Compositions and methods for increasing wet and dry strength
By developing high-content cationic glyoxalated polyacrylamide, the problems of high transportation cost and low practicality of existing GPAM products have been solved, and the wet strength and dry strength can be efficiently enhanced in papermaking, and the transportation volume and cost can be reduced.
Patent Information
- Application Number
- CN202180021098.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing glyoxalated polyacrylamide (GPAM) products have problems with high transportation costs and low practicability in the paper industry, mainly because they require a large amount of water-containing carriers for storage and transportation, resulting in large volumes and high costs.
Develop a cationic glyoxalated polyacrylamide (GPAM) containing at least 15% cationic monomer, a base polymer weight average molecular weight of at least 25,000 Da, and a weight ratio of glyoxal to base polymer of 17:83 to 25:75 and solids percentages between 2% and 11%, enabling storage and transportation with reduced or no need for large amounts of aqueous carriers.
It achieves a reduction in the transportation cost and storage volume of GPAM products, improves its wet strength and dry strength enhancement effect in papermaking, while reducing the volume and handling complexity required for transportation.
Smart Images

Figure BDA0003844815080000221 
Figure BDA0003844815080000231 
Figure BDA0003844815080000241
Abstract
Description
Technical Field
[0001] The present disclosure relates generally to glyoxalated polyacrylamide (GPAM) products, compositions and articles containing the same and methods of use thereof, particularly GPAM products for use in the papermaking industry, and more particularly cationic GPAM compositions and their use in papermaking applications and products such as paper-based products. Background Art
[0002] Glyoxalated polyacrylamide (GPAM) products are widely used in the paper industry, typically to increase wet and dry strength of paper. For example, glyoxalated polyacrylamide can increase the initial wet strength of many household paper towels, which is a useful property because household paper towels are often in contact with water during use. The application of glyoxalated polyacrylamide to paper products can also increase the compressive strength and dimensional stability of many board-grade paper products.
[0003] GPAM is usually prepared by the reaction between glyoxal and a polyacrylamide base polymer such as a cationic polyacrylamide backbone. In some cases, the reaction between glyoxal and the cationic polyacrylamide is carried out in a weakly alkaline aqueous solution and is stable under acidic conditions. In practice, the polyacrylamide component of a GPAM product usually contains a relatively small amount of cationic monomer, usually less than about 5 mol%, thereby limiting the contribution of cationic charge to the GPAM product.
[0004] In addition, GPAM prepared by conventional methods cannot usually be dried into a solid particle form without inducing significant and rapid crosslinking of the GPAM, which limits the practicality of the resulting GPAM product. Therefore, GPAM is usually stored and transported in a bulk aqueous fluid carrier. The volume of GPAM products transported in this way may be quite large, which usually requires large-volume containers or tankers to transport. Transporting such a large amount of product significantly increases the cost of transporting and using the GPAM product.
[0005] Due to the properties of current GPAM products and logistical considerations regarding their transportation, there remains a need for GPAM products that include properties that facilitate lower shipping costs and / or lower shipping volumes of GPAM products while still maintaining the desired properties of GPAM products. Summary of the invention
[0006] The present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises: a. a base polymer comprising at least 15 wt. % of a cationic monomer, optionally wherein the cationic monomer comprises DADMAC and / or acryloxyethyltrimethylammonium chloride ("Q9"); b. the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da; c. the cationic GPAM comprises at least about 17:83, optionally wherein the cationic GPAM is capable of being stored and transported without adding large amounts of aqueous carriers or using reduced volumes of aqueous carriers compared to conventional GPAMs used in papermaking.
[0007] In addition, the present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises: a. a base polymer of at least 15 wt. % of a cationic monomer, optionally wherein the cationic monomer comprises DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9"); b. the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da; c. the cationic GPAM comprises at least about 17:83, optionally at least about 20:80, further optionally at least about 23:77, further optionally at least about 25: 75% by weight of glyoxal:base polymer; and d. the GPAM optionally comprises a solids percentage of from about 2% to about 11%, optionally greater than about 4% to about 11%, further optionally greater than about 4% to about 8%, further optionally greater than about 4% to about 7%; further optionally wherein the cationic GPAM has a GPAM content of from about 2% to about 11%, optionally from about 3% to about 10%, further optionally from about 4% to about 8%, further optionally from about 5% to about 7%; wherein optionally, the cationic GPAM can be stored and transported without adding large amounts of aqueous carrier or using a reduced volume of aqueous carrier compared to conventional GPAM used in papermaking.
[0008] In some embodiments, the cationic GPAM may have a GPAM content of about 2% to about 11%, optionally about 3% to about 10%, further optionally about 4% to about 8%, further optionally about 5% to about 7%. In some embodiments, the base polymer may comprise a weight average molecular weight of about 25 kDa or more, 30 kDa or more, 40 kDa or more, 50 kDa or more, 75 kDa or more, 100 kDa or more, 125 kDa or more, 150 kDa or more, 175 kDa or more, 200 kDa or more, 225 kDa or more, 250 kDa or more, 275 kDa or more, 300 kDa or more, 325 kDa or more, 350 kDa or more, 375 kDa or more, 400 kDa or more, or 500 kDa or more. In some embodiments, the base polymer may comprise a charge of at least 15 wt%, at least 20 wt%, at least 25 wt%, at least 30 wt%, at least 35 wt%, at least 40 wt%, at least 50 wt%, or at least 60 wt%. In some embodiments, the cationic GPAM may comprise a solids percentage of about 2% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, 4.5% or more, 5.0% or more, 5.5% or more, 6.0% or more, 6.5% or more, 7.0% or more, 7.5% or more, 8.0% or more, 8.5% or more, 9.0% or more, 9.5% or more, 10.0% or more, 10.5% or more, 11.0% or more, or 11.5% or more. In some embodiments, the cationic GPAM may comprise a weight ratio of glyoxal:base polymer of at least about 17:83, at least about 18:82, at least about 19:81, at least about 20:80, at least about 21:79, at least about 22:78, at least about 23:77, at least about 24:76, at least about 25:75, at least about 26:74, at least about 27:73, at least about 28:72, at least about 29:71, or at least about 30:70. In some embodiments, the cationic GPAM may comprise a base polymer comprising a cationic monomer:acrylamide weight ratio of from about 15:85 to about 60:40, optionally from about 20:80 to about 55:45, further optionally from about 25:75 to about 50:50. In some embodiments, the backbone may comprise one or more cationic monomers. In some embodiments, the cationic GPAM may comprise a viscosity of about 30 cPs or greater, about 31 cPs or greater, about 32 cPs or greater, about 33 cPs or greater, about 34 cPs or greater, or about 35 cPs or greater, as measured, for example, by a Brookfield viscometer. In some embodiments, the backbone polymer may comprise a copolymer of acrylamide or methacrylamide and one or more cationic monomers.In some embodiments, the backbone polymer may include an acrylamide-based polymer. In some embodiments, the aqueous carrier may include water. In some embodiments, the cationic GPAM may include a solid percentage of about greater than 4% to about 8%, optionally about greater than about 4% to about 7%, further optionally about 5% to about 7%, for example about 5% to about 6%.
[0009] In some embodiments, the one or more cationic monomers may be selected from the group consisting of acryloxyethyltrimethylammonium chloride (“AETAC”), methacryloyloxyethyltrimethylammonium chloride, methacrylamidopropyltrimethylammonium chloride (“MAPTAC”), acrylamidopropyltrimethylammonium chloride, methacryloyloxyethyldimethylammonium sulfate, dimethylaminoethyl acrylate, dimethylaminopropyl methacrylamide, Q6 (methacryloyloxyethyltrimethylammonium chloride), Q6o (dimethylaminoethyl methacrylate sulfate), diallyldimethylammonium chloride (“DADMAC”); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate methyl chloride quaternary salt (“DMAEA.MCQ”), dimethylaminoethyl acrylate methyl sulfate quaternary salt (“DMAEM.MCQ”), dimethylaminoethyl acrylate benzyl chloride quaternary salt (“DMAEA.BCQ”), dimethylaminoethyl acrylate sulfate, dimethacrylate methylaminoethyl hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacryloyl hydrochloride; dialkylaminoalkyl acrylamide or dialkylaminoalkyl methacrylamide and their quaternary ammonium salts or acid salts, such as acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, such as diallyl diethylammonium chloride and diallyl dimethyl ammonium chloride. In some embodiments, the one or more cationic monomers may include DADMAC. In some embodiments, the one or more cationic monomers may include acryloyloxyethyltrimethylammonium chloride ("Q9"). In some embodiments, the one or more cationic monomers may include DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9").In some embodiments, the one or more cationic monomers may be selected from the group consisting of methacryloyloxyethyltrimethylammonium chloride, acryloxyethyltrimethylammonium chloride (also known as Q9), 3-(methacrylamido)propyltrimethylammonium chloride, 3-(acrylamido)propyltrimethylammonium chloride, diallyldimethylammonium chloride (DADMAC), dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide, dimethylaminopropyl methacrylamide.
[0010] In some embodiments, the backbone polymer may include one or more primary amide-containing monomers. In some embodiments, the backbone polymer may include one or more monomers selected from the group consisting of acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide, and any combination thereof. In some embodiments, the backbone polymer may include one or more acrylamide monomers.
[0011] In addition, the present disclosure generally relates to paper products comprising one or more cationic GPAMs as discussed herein. In some embodiments, the paper product may include at least one paper layer or paper web containing the cationic GPAM. In some embodiments, the paper product may include one or more of paper, paperboard, tissue, and wallboard. In some embodiments, the paper product may include one or more of kraft paper, sulfite paper, semi-chemical paper, and the like, including paper produced using bleached pulp, unbleached pulp, or a combination thereof. In some embodiments, the paper product may include a fiber-based product. In some embodiments, the paper product may include one or more of hand sheets, board-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board grades, and tissue and towel grade paper materials, paper towels, diapers, sanitary napkins, training pants, pantiliners, incontinence briefs, tampons, urine pads, trash can liners, coffee filter bags, air filter materials, dryer pads, floor cleaning pads, absorbent facial tissues, absorbent toilet tissues, napkins, wrapping paper, and / or other paperboard products such as paper boxes and bag papers. In some embodiments, the paper product may include a cellulosic paperboard web, optionally comprising primarily cellulosic fibers. In some embodiments, the paper product may include from about 0.02% to about 10% cationic GPAM based on the dry weight of the cellulosic fibers, optionally in the range of about 0.05% to 5% by weight of the dry paper weight. In some embodiments, the paper product may comprise an improvement in STFI value of 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, or 25.0% or greater when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton, as compared to a blank sample of the STFI test for the paper product. In some embodiments, the paper product may comprise a 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, 25.0% or greater, 27.5% or greater, 30.0% or greater, 32.5% or greater, 35.0% or greater, 37.5% or greater, or 40% or greater improvement in burst strength value when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton, as compared to a blank sample tested for burst strength.
[0012] Furthermore, the present disclosure is generally directed to a papermaking process, wherein the process includes adding one or more cationic GPAMs as discussed herein during the papermaking process in an amount effective to increase the wet strength and / or dry strength of a paper product produced by the process.
[0013] In addition, the present disclosure generally relates to a method of making hand sheets, the method comprising: a. providing a pulp slurry; b. diluting the pulp slurry; c. adding one or more salts to a desired conductivity level; d. adjusting the pH to a desired value; e. adding one or more cationic GPAMs as discussed herein; f. adding the treated pulp to a powered paper former; g. pressing the paper produced by f.; h. drying the paper; and i. finishing the paper.
[0014] Additionally, the present disclosure generally relates to a method of making one or more paper products, wherein the method comprises: a. providing a composition comprising primarily cellulosic fibers; b. adding a predetermined amount of one or more cationic GPAMs as discussed herein; and c. forming the desired paper product.
[0015] In addition, the present disclosure generally relates to a method of making one or more paper products, optionally one or more absorbent paper products, wherein the method comprises: a. providing a composition comprising any of softwood fibers, hardwood fibers, recycled fibers, refined fibers, or a mixture of any of the foregoing, in an amount sufficient to form a total furnish of approximately 1% to 100% hardwood fibers, softwood fibers, recycled fibers, refined fibers, or a mixture of any of the foregoing; (b) adding a predetermined amount of one or more cationic GPAMs as discussed herein; and (c) forming the paper product by drying on one or more drying devices to a desired moisture content level.
[0016] Additionally, the present disclosure is generally directed to a method for strengthening paper comprising contacting pulp fibers with a reinforcing resin comprising at least a cationic GPAM as discussed herein, and at least partially curing the cationic GPAM in the mixture of pulp fibers and cationic GPAM to produce a paper product having enhanced strength.
[0017] In some embodiments, the cationic GPAM may be added to a cellulosic fiber suspension at the wet end of a papermaking facility. In some embodiments, the cationic GPAM may be added in an amount of about 0.02% to about 10% by dry weight of the cellulosic fibers, optionally in a range of about 0.05% to 5% by weight of the dry paper weight. In some embodiments, the cationic GPAM may be added before, during, and / or after forming the paper. In some embodiments, the paper product may include an STFI value improvement of 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, 25.0% or greater when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton, compared to a blank sample of the STFI test for the paper product. In some embodiments, the paper product may comprise a 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, 25.0% or greater, 27.5% or greater, 30.0% or greater, 32.5% or greater, 35.0% or greater, 37.5% or greater, or 40% or greater improvement in burst strength value when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton, as compared to a blank sample tested for burst strength. In some embodiments, the paper product may include one or more of hand sheets, board-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board grades and tissue and towel grade paper materials, paper towels, diapers, sanitary napkins, training pants, pantiliners, incontinence briefs, tampons, urine pads, trash can liners, coffee filter bags, air filter materials, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent toilet paper, napkins, wrapping paper, and / or other paperboard products such as cartons and bag paper. In some embodiments, the paper product may include a cellulose paperboard web, optionally comprising primarily cellulose fibers. In some embodiments, the cationic GPAM composition can achieve effective drainage, such as drainage of OCC pulp, such as showing an improvement in drainage time (e.g., the time to collect a given amount of filtrate from OCC pulp) of 25.0% or more, 30.0% or more, 35.0% or more, 40.0% or more, 45.0% or more, 50.0% or more, 55.0% or more, compared to drainage without the use of the cationic GPAM composition. In some embodiments, the cationic GPAM can increase the drainage rate of the treated sample, resulting in an increase in paper production rate, compared to drainage without the use of the cationic GPAM composition.In addition, the cationic GPAM composition can achieve a reduction in the total amount of solids present in the treated sample, for example, a reduction in the total solids present in the filtrate collected from OCC pulp treated with the cationic GPAM, for example, a reduction in the solids content of white water from a tray or post-sheet forming silo, such as an improvement (reduction in solids content) of 15% or more, 17.5% or more, 20.0% or more, 22.5% or more, 25.0% or more, 27.5% or more, 30.0% or more, or 32.5% or more, compared to the total amount of solids present in the sample without the cationic GPAM composition. In some embodiments, the cationic GPAM can improve drying energy savings.
[0018] In addition, the present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises a base polymer of at least 15 wt% of a cationic monomer, wherein the cationic monomer comprises DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9"), further wherein the base polymer comprises a weight average molecular weight of at least 30,000 Da, wherein the cationic GPAM comprises a glyoxal:base polymer weight ratio of at least about 17:83, optionally about 20:80, wherein the GPAM comprises a solids percentage of from about 2% to about 11%, optionally greater than 4% to about 11%, further optionally greater than 4% to about 8%, further optionally greater than 4% to about 7%, and further wherein the base polymer comprises one or more acrylamide monomers, and further optionally wherein the cationic GPAM is capable of being stored and transported without the addition of a substantial amount of an aqueous carrier, optionally wherein the aqueous carrier comprises water, further optionally wherein the cationic GPAM is capable of being stored and transported without the addition of a substantial amount of an aqueous carrier.
[0019] In addition, the present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises a base polymer of at least 15 wt% of a cationic monomer, wherein the cationic monomer comprises DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9"), further wherein the base polymer comprises a weight average molecular weight of at least 30,000 Da, wherein the cationic GPAM comprises a glyoxal:base polymer weight ratio of at least about 17:83, optionally about 20:80, wherein the GPAM comprises a solids percentage of from about 2% to about 11%, optionally greater than 4% to about 11%, further optionally greater than 4% to about 8%, further optionally greater than 4% to about 7%; and further wherein the cationic GPAM has a GPAM content of from about 2% to about 11%, optionally from about 3% to about 10%, further optionally from about 4% to about 8%, further optionally from about 5% to about 7%, further optionally wherein the cationic GPAM is capable of being stored and transported without the addition of large amounts of aqueous carriers.
[0020] In some embodiments, the GPAM will comprise one or more of the following:
[0021] i. The backbone polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9");
[0022] ii. the backbone polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9"), and optionally comprises a molecular weight in the range of at least about 50 kDa to 1500 kDa, further optionally at least about 100 kDa to 1000 kDa, or still further optionally at least about 140 kDa to 1000 kDa;
[0023] iii. the backbone polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from DADMAC and / or acryloyloxyethyltrimethylammonium chloride ("Q9"), and optionally comprises a molecular weight in the range of at least about 50 kDa to 1500 kDa, or at least about 100 kDa to 1000 kDa, or at least about 140 kDa to 1000 kDa, and the base polymer charge of the base polymer optionally ranges from 15%-60%, 20%-50%, 20%-40%, or optionally comprises 20%, 30% or 40%; and the cationic GPAM optionally comprises a glyoxal:base polymer weight ratio of at least about 17:83, or optionally about 20:80, further optionally at least about 23:77 to about 29:71, still further optionally at least about 25:75, 26:74, 27:73, 28:72 or 29:71;
[0024] iv. an aqueous carrier comprising water;
[0025] v. the cationic GPAM comprises a solids percentage of greater than about 4% to about 8%, optionally about 5% to about 7%, optionally about 7%, 5.5% or 5.0%; and / or
[0026] vi. A combination of any two or more of (i)-(v). DETAILED DESCRIPTION
[0027] definition
[0028] As used herein, the singular forms "a", "an", and "the" include plural referents unless the context clearly dictates otherwise. Unless otherwise specifically indicated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0029] As used herein, the term "monomer" generally refers to nonionic monomers, anionic monomers, cationic monomers, zwitterionic monomers, betaine monomers, and zwitterion pair monomers.
[0030] As used herein, the terms "polymer", "polymers", "polymeric" and similar terms are used in their ordinary meaning as understood by those skilled in the art, and thus may be used herein to refer to or describe a macromolecule (or a group of such molecules) comprising repeating units. Polymers can be formed in various ways, including by polymerizing monomers and / or by chemically modifying one or more repeating units of a precursor polymer. Unless otherwise specified, polymers may include "homopolymers", which may include substantially identical repeating units that may be formed by various methods, such as by polymerizing specific monomers. Unless otherwise specified, polymers may also include "copolymers", which may include two or more different repeating units that may be formed, for example, by copolymerizing two or more different monomers and / or by chemically modifying one or more repeating units of a precursor polymer. Unless otherwise specified, polymers or copolymers may also include "terpolymers", which may include polymers that may include three or more different repeating units. As used herein, the term "polymer" is intended to include the acid form of the polymer as well as various salts thereof. The polymer may be amphoteric in nature, i.e., contain anionic and cationic substituents, although not necessarily in the same proportions.
[0031] As used herein, the term "nonionic monomer" generally refers to a monomer having a neutral charge.
[0032] As used herein, the term "anionic monomer" may refer to anionic monomers that are substantially all or partially (balanced) anionic at a pH in the range of about 4.0 to about 9.0. An "anionic monomer" may be neutral at low pH (a pH of about 2 to about 6), or anionic at low pH.
[0033] As used herein, the term "cationic monomer" generally refers to a monomer having a positive charge. Examples of cationic monomers may include, but are not limited to, those comprising acryloxyethyltrimethylammonium chloride ("AETAC"), methacryloyloxyethyltrimethylammonium chloride, methacrylamidopropyltrimethylammonium chloride ("MAPTAC"), acrylamidopropyltrimethylammonium chloride, methacryloyloxyethyldimethylammonium sulfate, dimethylaminoethyl acrylate, dimethylaminopropyl methacrylamide, Q6 (methacryloyloxyethyltrimethylammonium chloride), Q6o (methacrylic acid dimethylaminoethyl sulfate) and / or diallyldimethylammonium chloride ("DADMAC"). The cationic monomers may also include, but are not limited to, dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including, but not limited to, dimethylaminoethyl acrylate methyl chloride quaternary salt ("DMAEA.MCQ"), dimethylaminoethyl acrylate methyl sulfate quaternary salt ("DMAEM.MCQ"), dimethylaminoethyl acrylate benzyl chloride quaternary salt ("DMAEA.BCQ"), dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate , dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacryloyl hydrochloride; dialkylaminoalkyl acrylamide or dialkylaminoalkyl methacrylamide and their quaternary ammonium salts or acid salts, such as acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide methylsulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide methylsulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, such as diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride. Alkyl groups generally include, but are not limited to, groups comprising C 1-8 In some embodiments, the cationic monomers may include quaternary ammonium salts or acid salts of vinyl amides, vinyl carboxylic acids, methacrylates, and derivatives thereof. Cationic monomers may be combined, for example, to form a terpolymer of dimethylaminoethyl methacrylate methyl chloride quaternary salt, diallyldimethylammonium chloride, and acrylamide.
[0034] As used herein, the terms "papermaking process" and "papermaking application" generally refer to any process in which any form of paper and / or paperboard product can be produced. For example, such processes include making paper products from pulp, such as processes including forming an aqueous cellulosic papermaking furnish, draining the furnish to form paper, and drying the paper. The steps of forming the papermaking furnish, draining, and drying can be carried out in any conventional manner generally known in the art.
[0035] As used herein, the term "polyacrylamide" or "PAM" generally refers to polymers and copolymers comprising an acrylamide moiety, and the term encompasses any polymer or copolymer comprising an acrylamide moiety, such as one or more acrylamide (co)polymers. In some cases, the PAM may include anionic PAMs (APAM), cationic PAM (CPAM) and / or sulfonated PAM (SPAM). In some embodiments, the polyacrylamide may be a cationic polyacrylamide (cPAM).
[0036] As used herein, the term "glyoxalated polyacrylamide" ("GPAM") generally refers to a polymer obtained by reacting glyoxal with a polyacrylamide base polymer. Methods for producing glyoxalated polyacrylamide are known in the art. (See, e.g., U.S. Pat. No. 3,556,932, which first disclosed the synthesis of GPAM products prepared by reacting glyoxal with cationic polyacrylamide). In some cases, the polyacrylamide backbone of GPAM can incorporate a small amount of cationic monomers to make the polymer self-retaining on the fiber. Typically, GPAM comprises a reactive polymer that can covalently bind to cellulose when dehydrated.
[0037] The present invention provides a cationic GPAM with a specific composition and properties, which is very suitable for use in papermaking methods, i.e., as an additive for increasing the wet strength and / or dry strength of paper; and it has enhanced storage and transportation properties, for example, unlike conventional GPAM used in papermaking methods, the cationic GPAM of the present invention can be stored and transported without the need to add a large amount of aqueous carrier, which is undesirable and expensive because it usually requires a large volume of containers or tankers for transportation. In some cases, the aqueous carrier may include water. In some cases, the volume of the aqueous carrier used during the transportation of the cationic GPAM discussed herein may be less than the volume of the aqueous carrier used to transport conventional GPAM. For example, in some cases, conventional GPAM may include a solid percentage of 4% or less, while in some embodiments, the cationic GPAM may include greater than 4%, i.e., greater than 4% to about 11%, for example, about greater than 4% to about 8%, about greater than 4% to about 7%, about 5% to about 7%, or about 5% to about 6%. The solid percentage.
[0038] As used herein, the term "cationic GPAM" generally refers to a GPAM composition comprising a base polymer, the base polymer comprising at least 15% by weight of a cationic monomer, optionally wherein the cationic monomer comprises DADMAC, wherein the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da, further wherein the GPAM comprises a weight ratio of glyoxal:base polymer of at least about 17:83, optionally at least about 20:80, such as at least about 23:77, such as at least about 25:75, and further optionally wherein the GPAM comprises a solids percentage of from about 2% to about 11%, such as from about greater than 4% to about 8%, such as from about greater than 4% to about 7%, such as from about 5% to about 7%, such as from about 5% to about 6%, further optionally wherein the cationic GPAM is capable of being stored and transported without the addition of a large amount of an aqueous carrier. In some cases, the GPAM content of the cationic GPAM may range from about 2% to about 11%, optionally from about 3% to about 10%, further optionally from about 4% to about 8%, further optionally from about 5% to about 7%. In some embodiments, the cationic GPAM may comprise a base polymer having a weight average molecular weight of about 25 kDa or more, 30 kDa or more, 40 kDa or more, 50 kDa or more, 75 kDa or more, 100 kDa or more, 125 kDa or more, 150 kDa or more, 175 kDa or more, 200 kDa or more, 225 kDa or more, 250 kDa or more, 275 kDa or more, 300 kDa or more, 325 kDa or more, 350 kDa or more, 375 kDa or more, 400 kDa or more, or 500 kDa or more. In some embodiments, the base polymer may comprise at least 15 wt%, at least 20 wt%, at least 25 wt%, at least 30 wt%, at least 35 wt%, at least 40 wt%, at least 50 wt%, or at least 60 wt% charge. In some embodiments, the cationic GPAM may comprise about 2% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, 4.5% or more, 5.0% or more, 5.5% or more, 6.0% or more, 6.5% or more, 7.0% or more, 7.5% or more, 8.0% or more, 8.5% or more, 9.0% or more, 9.5% or more, 10.0% or more, 10.5% or more, 11.0% or more, or 11.5% or more solids percentage.In some embodiments, the cationic GPAM may comprise a weight ratio of glyoxal to base polymer of at least about 17:83, at least about 18:82, at least about 19:81, at least about 20:80, at least about 21:79, at least about 22:78, at least about 23:77, at least about 24:76, at least about 25:75, at least about 26:74, at least about 27:73, at least about 28:72, at least about 29:71, or at least about 30:70. In some embodiments, the cationic GPAM may comprise a base polymer comprising a weight ratio of cationic monomer to acrylamide of from about 15:85 to about 60:40, optionally from about 20:80 to about 55:45, further optionally from about 25:75 to about 50:50, optionally wherein the cationic monomer comprises DADMAC. In some embodiments, the cationic GPAM may include a viscosity of about 30 cPs or greater, about 31 cPs or greater, about 32 cPs or greater, about 33 cPs or greater, about 34 cPs or greater, or about 35 cPs or greater, for example, measured by a Brookfield viscometer. In some embodiments, the cationic monomer of the polymer backbone of the cationic GPAM may include any one or more of the cationic monomers described herein. In some cases, the cationic monomer may include DADMAC and / or may include acryloxyethyl trimethyl ammonium chloride (also known as Q9). In some embodiments, the backbone polymer may include an acrylamide-based polymer, wherein the acrylamide monomer is replaced by other monomers containing primary amides, such as methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide or N-ethyl methacrylamide or any combination thereof. In some embodiments, the backbone polymer includes an acrylamide monomer. The cationic GPAM described herein may be used in any papermaking method as further described herein. Furthermore, the cationic GPAMs described herein have properties that reduce shipping costs and manufacturing costs, thereby providing benefits to manufacturers and end users of cationic GPAMs.
[0039] As used herein, the term "white water" generally refers to process water and / or process water that may be removed from the pulp furnish during the formation of a paper product (such as paper, for example, handsheets).
[0040] Compositions and methods
[0041] GPAM products and compositions containing them include known uses in the papermaking industry, typically as wet and / or dry strengthening agents. However, conventional GPAMs typically need to be stored and transported in large volumes of bulk aqueous fluid carriers, which typically require large volume containers or tankers for transportation. Transporting such large quantities of product significantly increases the cost of transporting and using GPAM products. Therefore, there is a need for improved GPAM products and compositions, such as those containing cationic GPAMs, which can be used in papermaking processes based on their composition and which have storage properties that should result in reduced transportation costs.
[0042] To this end, the present disclosure is generally directed to improved GPAM products and compositions comprising one or more cationic GPAMs, wherein the cationic GPAM comprises a base polymer, optionally an acrylamide-based base polymer, further optionally a cationic polyacrylamide base polymer, comprising at least 15 wt % of a cationic monomer, optionally wherein the cationic monomer comprises DADMAC, further wherein the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da, and wherein the GPAM comprises at least about 17:83, optionally about 20:80, For example, a weight ratio of glyoxal:base polymer of about 23:77, such as about 25:75, and further optionally wherein the GPAM comprises a solid percentage of about 2% to about 11%, such as about greater than 4% to about 8%, such as about greater than 4% to about 7%, such as about 5% to about 7%, such as about 5% to about 6%, the composition can be used in a papermaking process and it has improved storage properties that should result in reduced transportation costs, further optionally wherein the cationic GPAM can be stored and transported without adding a large amount of aqueous carrier or using a reduced volume of aqueous carrier compared to conventional GPAM used in papermaking. For example, the volume of aqueous carrier used during transportation of the cationic GPAM discussed herein may be less than the volume of aqueous carrier used to transport conventional GPAM. For example, in some cases, conventional GPAM may contain a solid percentage of 4% or less, while in some embodiments, the cationic GPAM may contain a solid percentage of greater than 4%, i.e., greater than 4% to about 11%, such as about greater than 4% to about 8%, such as about greater than 4% to about 7%, about 5% to about 7%, or about 5% to about 6%.
[0043] In addition, the present disclosure generally relates to improved GPAM products and compositions comprising cationic glyoxalated polyacrylamide ("GPAM") suitable for use as dry and / or wet strengthening agents, wherein the cationic GPAM comprises a base polymer of at least 15 wt. % of a cationic monomer, optionally wherein the cationic monomer comprises DADMAC, further wherein the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da, wherein the cationic GPAM comprises a glyoxal:glyoxal ratio of at least about 17:83, optionally about 20:80, further optionally about 23:77, further optionally about 25:75. The composition may include a GPAM having a solid content of about 2% to about 11%, such as about greater than 4% to about 8%, such as about greater than 4% to about 7%, such as about 5% to about 7%, such as about 5% to about 6%, further optionally wherein the GPAM content of the cationic GPAM is about 2% to about 11%, optionally about 3% to about 10%, further optionally about 4% to about 8%, further optionally about 5% to about 7%, further optionally wherein the cationic GPAM can be stored and transported without adding a large amount of aqueous carrier or using a reduced volume of aqueous carrier compared to conventional GPAM used in papermaking. In some embodiments, the composition may include a cationic GPAM having a GPAM content of about 2% to about 11%, optionally about 3% to about 10%, further optionally about 4% to about 8%, further optionally about 5% to about 7%.
[0044] In some embodiments, the cationic GPAM may comprise a base polymer having a weight average molecular weight of about 25 kDa or more, 30 kDa or more, 40 kDa or more, 50 kDa or more, 75 kDa or more, 100 kDa or more, 125 kDa or more, 150 kDa or more, 175 kDa or more, 200 kDa or more, 225 kDa or more, 250 kDa or more, 275 kDa or more, 300 kDa or more, 325 kDa or more, 350 kDa or more, 375 kDa or more, 400 kDa or more, 500 kDa, 1000 kDa, 1500 kDa or more.
[0045] In some embodiments, the base polymer may comprise at least 15 wt%, at least 20 wt%, at least 25 wt%, at least 30 wt%, at least 35 wt%, at least 40 wt%, at least 50 wt%, or at least 60 wt%, optionally about 20 wt%-40 wt% charge. In some embodiments, the cationic GPAM may comprise about 2% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, 4.5% or more, 5.0% or more, 5.5% or more, 6.0% or more, 6.5% or more, 7.0% or more, 7.5% or more, 8.0% or more, 8.5% or more, 9.0% or more, 9.5% or more, 10.0% or more, 10.5% or more, 11.0% or more, or 11.5% or more solids percentage. In some embodiments, the cationic GPAM may comprise a solids percentage of about greater than 4% to about 8%, optionally about greater than 4% to about 7%, further optionally about 5% to about 7%, such as about 5% to about 6%.
[0046] In some embodiments, the cationic GPAM may comprise a weight ratio of glyoxal to base polymer of at least about 17:83, at least about 18:82, at least about 19:81, at least about 20:80, at least about 21:79, at least about 22:78, at least about 23:77, at least about 24:76, at least about 25:75, at least about 26:74, at least about 27:73, at least about 28:72, at least about 29:71, or at least about 30:70. In some embodiments, the cationic GPAM may comprise a base polymer comprising a weight ratio of cationic monomer to acrylamide of from about 15:85 to about 60:40, optionally from about 20:80 to about 55:45, further optionally from about 25:75 to about 50:50, optionally wherein the cationic monomer comprises DADMAC and / or acryloyloxyethyltrimethylammonium chloride (also known as Q9).
[0047] In some embodiments, the cationic GPAM can comprise a viscosity of about 30 cPs or greater, about 31 cPs or greater, about 32 cPs or greater, about 33 cPs or greater, about 34 cPs or greater, or about 35 cPs or greater, for example, as measured by a Brookfield viscometer.
[0048] In some embodiments, the cationic monomer of the polymer backbone of the cationic GPAM may include any one or more of the cationic monomers described herein. In some cases, the cationic monomer may include DADMAC and / or may include acryloyloxyethyl trimethyl ammonium chloride (also known as Q9). The properties of such cationic GPAM compositions, such as cationic charge, solid percentage, and / or GPAM content, demonstrate desirable and effective end-use performance compared to conventional GPAMs, and the properties of the cationic GPAMs disclosed and exemplified herein should translate into a huge reduction in the volume of products that need to be transported and handled, for example, in situations involving railroad tank cars or tank truck transportation, etc., and therefore significant savings in cost and handling can be obtained using the cationic GPAMs of the present invention.
[0049] In some embodiments, the cationic polyacrylamide of the cationic GPAM may include a cationic copolymer of acrylamide or methacrylamide. In some embodiments, PAM may include a cationic copolymer of acrylamide or methacrylamide, which can be prepared by copolymerizing acrylamide or methacrylamide with one or more cationic monomers. In some embodiments, the one or more cationic monomers may include any one or more of the cationic monomers discussed herein. In some embodiments, the one or more cationic monomers may include, but are not limited to, methacryloyloxyethyl trimethylammonium chloride, acryloxyethyl trimethylammonium chloride (also known as Q9), 3-(methacrylamide) propyl trimethylammonium chloride, 3-(acrylamide) propyl trimethylammonium chloride, diallyl dimethyl ammonium chloride (DADMAC), dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, dimethylaminopropyl acrylamide, dimethylaminopropyl methacrylamide and similar monomers. In some embodiments, the cationic GPAM may include a cationic monomer including any one or more of 2-vinylpyridine, 2-vinyl-N-methylpyridinium chloride, (p-vinylphenyl)trimethylammonium chloride, diallyldimethylammonium chloride, 2-(dimethylamino)ethyl acrylate, trimethylp-vinylbenzyl)ammonium chloride, p-dimethylaminoethylstyrene, dimethylaminopropylacrylamide, 2-methacryloyloxyethyltrimethylammonium methylsulfate, or 3-acrylamido-3-methylbutyltrimethylammonium chloride, or any combination thereof. In some embodiments, the cPAM may include a copolymer of acrylamide or methacrylamide and DADMAC. In some embodiments, the cPAM may include a copolymer of acrylamide or methacrylamide and Q9 (acryloyloxyethyltrimethylammonium chloride). In some embodiments, the cPAM may include one or more cationic monomers (such as those discussed herein), a net cationic charge, and an acrylamide or methacrylamide backbone. In some embodiments, the cPAM may comprise an acrylamide-based polymer or a methacrylamide-based polymer that has been treated after polymerization to render it cationic, for example, by using a Hofmann or Mannich reaction. In some embodiments, the cPAM may comprise a cationic copolymer of acrylamide or methacrylamide that may be prepared by conventional free radical initiated polymerization methods.
[0050] In some embodiments, the backbone polymer may comprise an acrylamide-based polymer wherein the acrylamide monomer is replaced by other primary amide-containing monomers such as methacrylamide, ethylacrylamide, crotonamide, N-methylacrylamide, N-butylacrylamide, or N-ethylmethacrylamide, or any combination thereof. In some embodiments, the backbone polymer may comprise an acrylamide monomer. In some embodiments, the one or more cationic monomers may be selected from the group consisting of acryloxyethyltrimethylammonium chloride (“AETAC”), methacryloyloxyethyltrimethylammonium chloride, methacrylamidopropyltrimethylammonium chloride (“MAPTAC”), acrylamidopropyltrimethylammonium chloride, methacryloyloxyethyldimethylammonium sulfate, dimethylaminoethyl acrylate, dimethylaminopropyl methacrylamide, Q6 (methacryloyloxyethyltrimethylammonium chloride), Q6o (dimethylaminoethyl methacrylate sulfate), diallyldimethylammonium chloride (“DADMAC”); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate methyl chloride quaternary salt (“DMAEA.MCQ”), dimethylaminoethyl acrylate methyl sulfate quaternary salt (“DMAEM.MCQ”), dimethylaminoethyl acrylate benzyl chloride quaternary salt (“DMAEA.BCQ”), dimethylaminoethyl acrylate sulfate, dimethacrylate methylaminoethyl hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacryloyl hydrochloride; dialkylaminoalkyl acrylamide or dialkylaminoalkyl methacrylamide and their quaternary ammonium salts or acid salts, such as acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, such as diallyl diethylammonium chloride and diallyl dimethyl ammonium chloride.
[0051] Based on the foregoing, the present disclosure also generally relates to a papermaking method, wherein the method includes adding one or more cationic GPAM products and compositions as described above, which can be used in the papermaking method based on their composition and also have storage properties that should lead to reduced transportation costs; the method generally includes adding one or more such cationic GPAMs during the papermaking method in an amount effective to increase the wet strength and / or dry strength of the paper. In some embodiments, the cationic GPAM may include any one or more of the cationic GPAMs disclosed herein. In some embodiments, the cationic GPAM may comprise a base polymer of at least 15 wt % of a cationic monomer, optionally based on acrylamide, further optionally cationic polyacrylamide, optionally wherein the cationic monomer comprises DADMAC, further wherein the base polymer comprises a weight average molecular weight of at least 25,000 Da, optionally at least 30,000 Da, wherein the GPAM comprises a glyoxal:base polymer weight ratio of at least about 17:83, optionally about 20:80, such as about 23:77, such as about 25:75, and further optionally wherein the GPAM comprises a solids percentage of about 2% to about 11%, such as about greater than 4% to about 8%, such as about greater than 4% to about 7%, such as about 5% to about 7%, such as about 5% to about 6%.
[0052] In some embodiments, the cationic GPAMs described herein provide thermosetting resins that are particularly suitable for use as additives in papermaking processes, i.e., where the addition of the cationic GPAM produces paper having desirable dry and temporary wet strengths, and / or increases papermaking dewatering rates.
[0053] In addition, the present disclosure also relates to paper products comprising one or more of the improved GPAM products and compositions disclosed herein, such as those comprising cationic GPAMs as described above. In some embodiments, the paper products may include at least one paper layer or web containing the cationic GPAM, such as paper, paperboard, tissue, and wallboard. The cationic GPAM is not limited to use in any particular type of paper or papermaking process, and should be applied to kraft paper, sulfite paper, semi-chemical paper, and the like, including paper produced using bleached pulp, unbleached pulp, or a combination thereof.
[0054] When using a cationic GPAM composition as disclosed herein during a papermaking process, the cationic GPAM composition can be added at any time before, during, and / or after paper formation. In some cases, the cationic GPAM composition can be added to a cellulose fiber suspension at the wet end of a papermaking facility, typically when a wet strength resin is conventionally added. In some embodiments, the cationic GPAM composition can be added to pre-prepared paper by padding, spraying, dipping, and / or printing, etc. In addition, in some embodiments, the cationic GPAM composition can be added to paper pulp at a wide range of pH values, such as about 4 to about 9.
[0055] In some cases, the amount of cationic GPAM composition added during the papermaking process may range from about 0.02 to about 10 dry weight % of the cellulosic fibers, such as in the range of about 0.05 to 5 weight % of the dry paper weight.
[0056] Still further, the present disclosure generally relates to a paper product, such as handsheets, comprising one or more cationic GPAMs, such as those described above, which can be used in papermaking processes based on their composition and optionally have storage properties that should result in reduced transportation costs. In some embodiments, the paper product can include fiber-based products, such as handsheets, board-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board grades and tissue and towel grade paper materials, paper towels, diapers, sanitary napkins, training pants, pantiliners, incontinence briefs, tampons, urine pads, trash can liners, coffee filter bags, air filter materials, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent toilet paper, napkins, wrapping paper and / or other paperboard products such as paper boxes and bag paper. In some embodiments, the paper product can include a cellulose paperboard web comprising: (a) primarily cellulose fibers and (b) one or more cationic GPAMs.
[0057] In some embodiments, the paper product may include handsheets. In some embodiments, handsheets comprising one or more cationic GPAMs may include 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, 25.0% or greater STFI value improvements when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton, compared to a blank sample tested for STFI.
[0058] In some embodiments, handsheets comprising one or more cationic GPAMs may comprise 6% or greater, 7% or greater, 8% or greater, 9% or greater, 10% or greater, 12.5% or greater, 15.0% or greater, 17.5% or greater, 20.0% or greater, 22.5% or greater, 25.0% or greater, 27.5% or greater, 30.0% or greater, 32.5% or greater, 35.0% or greater, 37.5% or greater, or 40% or greater improvement in burst strength values when tested at 4.5 lbs / ton, 5.0 lbs / ton, 9.0 lbs / ton, or 10 lbs / ton as compared to a blank sample tested for burst strength.
[0059] In some embodiments, the cationic GPAM composition can achieve effective drainage, such as drainage of OCC pulp, such as showing an improvement in drainage time (e.g., the time to collect a given amount of filtrate from OCC pulp) of 25.0% or more, 30.0% or more, 35.0% or more, 40.0% or more, 45.0% or more, 50.0% or more, 55.0% or more, compared to drainage without the use of the cationic GPAM composition. In some embodiments, the cationic GPAM increases the drainage rate of the treated sample compared to drainage without the use of the cationic GPAM composition, resulting in an increase in paper production rate. In addition, the cationic GPAM composition can achieve a reduction in the total amount of solids present in the treated sample, for example, a reduction in the total solids present in the filtrate collected from OCC pulp treated with the cationic GPAM, for example, a reduction in the solids content of white water from a tray or post-sheet forming silo, such as an improvement (reduction in solids content) of 15% or more, 17.5% or more, 20.0% or more, 22.5% or more, 25.0% or more, 27.5% or more, 30.0% or more, or 32.5% or more, compared to the total amount of solids present in the sample without the cationic GPAM composition. In some embodiments, the cationic GPAM can improve drying energy savings.
[0060] In addition, the present disclosure generally relates to a method of making hand sheets, the method comprising: a. providing a pulp slurry; b. diluting the pulp slurry; c. adding one or more salts to a desired conductivity level; d. adjusting the pH to a desired value; e. adding one or more cationic GPAMs; f. adding the treated pulp to a powered paper former; g. pressing the paper produced by f.; h. drying the paper; and i. finishing the paper.
[0061] Additionally, the present disclosure generally relates to a method of making one or more paper products, wherein the method comprises: a. providing a composition comprising primarily cellulosic fibers; b. adding a predetermined amount of one or more cationic GPAMs; and c. forming the desired paper product.
[0062] In addition, the present disclosure generally encompasses a method of making one or more paper products, such as one or more absorbent paper products, wherein the method comprises: a. providing a composition comprising any of softwood fibers, hardwood fibers, recycled fibers, refined fibers, or a mixture of any of the foregoing, in an amount sufficient to form a total furnish of approximately 1% to 100% hardwood fibers, softwood fibers, recycled fibers, refined fibers, or a mixture of any of the foregoing; (b) adding a predetermined amount of a cationic GPAM as discussed herein; and (c) forming the paper product by drying on one or more drying devices to a desired moisture content level.
[0063] Additionally, the present disclosure is generally directed to a method for strengthening paper, the method comprising (i) contacting pulp fibers with a reinforcing resin comprising at least one cationic GPAM, such as at least one improved cationic GPAM product and composition disclosed herein, the GPAM having specific properties that make it well suited for use in papermaking processes, and (ii) at least partially curing the cationic GPAM in the mixture of pulp fibers and cationic GPAM to produce a paper product of enhanced strength.
[0064] In addition, the present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises a base polymer of at least 15 weight percent of a cationic monomer, wherein the cationic monomer comprises DADMAC and / or Q9 (acryloyloxyethyltrimethylammonium chloride), further wherein the base polymer comprises a weight average molecular weight of at least 30,000 Da, wherein the cationic GPAM comprises a glyoxal:base polymer weight ratio of at least about 17:83, optionally about 20:80, wherein the GPAM comprises a solids percentage of about 2% to about 11%, such as about greater than 4% to about 8%, such as about greater than 4% to about 7%, such as about 5% to about 7%, such as about 5% to about 6%, and further wherein the base polymer comprises one or more acrylamide monomers. In addition, the present disclosure generally relates to a cationic glyoxalated polyacrylamide ("GPAM") suitable for use as a dry and / or wet strengthening agent, wherein the cationic GPAM comprises a base polymer of at least 15 wt% of a cationic monomer, wherein the cationic monomer comprises DADMAC and / or Q9 (acryloyloxyethyltrimethylammonium chloride), further wherein the base polymer comprises a weight average molecular weight of at least 30,000 Da, wherein the cationic GPAM comprises a glyoxal:base polymer weight ratio of at least about 17:83, optionally about 20:80, wherein the GPAM comprises a solids percentage of from about 2% to about 11%, such as from about greater than 4% to about 8%, such as from about greater than 4% to about 7%, such as from about 5% to about 7%, such as from about 5% to about 6%, and further wherein the cationic GPAM has a GPAM content of from about 2% to about 11%, optionally from about 3% to about 10%, further optionally from about 4% to about 8%, further optionally from about 5% to about 7%.
[0065] The compositions and methods exemplarily disclosed herein may suitably be practiced in the absence of any element not specifically disclosed herein and / or with any element not specifically disclosed herein.
[0066] Example
[0067] Example 1: Sample and Handsheet Preparation
[0068] The GPAM samples and handsheets used in the following examples were prepared as follows. All GPAM samples were prepared by reacting glyoxal with a cationic polyacrylamide base polymer. Table 1 presents the composition of the cationic polyacrylamide base polymer used for the GPAM sample preparation.
[0069] Table 1 – Base polymer composition
[0070]
[0071]
[0072] *Each of Base Polymers 1-9 is composed of acrylamide and DADMAC monomers. Cationic copolymers comprising acrylamide and DADMAC monomers are used in the examples herein because such copolymers are widely used as "model" cationic polymers. Therefore, it is reasonable to expect that the results obtained using these copolymers will be obtained using other cationic polymers, such as cationic copolymers comprising other cationic monomers disclosed herein.
[0073] The compositions of the GPAM samples prepared by reacting glyoxal with the base polymer of Table 1 are described in Table 2. Each of the GPAM samples had a final viscosity of 30 to 35 cps as measured by a Brookfield viscometer equipped with a LV-1 spindle.
[0074] Table 2 – GPAM sample composition
[0075] Sample name Base polymer Glyoxal / base polymer weight ratio solid% Comparison sample 1 Base polymer 1 29:71 11% Comparison sample 2 Base polymer 2 23:77 7% Sample 1 Base polymer 3 29:71 5.5% Sample 2 Base polymer 4 29:71 5% Sample 3 Base polymer 5 29:71 3% Sample 4 Base polymer 6 26:74 5% Sample 5 Base polymer 6 23:74 5% Sample 6 Base polymer 6 17:83 5% Sample 7 Base polymer 7 29:71 3.5% Sample 8 Base polymer 8 29:71 2.5% Sample 9 Base polymer 9 29:71 7%
[0076] Handsheets were prepared as follows. OCC pulp thick slurry was obtained from a recycled liner paper mill. First, the thick slurry was expanded to 0.5% consistency using tap water. NaCl was then added to the diluted pulp to match the conductivity of the paper mill white water. 1M HCl solution was added to the pulp to adjust the pH to 6.4. After pH adjustment, the GPAM product was introduced into the diluted pulp under overhead stirring. Next, the treated pulp was added to a dynamic paper former (DSF) (TECHPAP France, FDA type) to produce 110gsm paper. After the paper was produced, the formed paper was pressed with blotting paper at 15psi using a pneumatic roller press and then dried on a rotary dryer at 110°C. The dried paper was then oven cured at 105°C for 5 minutes using a forced ventilation conventional oven and then conditioned overnight in a standard TAPPI control room. After overnight conditioning, the paper strips were cut in the transverse direction and the STFI test was performed as generally described in TAPPI standard method T-826. Burst strength testing was performed as generally described in TAPPI Standard Method T-403.
[0077] Example 2: GPAM concentration
[0078] In this embodiment, the maximum GPAM concentration and critical base polymer concentration of base polymer 6, base polymer 7 and base polymer 8 (see Table 1) were evaluated. The maximum GPAM concentration is related to the concentration of the polyacrylamide and glyoxal mixture, above which the glyoxalation reaction proceeds rapidly, and the mixture viscosity reaches 30cps at a pH between 8.5 and 9.0 in less than 30 minutes. The critical base polymer concentration is related to such a concentration, above which the viscosity of the reaction mixture increases due to the forward direction of adduct formation, and below which the viscosity of the reaction mixture decreases due to the forward direction of adduct formation. The maximum GPAM concentration and critical base polymer concentration of base polymer 6, base polymer 7 and base polymer 8 are presented in Table 3.
[0079] Table 3 – Maximum GPAM concentrations and critical base polymer concentrations
[0080]
[0081] As shown in Table 3, the maximum GPAM concentration is generally proportional to the base polymer charge density. For example, Base Polymer 6 and Base Polymer 8 have a weight average molecular weight of approximately 300 kDa, and the 40% charged base polymer (Base Polymer 6) contains a maximum GPAM concentration of 5.5%, compared to the 20% charged base polymer (Base Polymer 8) which contains a maximum GPAM concentration of 4.0%.
[0082] Example 3: Handsheet Strength Test
[0083] Handsheets were prepared using various GPAM samples as described in Example 1. After preparation, the handsheets were subjected to strength tests, including STFI strength test and burst strength test. The results of the strength tests are presented in Tables 4 and 5. The compositions of the samples used are described in Table 2 of Example 1.
[0084] Table 4 – STFI strength test results
[0085]
[0086] Table 5 – Bursting Strength Test Results
[0087]
[0088] Comparative Sample 1 and Comparative Sample 2 were each prepared using a low weight average molecular weight base polymer (see Table 2 and Example 1). Sample 1, Sample 2, and Sample 3 were each prepared using a base polymer having a weight average molecular weight of more than 100 kDa (see Table 2 and Example 1). As shown in Tables 4 and 5, each of Sample 1, Sample 2, and Sample 3 exhibited higher STFI and rupture results compared to Comparative Sample 1 and Comparative Sample 2. In addition, Sample 2 having a GPAM content of 5% provided comparable strength compared to Sample 3 having a GPAM content of 3%. Note that a higher GPAM content is generally preferred because a higher GPAM content can result in lower shipping and handling costs.
[0089] Example 4: Retention / Drainage Test
[0090] In this example, retention / drainage tests were performed on various GPAM samples. Various GPAM samples were prepared according to Example 1. Retention / drainage tests were performed using a dynamic drainage analyzer 5 (DDA 5) (PulpEye). The OCC pulp used for the test was obtained from a boxboard mill without any wet end chemical additions. In a typical experiment, 1000 mL of OCC pulp was added to DDA 5 and the overhead stirrer was started at 1100 rpm. Then, one of the GPAM products was added to DDA 5 at 5 pounds per ton. Ten seconds after the GPAM was added, a flocculant with a high weight average molecular weight (10 mol% cation, SV=5) was added to DDA 5. After another 10 seconds, the overhead stirring speed was adjusted to 700 rpm. After the last 10 seconds of stirring, the overhead stirrer was stopped and the OCC pulp was discharged under a vacuum of 200 mbar. The time to collect 800 ml of filtrate was recorded as the drainage time. The total suspended solids (TSS) of the filtrate were also measured using a HACH turbidometer.
[0091] With respect to the results presented in Table 6, a lower drainage time indicates a faster drainage rate during the tests conducted, and a lower TSS indicates a higher retention efficiency during the tests conducted. The results obtained for the retention / drainage tests are presented in Table 6. The compositions of the samples used in this example are described in Table 2 of Example 1.
[0092] Table 6 – Retention / Drainage Test Results
[0093]
[0094] As shown in Table 6, Comparative Example 1 reduced the drainage time by about 5%. In contrast, Sample 2 and Sample 3 reduced the drainage time by 45% and 52%. In addition, Comparative Example 1 reduced the total suspended solids content (TSS) by 11%, while Sample 2 and Sample 3 reduced TSS by 26% and 30%, respectively. Therefore, Sample 2 and Sample 3 provide improved drainage rate and improved retention efficiency compared to Comparative Example 1.
[0095] Example 5: Handsheet Strength Test
[0096] Handsheets were prepared using various GPAM samples as described in Example 1. After preparation, the handsheets were subjected to strength tests, including STFI strength test and burst strength test. The results of the strength tests are presented in Table 7, Table 8 and Table 9. The compositions of the samples used are described in Table 2 of Example 1.
[0097] Table 7 – STFI strength test results
[0098] 4.5 lbs / ton 9 lbs / ton sample STFI improve STFI improve blank 8.71 NA 8.71 NA Sample 2 9.93 14.0% 10.65 22.3% Sample 4 9.65 10.8% 10.35 18.8% Sample 5 9.52 9.3% 10.02 15.0% Sample 6 8.96 7.2% 9.29 11.0%
[0099] Table 8 – STFI strength test results
[0100]
[0101] Table 9 – Bursting Strength Test Results
[0102]
[0103]
[0104] Reference is now made to Table 7, which presents a comparison of the strength properties of handsheets prepared with various GPAM samples, the samples being prepared using a base polymer having a weight average molecular weight of 246 kDa (see Tables 2 and 1). The various GPAM samples of Table 7 have different glyoxal / base polymer ratios (see Table 2). As shown in Table 7, higher glyoxal / base polymer ratios generally result in higher STFI values. For example, at a 4.5 lb / ton GPAM dosage, a ratio of 17:83 results in a 7.2% increase in STFI, while a ratio of 29:71 results in a 14.0% increase in STFI. Additionally, at a 9.0 lb / ton GPAM dosage, a ratio of 17:83 results in a 11.0% increase in STFI, while a ratio of 29:71 results in a 22.3% increase in STFI.
[0105] Tables 8 and 9 present a comparison of the STFI strength properties and burst strength properties of various GPAM samples, respectively. For the GPAM samples tested, the weight average molecular weight of the base polymer was about 200 kDa to about 350 kDa. In addition, as shown in Tables 8 and 9, the base polymer charge percentage varied from about 20% to about 60%.
[0106] Referring now to Table 8, Sample 2, Sample 7, Sample 8, and Sample 9 all showed improvements in STFI compared to the blank sample. For example, for the 4.5 lb / ton and 9 lb / ton STFI strength tests, Sample 2 showed improvements of 15.7% and 20.9%, respectively; for the 4.5 lb / ton and 9 lb / ton STFI strength tests, Sample 7 showed improvements of 14.1% and 22.0%, respectively; and for the 4.5 lb / ton and 9 lb / ton STFI tests, Sample 8 showed improvements of 15.2% and 19.1%, respectively.
[0107] Referring now to Table 9, Sample 2, Sample 7, Sample 8, and Sample 9 all showed improvements in burst strength values compared to the blank sample. For example, for 4.5 lbs / ton and 9 lbs / ton burst strengths, Sample 2 showed 24.4% and 38.2% improvements, respectively; for 4.5 lbs / ton and 9 lbs / ton burst strengths, Sample 7 showed 21.2% and 34.8% improvements, respectively; and for 4.5 lbs / ton and 9 lbs / ton burst strengths, Sample 8 showed 21.9% and 33.8% improvements, respectively.
[0108] In the foregoing procedures, various steps have been described. However, it will be apparent that various modifications and changes may be made thereto, and that additional processes may be implemented, without departing from the broader scope of the exemplary processes as set forth in the appended claims.
Claims
1. A cationic glyoxalated polyacrylamide suitable for use as a dry and / or wet strengthening agent, wherein the cationic glyoxalated polyacrylamide comprises: i. a base polymer comprising at least 15 wt % of a cationic monomer, and wherein the base polymer comprises a weight average molecular weight of at least 25 kDa; ii. a glyoxal:base polymer weight ratio of at least 17:83; and iii. a solid percentage greater than 4% to 11%; Optionally, the cationic glyoxalated polyacrylamide can be stored and transported without adding large amounts of aqueous carriers or using reduced volumes of aqueous carriers compared to conventional glyoxalated polyacrylamides used in papermaking.
2. A cationic glyoxalated polyacrylamide suitable for use as a dry and / or wet strengthening agent, wherein the cationic glyoxalated polyacrylamide comprises: i. a base polymer comprising at least 15 wt % of a cationic monomer, and wherein the base polymer comprises a weight average molecular weight of at least 25 kDa; ii. a glyoxal:base polymer weight ratio of at least 17:83; iii. a solids percentage of greater than 4% to 11%; and iv. a glyoxalated polyacrylamide content of greater than 4% to 11%; Optionally, the cationic glyoxalated polyacrylamide can be stored and transported without adding large amounts of aqueous carriers or using reduced volumes of aqueous carriers compared to conventional glyoxalated polyacrylamides used in papermaking.
3. The cationic glyoxalated polyacrylamide of claim 1 or claim 2, wherein: i. The cationic glyoxalated polyacrylamide has a glyoxalated polyacrylamide content of greater than 4% to 11%; ii. the base polymer comprises a weight average molecular weight of 30 kDa or greater; iii. the base polymer comprises at least 15 wt% charge; iv. the cationic glyoxalated polyacrylamide comprises a glyoxal:base polymer weight ratio of at least 18:82; v. the cationic glyoxalated polyacrylamide comprises a base polymer comprising a cationic monomer:acrylamide weight ratio of 15:85 to 60:40; vi. the base polymer comprises a backbone polymer comprising one or more cationic monomers; vii. The cationic glyoxalated polyacrylamide comprises a viscosity of 30 cPs or greater; viii. The main chain polymer comprises a copolymer of acrylamide or methacrylamide and one or more cationic monomers; ix. The backbone polymer comprises an acrylamide-based polymer; x. The main chain polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from diallyldimethylammonium chloride and / or acryloyloxyethyltrimethylammonium chloride; xi. the backbone polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from diallyldimethylammonium chloride and / or acryloxyethyltrimethylammonium chloride, and the charge of the base polymer optionally ranges from 15% to 60%; xii. The aqueous carrier comprises water; xiii. The cationic glyoxalated polyacrylamide comprises a solid percentage of greater than 4% to 8%; xiv. the base polymer comprises at least 20 wt% of a cationic monomer; and / or xv.A combination of any two or more of (i)-(xiv).
4. The cationic glyoxalated polyacrylamide according to claim 3, wherein In implementation scheme vi: i. the one or more cationic monomers are selected from the group consisting of dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, dialkylaminoalkyl acrylamides or dialkylaminoalkyl methacrylamides and their quaternary ammonium salts or acid salts, and diallyldialkylammonium halides; ii. the one or more cationic monomers include diallyldimethylammonium chloride; iii. the one or more cationic monomers include acryloyloxyethyltrimethylammonium chloride; iv. the one or more cationic monomers include diallyldimethylammonium chloride and / or acryloyloxyethyltrimethylammonium chloride; v. the one or more cationic monomers are selected from the group consisting of methacryloyloxyethyltrimethylammonium chloride, acryloxyethyltrimethylammonium chloride, 3-(methacrylamido)propyltrimethylammonium chloride, 3-(acrylamido)propyltrimethylammonium chloride, diallyldimethylammonium chloride, dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate and dimethylaminopropylacrylamide, dimethylaminopropylmethacrylamide; and / or vi. A combination of any two or more of (i)-(v).
5. The cationic glyoxalated polyacrylamide according to claim 4, wherein In embodiment i, the one or more cationic monomers are selected from the group consisting of acryloyloxyethyltrimethylammonium chloride, methacryloyloxyethyltrimethylammonium chloride, methacrylamidopropyltrimethylammonium chloride, acrylamidopropyltrimethylammonium chloride, methacryloyloxyethyldimethylammonium sulfate, dimethylaminoethyl acrylate, dimethylaminopropyl methacrylamide, dimethylaminoethyl methacrylate sulfate, and diallyldimethylammonium chloride.
6. The cationic glyoxalated polyacrylamide according to claim 3, wherein In implementation ix: i. the backbone polymer comprises one or more primary amide-containing monomers; ii. the backbone polymer comprises one or more monomers selected from the group consisting of acrylamide, methacrylamide, ethylacrylamide, crotonamide, N-methylacrylamide, N-butylacrylamide, N-ethylmethacrylamide, and any combination thereof; iii. the backbone polymer comprises one or more acrylamide monomers; and / or iv. A combination of any two or more of (i) to (iii).
7. A paper product comprising one or more cationic glyoxalated polyacrylamides according to any one of claims 1 to 6.
8. The paper product of claim 7, wherein the paper product: i. comprising at least one paper layer or paper web containing the cationic glyoxalated polyacrylamide; ii. including one or more of paper, paperboard and wallboard; iii. comprising one or more of kraft paper, sulfite paper, semi-chemical paper, or a combination thereof; iv. Including fiber-based products; v. including one or more of hand sheets, board-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board-grade and tissue and towel-grade paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, trash can liners, coffee filter bags, air filter materials, drying pads, floor cleaning pads, wrapping paper and / or other paperboard products; vi. comprising a cellulose paperboard web, said cellulose paperboard web optionally comprising primarily cellulose fibers; vii. comprising 0.02% to 10% cationic glyoxalated polyacrylamide based on the dry weight of cellulose fibers; viii. comprising a 6% or greater STFI value improvement when tested at 4.5 lbs / ton compared to a blank sample of the STFI test for the paper product; ix. comprising a 6% or greater improvement in burst strength value when tested at 4.5 lbs / ton compared to a blank sample used for burst strength testing; and / or x. Any combination of two or more of (i)-(ix).
9. A process for making paper, wherein the process comprises adding during the process one or more cationic glyoxalated polyacrylamides according to any one of claims 1 to 6 in an amount effective to increase the wet strength and / or dry strength of a paper product produced by the process.
10. A method of making one or more paper products, wherein the method comprises: (a) providing a composition comprising mainly cellulose fibers; (b) adding a predetermined amount of one or more cationic glyoxalated polyacrylamides as claimed in any one of claims 1 to 6; and (c) forming a desired paper product.
11. A method of making one or more paper products, wherein the method comprises: (a) providing a composition comprising softwood fiber, hardwood fiber, recycled fiber, refined fiber, or mixtures thereof in an amount sufficient to form a total furnish of 1% to 100% hardwood fiber, softwood fiber, recycled fiber, refined fiber, or mixtures thereof; (b) adding a predetermined amount of one or more cationic glyoxalated polyacrylamides as described in any one of claims 1 to 6; and (c) forming a paper product by drying on one or more drying devices to a desired moisture content level.
12. A method for strengthening paper, the method comprising contacting pulp fibers with a reinforcing resin comprising at least the cationic glyoxalated polyacrylamide according to any one of claims 1 to 6, and at least partially curing the cationic glyoxalated polyacrylamide in a mixture of pulp fibers and cationic glyoxalated polyacrylamide to produce a paper product having enhanced strength.
13. The method of any one of claims 9 to 12, wherein: i. adding the cationic glyoxalated polyacrylamide to a cellulosic fiber suspension at the wet end of a papermaking facility; ii. The cationic glyoxalated polyacrylamide is added to 0.02% to 10% by dry weight of the cellulose fiber; iii. adding the cationic glyoxalated polyacrylamide before, during and / or after forming the paper; iv. the paper product comprises an STFI value improvement of 6% or greater when tested at 4.5 lbs / ton compared to a blank sample of the STFI test for the paper product; v. The paper product comprises a 6% or greater improvement in burst strength value when tested at 4.5 lbs / ton compared to a blank sample for burst strength testing; vi. the paper product comprises one or more of hand sheets, board-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board grade and tissue and towel grade paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, trash can liners, coffee filter bags, air filter materials, drying pads, floor cleaning pads, and / or wrapping paper; vii. The paper product comprises a cellulose paperboard web, the cellulose paperboard web optionally comprising primarily cellulose fibers; viii. The cationic glyoxalated polyacrylamide composition increases the drainage time of the treated sample by 25.0% or more compared to the drainage without the cationic glyoxalated polyacrylamide composition; ix. The cationic glyoxalated polyacrylamide composition improves the drainage rate of the treated sample compared to the drainage without the cationic glyoxalated polyacrylamide composition, resulting in an increase in paper production rate; x. The cationic glyoxalated polyacrylamide improves drying energy saving; xi. The cationic glyoxalated polyacrylamide reduces the total solids content of the treated sample by 15% or more compared to the total solids present in the sample without the cationic glyoxalated polyacrylamide composition; and / or xii.A combination of any two or more of (i)-(xi).
14. A cationic glyoxalated polyacrylamide suitable for use as a dry and / or wet strengthening agent, wherein the cationic glyoxalated polyacrylamide comprises: i. a base polymer comprising (1) one or more acrylamide monomers and (2) at least 15 weight percent of a cationic monomer, wherein the cationic monomer comprises diallyldimethylammonium chloride and / or acryloxyethyltrimethylammonium chloride, and wherein the base polymer comprises a weight average molecular weight of at least 100 kDa; ii. a glyoxal:base polymer weight ratio of at least 17:83; iii. a solids percentage greater than 4% to 11%, The cationic glyoxalated polyacrylamide can be stored and transported without adding a large amount of aqueous carrier containing water.
15. A cationic glyoxalated polyacrylamide suitable for use as a dry and / or wet strengthening agent, wherein the cationic glyoxalated polyacrylamide comprises: i. a base polymer comprising (1) one or more acrylamide monomers and (2) at least 15 weight percent of a cationic monomer, wherein the cationic monomer comprises diallyldimethylammonium chloride and / or acryloxyethyltrimethylammonium chloride, and wherein the base polymer comprises a weight average molecular weight of at least 100 kDa; ii. a glyoxal:base polymer weight ratio of at least 17:83; iii. a solids percentage of greater than 4% to 11%; and iv. a glyoxalated polyacrylamide content of greater than 4% to 11%, The cationic glyoxalated polyacrylamide can be stored and transported without adding a large amount of aqueous carrier containing water.
16. The cationic glyoxalated polyacrylamide according to claim 14 or 15, wherein: i. The cationic glyoxalated polyacrylamide comprises a glyoxal:base polymer weight ratio of at least 18:82; ii. the base polymer comprises a weight average molecular weight of 150 kDa or greater; iii. the base polymer comprises a backbone polymer comprising acrylamide and / or methacrylamide monomers and a cationic monomer selected from diallyldimethylammonium chloride and / or acryloyloxyethyltrimethylammonium chloride or consisting thereof; iv. the main chain polymer comprises acrylamide and / or methacrylamide monomers and a cationic monomer selected from diallyldimethylammonium chloride and / or acryloyloxyethyltrimethylammonium chloride or consists of; v. the backbone polymer comprises or consists of acrylamide and / or methacrylamide monomers and a cationic monomer selected from diallyldimethylammonium chloride and / or acryloxyethyltrimethylammonium chloride, and the charge of the base polymer optionally ranges from 15% to 60%; vi. the aqueous carrier comprises water; vii. The cationic glyoxalated polyacrylamide comprises a solid percentage of greater than 4% to 8%; and / or viii. A combination of any two or more of (i)-(vii).
Citation Information
Patent Citations
Water-soluble,ionic,glyoxylated,vinylamide,wet-strength resin and paper made therewith
US3556932A
High Solids Glyoxalated Polyacrylamide
US20080308242A1
High Molecular Weight and High Cationic Charge Glyoxalated Polyacrylamide Copolymers and Their Methods of Manufacture and Use
US20160201269A1