, and iron slag is ≤3%; S2, add hydrogen peroxide and 1,2-propylene glycol to the iron-phosphorus liquid, first stir and react at room temperature for 10-30 minutes, then heat and stir and react at 70-100° C. for 3-6 hours, stand for aging and filter after the reaction is completed, wash and dry the obtained filter cake and then sinter at high temperature to obtain; the ratio of the iron source to the hydrogen peroxide is 1g:(1-2)mL, the mass fraction of the hydrogen peroxide is 20-30wt%; the mass ratio of the iron source to the 1,2-propylene glycol is 1:(0.05-0.1); the temperature of the high-temperature sintering is 600-800° C., and the time is 5-10h.
2. The method for preparing battery-grade single crystal iron phosphate according to claim 1, characterized in that: In S1, the dissolution temperature is 50-70°C and the dissolution time is 20-30h.
3. The method for preparing battery-grade single crystal iron phosphate according to claim 1, characterized in that: In S2, the stirring speed is 200-500 rpm.
4. The method for preparing battery-grade single crystal iron phosphate according to claim 1, characterized in that: In S2, the standing aging time is 10-30 minutes.
5. A battery-grade single crystal iron phosphate, characterized in that: Prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Cited By
Preparation method of blocky monocrystal iron phosphate
CN122013292A
A method for preparing bulk single-crystal iron phosphate
CN122013292B