A high-barrier yin-yang bag capable of high temperature sterilization and its preparation method and application

By using PET/PET-ALOx/CPP and PET/PET/AL/RCPP composite layer structures and dry lamination technology in high-barrier male and female bags, the problem that the existing technology cannot be effectively sterilized under high temperature conditions is solved and achieved Semi-high temperature sterilization at 115℃ and excellent preservation effect.

CN115534467BActive Publication Date: 2024-10-11PINGJIANG JINZAI FOOD CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202111651590.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-10-11
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

Existing high-barrier Yin and Yang bags cannot be effectively sterilized under high temperature conditions, resulting in packaging bags that are prone to wrinkles, air leakage, bag breakage, food leakage and other problems after cooking, and cannot meet the needs of semi-high temperature sterilization packaging.

Method used

Adopting a specific composite film structure, including a PET/PET-ALOx/CPP composite layer of the front structure and a PET/PET/AL/RCPP composite layer of the back structure, and using dry lamination and constant temperature curing technology, using an adhesive that is resistant to moisture, heat and high temperatures. Form an interpenetrating polymer network, increase the cross-linking density, and ensure the integrity and barrier properties of the packaging bag in high temperature environments.

Benefits of technology

The packaging bag can be semi-high temperature sterilized at 115°C, maintaining the integrity and barrier properties of the packaging bag, avoiding delamination, and ensuring the long-term preservation of the food's freshness and flavor.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of packaging bags, and in particular to a high-barrier yin-yang bag that can be sterilized at high temperature and a preparation method thereof, comprising a bag body, wherein the bag body comprises a symmetrical front structure and a back structure, wherein the front structure is compounded by a first PET film, a PET-ALOx film, and a CPP film in sequence, and the back structure is compounded by a first PET film, a second PET film, an aluminum foil, and a CPP film in sequence. After a sterilization test of 115°C×30min, the yin-yang bag of the present invention with a front PET / PET-ALOx / RCPP and a back PET / PET / AL / RCPP structure does not have the problems of packaging bag deformation, stratification, and content leakage, and can meet the sterilization conditions for food packaging applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of packaging bags, specifically to IPC classification number B32B27 / 08, and more specifically to a high-temperature sterilizable high-barrier yin-yang bag and a preparation method and application thereof. Background Art

[0002] Chinese patent CN201610441375.0 discloses a leak-proof, pressure-resistant, high-temperature-resistant, high-barrier vertical food oil bag and a preparation method thereof. The high-barrier packaging material composite film includes a scratch-resistant polyethylene film layer, an adhesive layer, a vacuum polyester aluminum-plated film layer (VMPET), an adhesive layer, a high-barrier plastic film layer, an adhesive layer, and a biaxially oriented polypropylene film (BOPP) layer. Through a multi-layer specific structural design, it has high barrier air tightness, oil resistance, moisture resistance, odor retention, and moisture retention properties, but does not solve the problem of high-temperature sterilization resistance.

[0003] In addition, many high-barrier yin-yang bags on the market currently have a structure of PET / VMPET / CPP, which can only be used for room temperature packaging (below 100°C) and cannot be used for semi-high temperature sterilization packaging (100°C~121°C). Therefore, the development of a high-barrier yin-yang packaging bag that is resistant to high temperature sterilization has very important application value. Summary of the invention

[0004] In response to the above-mentioned technical problems, on the one hand, the present invention provides a high-barrier yin-yang bag that can be sterilized at high temperature, including a bag body, wherein the bag body includes a symmetrical front structure and a back structure, wherein the front structure is sequentially composited by a first PET film, a PET-ALOx film, and a CPP film, and the back structure is sequentially composited by a first PET film, a second PET film, an aluminum foil, and a CPP film.

[0005] In some embodiments, the first PET film has a thickness of 10-15 μm.

[0006] Preferably, the thickness of the first PET film is 12 μm.

[0007] In some embodiments, the width of the first PET film is 500 mm.

[0008] In some embodiments, the PET-ALOx film has a thickness of 10-15 μm.

[0009] Preferably, the PET-ALOx film has a thickness of 12 μm.

[0010] In some embodiments, the PET-ALOx film has a width of 250 mm.

[0011] In some embodiments, the oxygen transmission rate of the PET-ALOx film is ≤1 cc / m2 *24h*0.1Mpa, water vapor transmission rate ≤1g / m 2 *24h*0.1Mpa.

[0012] In some embodiments, the aluminum foil has a thickness of 10-15 μm.

[0013] Preferably, the thickness of the aluminum foil is 12 μm.

[0014] In some embodiments, the width of the aluminum foil is 250 mm.

[0015] In some embodiments, the second PET film has a thickness of 5-10 μm.

[0016] Preferably, the thickness of the second PET film is 7 μm.

[0017] In some embodiments, the width of the second PET film is 250 mm.

[0018] In some embodiments, the CPP film has a thickness of 60-80 μm.

[0019] Preferably, the CPP film has a thickness of 70 μm.

[0020] In some embodiments, the width of the CPP film is 500 mm.

[0021] In some embodiments, the CPP film is a retort-grade CPP film, namely, a RCPP film.

[0022] At present, food packaging bags need to be sterilized by high-temperature cooking after packaging. In particular, vacuum packaging is usually used for foods such as meat and soy products. After high-temperature sterilization, they can be stored at room temperature. Many high-barrier yin-yang bags on the market have a structure of PET / VMPET / CPP, which can only be used for room temperature packaging (below 100°C) and cannot be used for semi-high temperature sterilization packaging (100°C-121°C). In the actual production process, many quality problems will occur, such as wrinkling, air leakage, bag breakage, and even food leakage after cooking. After a lot of research, the applicant found that the front structure of the yin-yang bag is set to a PET / PET-ALOx / CPP composite layer of a specific thickness, and the back structure is set to a PET / PET / AL / RCPP composite layer of a specific thickness through a special composite method. Not only the front side is transparent, but the back side has an opaque effect of blocking light. At the same time, the yin-yang bag obtained by composite can be used for semi-high temperature sterilization at 115°C, and it is also guaranteed to have excellent barrier properties. In addition, during the cooking process, the packaging bags are prone to delamination in a high temperature environment, and the preservation effect cannot be achieved. After a large number of experiments, the applicant found that the use of a specific adhesive for dry compounding and aging under specific conditions can make the prepared yin-yang bag still maintain the integrity of the packaging bag and prevent delamination after cooking. The applicant believes that the possible reason is that the adhesive used in the present invention introduces a molecular structure that is resistant to moisture, heat and high temperature, and at the same time, the interpenetrating polymer network formed between molecules increases the cross-linking density. At the same time, constant temperature aging at 50°C promotes the complete aging of the adhesive between the composite layers, thereby making the composite structural layers more stable, and having excellent high temperature resistance and hydrolysis performance, thereby ensuring the good water boiling resistance of the yin-yang bag.

[0023] The second aspect of the present invention provides a method for preparing a high-barrier yin-yang bag that can be sterilized at high temperature, comprising at least the following steps:

[0024] (1) dividing the entire page of the first PET film into page A and page B in half, and printing the entire page;

[0025] (2) After printing is completed, the non-printing surface of the first PET film of the A plate is dry-laminated with the PET-ALOx film to obtain a composite layer a;

[0026] (3) dry-laminating the non-printing surface of the first PET film on the B plate with the second PET film to obtain a composite layer b;

[0027] (4) Dry-compounding the composite layer b with the aluminum foil to obtain a composite layer c;

[0028] (5) Dry-compounding the composite layer a and the composite layer c with the CPP film at the same time to obtain a composite product;

[0029] (6) placing the composite product in a constant temperature curing chamber for curing;

[0030] (7) Bag-making is performed on the matured product to obtain the yin-yang bag.

[0031] In some embodiments, the printing device in step (1) is a 9-color gravure printing machine.

[0032] In some embodiments, the adhesive used in the dry compounding includes two components A and B. In terms of weight, the component A consists of: 65-75 parts of isocyanate, 15-20 parts of polyol, and 10-12 parts of silane coupling agent; the component B is polyester polyol.

[0033] In some embodiments, the isocyanate in the A component includes at least one of dicyclohexylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, lysine diisocyanate, hexamethylene diisocyanate, and aliphatic isocyanate.

[0034] The preparation method of the component A comprises: heating the polyol component at 135-145° C. for 3.5 hours, cooling to 45° C., adding isocyanate and silane coupling agent and reacting for 2.5 hours to obtain the component A.

[0035] In some embodiments, the silane coupling agent includes one of KH550 or KH560.

[0036] In some embodiments, the polyol in component A includes at least one of ethylene glycol, pentaerythritol, 2-propylene glycol, 1,6-hexanediol, 1,4-butanediol, diethylene glycol, neopentyl glycol, dipropylene glycol, trimethylolpropane, polyoxypropylene triol, and diethylene glycol.

[0037] In some embodiments, the preparation method of the polyester polyol is as follows: add polyacid and polyol to a reaction kettle in sequence, heat and stir, raise the temperature to 175°C-185°C and keep it warm for 2-4 hours, and then raise the temperature of the reaction kettle to 215°C to obtain the B component.

[0038] In some embodiments, the polyacid in the B component includes a mixture of terephthalic acid, isophthalic acid, and azelaic acid, and the weight ratio is 1:(0.8-1.2):(0.5-1), preferably 1:1:0.7.

[0039] In some embodiments, the polyol in the B component includes hexanediol and butanediol in a weight ratio of 1:0.75.

[0040] In some embodiments, the weight ratio of component A to component B is 1:(4-6), preferably 1:5.

[0041] In some embodiments, the width of the glue pressing roller used for compounding in step (5) is twice the width of the glue pressing roller used for compounding in steps (3) and (4).

[0042] In some embodiments, the temperature of the constant temperature aging chamber in step (6) is 45-55°C.

[0043] Preferably, the temperature of the constant temperature aging chamber in step (6) is 50°C.

[0044] In some embodiments, the time of the constant temperature aging chamber in step (6) is 65-80 hours.

[0045] Preferably, the time in the constant temperature aging chamber in step (6) is 72 hours.

[0046] In some embodiments, the compounding equipment is a three-stage oven dry compounding machine.

[0047] The third aspect of the present invention provides an application of a high-temperature sterilizable high-barrier yin-yang bag in the field of food packaging.

[0048] Beneficial effects:

[0049] (1) The present invention sets the front structure of the yin-yang bag to a PET / PET-ALOx / CPP composite layer of a specific thickness, and the back structure to a PET / PET / AL / RCPP composite layer of a specific thickness through a special composite method, which not only achieves the effect of light transmission and transparency on the front side, but also has the effect of blocking light and being opaque on the back side;

[0050] (2) The compounded yin-yang bag of the present invention can be used for semi-high temperature sterilization at 115°C, solving the problem that the current yin-yang bag cannot be sterilized by steaming;

[0051] (3) The present invention uses a specific adhesive for dry compounding and performs aging under specific conditions, so that the prepared yin-yang bag can still maintain the integrity of the packaging bag and not delaminate after being steamed;

[0052] (4) The present invention promotes the complete maturation of the adhesive between the composite layers by controlling the maturation conditions, thereby making the composite structural layers more stable, having excellent high temperature resistance and hydrolysis performance, and ensuring the good boiling resistance of the yin-yang bag;

[0053] (5) The yin-yang bag prepared by the present invention has excellent barrier properties, can block moisture, water vapor, oxygen, etc., inhibit the growth of microorganisms, and can maintain the flavor and quality of food for a long time. DETAILED DESCRIPTION

[0054] Example 1

[0055] A first aspect of the present embodiment provides a high-barrier yin-yang bag that can be sterilized at high temperature, including a bag body, wherein the bag body includes a symmetrical front structure and a back structure, wherein the front structure is sequentially composited by a first PET film, a PET-ALOx film, and a CPP film, and the back structure is sequentially composited by a first PET film, a second PET film, an aluminum foil, and a CPP film.

[0056] The first PET film has a thickness of 12 μm and a width of 500 mm.

[0057] The PET-ALOx film has a thickness of 12 μm and a width of 250 mm.

[0058] The oxygen permeability of the PET-ALOx film is 1cc / m 2 *24h*0.1Mpa, water vapor transmission rate 1g / m 2 *24h*0.1Mpa, the PET-ALOx film was purchased from Foshan Cailong Coating Packaging Materials Co., Ltd.

[0059] The aluminum foil has a thickness of 12 μm and a width of 250 mm.

[0060] The second PET film has a thickness of 7 μm and a width of 250 mm.

[0061] The CPP film has a thickness of 70 μm and a width of 500 mm.

[0062] The CPP film is an RCPP film.

[0063] The second aspect of this embodiment provides a method for preparing a high-barrier yin-yang bag that can be sterilized at high temperature, comprising the following steps:

[0064] (1) dividing the entire page of the first PET film into page A and page B in half, and printing the entire page;

[0065] (2) After printing is completed, the non-printing surface of the first PET film of the A plate is dry-laminated with the PET-ALOx film to obtain a composite layer a;

[0066] (3) Dry-laminating the non-printing surface of the first PET film on the B plate with the second PET film, with a glue pressing roller width of 240 mm, to obtain a composite layer b;

[0067] (4) Dry-compounding the composite layer b with the aluminum foil, with a glue pressing roller width of 240 mm, to obtain a composite layer c;

[0068] (5) Dry-compounding the composite layer a and the composite layer c with the CPP film at the same time, with the glue pressing roller having a width of 480 mm, to obtain a composite product;

[0069] (6) placing the composite product in a constant temperature curing room at 50°C for 72 hours;

[0070] (7) Bag-making is performed on the matured product to obtain the yin-yang bag.

[0071] The adhesive used in the dry compounding comprises two components, A and B. In terms of weight parts, the component A consists of the following: 70 parts of isocyanate, 18 parts of polyol, and 11 parts of silane coupling agent; the component B is polyester polyol.

[0072] The isocyanate in the A component is isophorone diisocyanate.

[0073] The preparation method of the component A comprises: heating the polyol component at 140° C. for 3.5 hours, cooling to 45° C., adding isocyanate and silane coupling agent and reacting for 2.5 hours to obtain the component A.

[0074] The silane coupling agent is KH560.

[0075] The polyol in the A component includes 1,6-hexanediol and dipropylene glycol in a weight ratio of 1:1.

[0076] The preparation method of the polyester polyol is as follows: polyacid and polyol are added into a reaction kettle in sequence, heated and stirred, heated to 180° C. and kept warm for 3 hours, and then the temperature of the reaction kettle is heated to 215° C. to obtain the B component.

[0077] The polyacid in the B component includes a mixture of terephthalic acid, isophthalic acid and azelaic acid, and the weight ratio is 1:1:0.7.

[0078] The polyol in the B component includes hexanediol and butanediol in a weight ratio of 1:0.75.

[0079] The weight ratio of component A to component B is 1:5.

[0080] Performance Testing

[0081] 1. Yin-Yang Bag Sterilization Experiment

[0082] The specific method is as follows:

[0083] (1) Take the Yin-Yang bag prepared in Example 1, put it into the deep-sea fish product of Jinzi Food Co., Ltd. with a net content of 36 g, and seal it with a vacuum sealer;

[0084] (2) Put 50 packages of packaged products into the FY50 fully automatic reverse high-temperature cooking pot of Shanghai Sanshen Medical Instrument Co., Ltd., cover the pot, set the sterilization temperature to 115°C, set the sterilization time to 30 minutes, turn on the switch, and start the test;

[0085] (3) After sterilization, check whether the packaging bag is deformed, stratified, or leaking after sterilization, and record the test results.

[0086] Experimental results: A total of 50 bags were tested in this experiment. After sterilization at 115℃×30min, no deformation or delamination of the packaging bags and no leakage of the contents were found.

[0087] Conclusion: Through the above experiments, it is concluded that the yin-yang bag prepared by the present invention has no problems of deformation, delamination and leakage of contents after the sterilization test at 115°C×30min, and can meet the food packaging application of this sterilization condition.

Claims

1. A high-barrier yin-yang bag that can be sterilized at high temperature, characterized in that: The bag body comprises a symmetrical front structure and a back structure, wherein the front structure is sequentially compounded by a first PET film, a PET-ALOx film, and a CPP film, and the back structure is sequentially compounded by a first PET film, a second PET film, an aluminum foil, and a CPP film; The first PET film has a thickness of 12 μm and a width of 500 mm; The PET-ALOx film has a thickness of 12 μm and a width of 250 mm; The oxygen permeability of the PET-ALOx film is 1cc / m 2 *24h*0.1MPa, water vapor transmission rate 1g / m 2 *24h*0.1MPa; The aluminum foil has a thickness of 12 μm and a width of 250 mm; The second PET film has a thickness of 7 μm and a width of 250 mm; The CPP film has a thickness of 70 μm and a width of 500 mm; The CPP film is a RCPP film; The method for preparing the high-barrier yin-yang bag capable of high temperature sterilization comprises the following steps: (1) dividing the entire page of the first PET film into page A and page B in half, and printing the entire page; (2) After printing is completed, the non-printing surface of the first PET film of the A plate is dry-laminated with the PET-ALOx film to obtain a composite layer a; (3) Dry-laminating the non-printing surface of the first PET film of the B plate with the second PET film, with a glue pressing roller width of 240 mm, to obtain a composite layer b; (4) Dry-compounding the composite layer b with the aluminum foil, with a glue pressing roller width of 240 mm, to obtain a composite layer c; (5) Dry-compounding the composite layer a and the composite layer c with the CPP film at the same time, with the glue pressing roller having a width of 480 mm, to obtain a composite product; (6) placing the composite product in a constant temperature curing room at 50°C for 72 hours; (7) bagging the matured product to obtain the yin-yang bag; The adhesive used in the dry compounding includes two components A and B. In terms of weight, the component A is composed of the following: 70 parts of isocyanate, 18 parts of polyol, and 11 parts of silane coupling agent; the component B is polyester polyol; The isocyanate in the A component is isophorone diisocyanate.

Citation Information

Patent Citations

  • Anti-leaking pressure-resistant high-temperature-resistant high-barrier vertical food oil bag and preparation method thereof

    CN106042568A

  • Steam-resistant solvent-free laminating adhesive and preparation method thereof

    CN102604583A

  • Composite film of cooking-resistant packaging bag and RCPP layer preparation method

    CN107538837A

  • Steaming-resistant solvent-free polyurethane adhesive and preparation method thereof

    CN111205808A

  • Pomegranate cultivation bag capable of preventing sunburn

    CN203538002U