A low dielectric ink for 3D printing based on thiol-ene click chemistry and its preparation method and application
Through the combination of side-chain cross-linked heteronaphthalene biphenyl polyfluoroarylene ethers and thiol-ene click chemistry, the problems of oxygen sensitivity and poor thermal stability of photosensitive resins in electronic devices have been solved, and a new product with low dielectric constant and Dielectric loss 3D printing ink achieves high mechanical properties and excellent thermal stability, making it suitable for high-speed communication equipment.
Patent Information
- Application Number
- CN202211160983.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-22
AI Technical Summary
Existing photosensitive resins in electronic equipment have problems such as oxygen sensitivity, brittleness, and poor thermal stability, resulting in low surface curing, poor mechanical properties, and poor dielectric properties. It is difficult to meet the requirements of low dielectric constant and low dielectric properties of high-speed communication equipment. electrical loss requirements.
Using side-chain cross-linked heteronaphthalene biphenyl polyfluoropolyaryl ether as the prepolymer, combined with thiol-ene click chemistry, and compounded by diluting monomers and initiators, a product with high mechanical properties, low dielectric constant and Dielectric loss 3D printing ink and molded by inkjet printing to form a cured material with excellent thermal stability and mechanical properties.
It achieves high mechanical properties, low dielectric constant and dielectric loss of the cured material, and is suitable for high-tech fields such as microelectronics and communications, providing good application prospects.
Smart Images

Figure CN115536834B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer materials, and in particular relates to a low dielectric ink for 3D printing based on thiol-ene click chemistry, and a preparation method and application thereof. Background Art
[0002] With the rapid development of 5G communication networks, high-speed communication equipment has put forward higher requirements for the application of low dielectric constant and low dielectric loss materials. In view of the shortcomings of material processing methods, the rapid development of additive manufacturing has attracted people's attention. Compared with traditional subtractive manufacturing, additive manufacturing has great design freedom, saves material costs, saves processing time, and can obtain electronic equipment with complex shapes with extremely high precision. Photosensitive resins are mainly divided into unsaturated polyesters, unsaturated polyurethanes, acrylates, etc. Due to their characteristics of fast curing, low energy consumption, low viscosity and low emissions, they are particularly suitable for additive manufacturing technology. However, their sensitivity to oxygen and inherent brittleness and heat resistance make them used in communication equipment such as circuit substrates, and often have the disadvantages of low surface curing, poor mechanical properties and poor thermal stability.
[0003] The following documents and patents have improved the shortcomings of photosensitive resins, such as sensitivity to oxygen, brittleness, and poor heat resistance. By adding active amines and other additives to the photosensitive resin system to inhibit oxygen inhibition (for example: Fine Petrochemicals, 2005, (1): 23-25, Impact Science and Photochemistry, 2013, 31 (4): 276-285, Journal of Photopolymer Science and Technology, 2010, 23 (1): 109-114, Journal of Polymer Science Part A: Polymer Chemistry, 2006, 44 (6): 2007-2014); by introducing rigid groups in the prepolymer structure design (for example: CN109422881A, Materials (Basel), vol. 14, no. 7, Mar 30 2021, Acta Polymerica Sinica, vol. 52, no. 4, pp. 371-380, Apr 2021), by introducing rigid groups in the dilute monomer structure design (for example: CN111440115A, Advanced Materials Technologies, vol. 4, no. 10, 2019, Progress in Organic Coatings, vol. 126, pp. 162-167, 2019), by adding modified silica (SiO2) nanoparticles (ACS Appl.Polym.Mater.2020,2,11,5228–5237), the above-mentioned method of adding active amines and other additives to the photosensitive resin system to inhibit oxygen inhibition can inhibit oxygen inhibition, but the presence of small molecule additives will also damage the thermal stability and dielectric properties of the material; by introducing rigid groups into the prepolymer structure and the diluent monomer structure, although the heat resistance and mechanical properties of the photosensitive resin can be improved, the introduction of rigid groups will greatly increase the viscosity of the photosensitive resin system, thereby damaging its processing performance; by adding inorganic nanoparticles, the dispersion in the photosensitive resin system will be uneven, thereby making the performance of the material uneven.
[0004] Therefore, it is particularly important to provide a photosensitive resin that can overcome the negative effects of oxygen inhibition and has good thermal stability, mechanical properties, processing properties, low dielectric constant and low dielectric loss. Summary of the invention
[0005] In view of the shortcomings and defects of the prior art, the purpose of the present invention is to provide a low dielectric ink for 3D printing based on thiol-ene click chemistry and its preparation method and application. The present invention first provides a side chain cross-linked polyfluoropolyarylether of naphthalene biphenyl with good thermal stability, mechanical properties and low dielectric constant and dielectric loss as a prepolymer, and then compound it with a diluent monomer, initiator, and organic solvent that can overcome the negative effects of system oxygen inhibition and participate in the photocuring reaction to obtain a 3D printing ink, and then obtain a solidified material of the desired shape and structure by inkjet printing. The solidified material has high mechanical properties, high thermal stability, low dielectric constant and low dielectric loss, and has good application prospects in high-tech fields such as microelectronics and communications.
[0006] In order to achieve the above object, the first aspect of the present invention provides a side chain cross-linked polyfluorophenyl phthalate polyether, which adopts the following technical scheme:
[0007] A side chain cross-linked polyfluorophenylene ether having a structure shown in Formula I:
[0008]
[0009] Formula I; n=10, m=0-8 (e.g., 1, 2, 3, 4, 5, 6, 7), l=2-10 (e.g., 3, 4, 5, 6, 7, 8, 9, 10);
[0010] Ar
[0011]
[0012] One or more of .
[0013] In the present invention, a photocurable side chain cross-linked naphthalene biphenyl polyfluoro polyarylether is selected as a prepolymer because the polyarylether itself is a material with excellent thermal stability, mechanical properties and dielectric properties. The solubility, thermal stability and mechanical properties are further improved by introducing a twisted non-coplanar naphthalene biphenyl structure, and the dielectric constant and dielectric loss of the polymer are reduced by introducing a low-polarity CF bond. At the same time, the unsaturated double bonds on the side chains of the polyfluoro polyarylether can give the polymer the ability to be photocurable, so that it can be used as a prepolymer in an ink system. In addition, the present invention limits the synthesis raw materials of the prepolymer polyfluoro polyarylether to 4-(4-hydroxyphenyl)-2,3-naphthalene-1-one (DHPZ) and bisphenol monomers, diallyl bisphenol A (DABP A) is used to strictly control the molecular weight of the prepolymer polyfluoropolyarylether and the carbon-carbon double bond content in the prepolymer; if in the prepolymer structural formula I, n<10, m=0, l<2, the molecular weight of the prepolymer will be less than 10000, and too low a molecular weight will destroy the mechanical properties of the system; if n>10, m>8, l>10, the molecular weight of the prepolymer will be greater than 30000, which will lead to the carbon-carbon double bonds in the polymer molecular chain being too long, resulting in a decrease in the mobility of the molecular chain, causing a decrease in activity, and being unable to participate in the curing reaction; finally, the n in the prepolymer structure is limited to a quantitative value of 10, so that the prepolymer has excellent heat resistance. Preferably, the ratio of m and l is regulated to be 0:5-4:1, thereby further regulating the crosslinking density and dielectric properties of the system.
[0014] The second aspect of the present invention provides a method for preparing the above-mentioned side chain cross-linked naphthyridin-1-one polyfluoro polyarylether, comprising: adding 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one (DHPZ), diallyl bisphenol A (DABPA), bisphenol monomer, alkaline catalyst, and dehydrating agent to a polymerization solvent, heating to reflux the dehydrating agent under nitrogen conditions, cooling to room temperature after removing the dehydrating agent, and then adding decafluorobiphenyl and heating to react to prepare the side chain cross-linked naphthyridin-1-one polyfluoro polyarylether; preferably, heating to reflux the dehydrating agent under nitrogen conditions, and reacting for 1-4 hours (such as 1.5 hours, 2 hours, 3 hours, 3.5 hours).
[0015] In the preparation method of the side chain cross-linked phthalazin-1-one polyfluoropolyarylether, as a preferred embodiment, the bisphenol monomer is selected from one or more of biphenyl bisphenol, hydroquinone, hexafluorobisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxybenzophenone, bisphenol A, and bisphenol fluorene; preferably, the molar ratio of the bisphenol monomer to 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one (DHPZ) and diallyl bisphenol A (DABPA) is 0 to 4:5: 1 to 5 (for example, 0:5:5, 1:5:4, 2:5:3, 3:5:2, 4:5:1); preferably, based on the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazin-1-one and diallyl bisphenol A as a whole, the molar ratio of the decafluorobiphenyl to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazin-1-one and diallyl bisphenol A as a whole is 1:0.95-1.05 (for example, 1:0.96, 1:0.98, 1:1, 1:1.02).
[0016] In the above-mentioned preparation method of side chain cross-linked polyfluoropolyarylether of naphthoxydiphenyl, as a preferred embodiment, the polymerization solvent is selected from one or more of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, and cyclopentane sulfone; preferably, taking the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole, the molar ratio of the polymerization solvent to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A is 3-5:1 (for example, 3.5:1, 4:1, 4.5:1, 4.8:1).
[0017] In the above-mentioned preparation method of side chain cross-linked naphthyridin-1-one polyfluoropolyarylether, as a preferred embodiment, the alkaline catalyst is selected from one or more of K2CO3, Na2CO3, CaCO3, and KF; preferably, taking the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole, the molar ratio of the alkaline catalyst to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A is 1.05-2.5:1 (for example, 1.2:1, 1.5:1, 1.8:1, 2:1, 2.2:1).
[0018] In the above-mentioned preparation method of side-chain cross-linked polyfluoropolyphenylene ether, as a preferred embodiment, the dehydrating agent is selected from one or both of xylene and toluene; preferably, the volume ratio of the dehydrating agent to the polymerization solvent is 0.3-2:1 (such as 0.5:1, 0.8:1, 1:1, 1.5:1, 1.8:1).
[0019] In the above-mentioned preparation method of side chain cross-linked polyfluorophenyl naphthalene, as a preferred embodiment, the reaction temperature for adding decafluorobiphenyl and heating the reaction is 130-150°C (for example, 135°C, 140°C, 145°C, 148°C), and the reaction time is 5-10h (for example, 6h, 7h, 8h, 9h); preferably, the polymer obtained after the reaction is precipitated in ethanol, and then crushed, washed and dried to obtain a prepolymer side chain cross-linked polyfluorophenyl naphthalene.
[0020] The reaction endpoint in the present invention is when the viscosity of the polymer in the polymerization system does not change after three hours.
[0021] A third aspect of the present invention provides a low dielectric ink for 3D printing based on thiol-ene click chemistry, wherein the raw materials of the low dielectric ink include: 70wt%-80wt% (e.g., 70.5wt%, 72wt%, 74wt%, 75wt%, 77wt%, 79wt%, 79.5wt%) of an ink mixture, and the balance is an organic solvent; wherein, in terms of mass percentage, the ink mixture includes: 80wt%-90wt% (e.g., 80.5wt%, 82wt%, 84wt%, 85wt%, 87wt%, 89wt%, 89.5wt%) of a prepolymer, 5wt%-15wt% (e.g., 5.5wt%, 7wt%, 9wt%, 10wt%, 11wt%, 13wt%, 14.5wt%) of a diluent monomer, and 5wt%-10wt% (e.g., 5.5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 9.5wt%) of an initiator;
[0022] The prepolymer is the side chain cross-linked polyfluorophenylene phthalate having a structure shown in Formula I or the side chain cross-linked polyfluorophenylene phthalate prepared by the above preparation method;
[0023] The diluent monomer is selected from one or more of 3,6-dioxa-1,8-octanedithiol (DOT), trimethylolpropane tris(3-mercaptopropionate) (TMP), and pentaerythritol tetrakis-3-mercaptopropionate (PTP).
[0024] In the present invention, the thiol diluent monomer can reduce the viscosity of the ink mixture on the one hand, and on the other hand, the sulfur-based structure in the diluent monomer and the allyl group on the side chain of the prepolymer will undergo thiol-ene click chemistry to form a dense cross-linked network, which can further be regulated by regulating the cross-linking density of the two to achieve regulation of various ink properties; in addition, the thiol diluent monomer can also react with peroxide free radicals, perfectly overcoming the influence of oxygen on free radical curing, and this curing system does not require the additional addition of oxygen scavengers, eliminating the adverse effects of small molecules on various properties of the cured material.
[0025] The diluent monomer of the present invention is selected from one or more of 3,6-dioxa-1,8-octanedithiol (DOT), trimethylolpropane tris(3-mercaptopropionate) (TMP), and pentaerythritol tetrakis-3-mercaptopropionate (PTP). The above-mentioned diluent monomers all contain a thiol structure. Under the initiation of a photoinitiator, more active thiol free radicals are generated, which drive the relatively low-activity allyl free radicals in the side chain of the prepolymer polyfluoropolyaryl ether to gradually polymerize and form a dense cross-linked network; wherein, the DOT structure has a long fatty chain that can effectively reduce the dielectric constant, the TMP structure enables the ink to have better curing activity and lower viscosity, and PTP is a tetrafunctional thiol that enables the ink to have the highest curing activity; the present invention selects one or more of the above-mentioned diluent monomers and adds different proportions to appropriately adjust the viscosity of the ink system, the flexibility of the cured material, and the dielectric properties.
[0026] In the above-mentioned low-dielectric ink for 3D printing based on thiol-ene click chemistry, as a preferred embodiment, the low-dielectric ink is formed by inkjet printing to obtain a cured material; preferably, in the inkjet printing, the curing program is set to select 300-400nm (such as 320nm, 340nm, 350nm, 370nm, 390nm) wavelength light exposure for 5-60s (such as 10s, 20s, 30s, 40s, 50s), and then heat to 80°C and keep warm for 30-120min (such as 50min, 70min, 90min, 100min, 110min), then heat to 120°C and keep warm for 30-120min (such as 50min, 70min, 90min, 100min, 110min), and then heat to 150°C and keep warm for 30- Preferably, the cured material has a glass transition temperature Tg of 140-220°C (e.g. 150°C, 170°C, 190°C, 210°C), a tensile strength of 40-65MPa (e.g. 45MPa, 50MPa, 55MPa, 60MPa), an elongation at break of 7%-20% (e.g. 8%, 10%, 15%, 18%), a dielectric constant (@1MHz-10GHz) of 2.51-2.90 (e.g. 2.60, 2.70, 2.80, 2.85), and a dielectric loss (@1MHz-10GHz) of 0.006-0.035 (e.g. 0.010, 0.015, 0.020, 0.030).
[0027] In the above-mentioned low dielectric ink for 3D printing based on thiol-ene click chemistry, as a preferred embodiment, the initiator is selected from one or both of 1-hydroxycyclohexyl phenyl ketone and 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone.
[0028] In the above-mentioned low dielectric ink for 3D printing based on thiol-ene click chemistry, as a preferred embodiment, the organic solvent is one or more of acetone, cyclohexanone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0029] The fourth aspect of the present invention provides a method for preparing the above-mentioned low dielectric ink for 3D printing based on thiol-ene click chemistry, comprising: first preparing a prepolymer side chain cross-linked polyfluoropolyphenylene ether; then adding the prepolymer side chain cross-linked polyfluoropolyphenylene ether, a diluent monomer, and an initiator to an organic solvent, stirring them to fully mix them under light-proof conditions, and then subjecting them to a bubbling treatment to obtain the ink; preferably, the bubbling treatment is ultrasonic or vacuum.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention uses side-chain cross-linked polyfluoropolyarylether of naphthalene biphenyl with good thermal stability, mechanical properties, low dielectric constant and dielectric loss as a prepolymer, and compounding it with a diluent monomer, an initiator and an organic solvent that can overcome the negative effects of oxygen inhibition of the system and participate in a photocuring reaction to obtain a low dielectric ink for 3D printing, and then forming it by inkjet printing to obtain a solidified material with a desired shape and structure. The solidified material has a glass transition temperature Tg of 140 to 220° C., a tensile strength of 40 to 65 MPa, an elongation at break of 7% to 20%, a dielectric constant (@1 MHz to 10 GHz) of 2.51 to 2.90, and a dielectric loss (@1 MHz to 10 GHz) of 0.006 to 0.035. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The nuclear magnetic hydrogen spectrum of the side chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE) prepared in Preparation Example 1-4 of the present invention;
[0033] Figure 2 The differential scanning calorimetry analysis diagram of the side chain cross-linked naphthalene biphenyl hexafluorobisphenol A type polyfluoroarylether (DA-AF-FPPE) prepared in Preparation Example 1-4 of the present invention;
[0034] Figure 3The tensile-displacement graph of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked 3D printing bis(hexafluorobisphenol A) polyfluoropolyarylether low dielectric ink (DA / DOT) prepared in Examples 1-4 of the present invention based on thiol-ene click chemistry;
[0035] Figure 4 The graphs of tensile strength and elongation at break of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked 3D printing bis(hexafluorobisphenol A) polyfluoropolyarylether low dielectric ink (DA / DOT) prepared in Examples 1-4 of the present invention based on thiol-ene click chemistry;
[0036] Figure 5 This is a dynamic thermomechanical analysis diagram of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether low dielectric ink (DA / DOT) for 3D printing based on thiol-ene click chemistry prepared in Examples 1-4 of the present invention. DETAILED DESCRIPTION
[0037] The low dielectric ink for 3D printing based on thiol-ene click chemistry and its preparation method of the present invention are described below in conjunction with the accompanying drawings and examples. It should be understood that these embodiments are only used to explain the present invention and are not intended to limit the scope of the present invention. It should be understood that after reading the contents of the present invention, those skilled in the art make various changes and modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
[0038] The sources of raw materials used in the following examples are:
[0039] Decafluorobiphenyl (DFBP): Tianjin Chemical Reagent Plant No. 2, analytical grade;
[0040] 4-(4-Hydroxyphenyl)-2,3-naphthyridin-1-one (DHPZ): provided by Dalian Baolimo New Materials Co., Ltd., with a purity of 99wt%;
[0041] 2,2'-Diallylbisphenol A (DABPA): Sigma-Aldrich, analytical grade;
[0042] Hexafluorobisphenol A (6F-BPA): Xilong Chemical Plant, analytical grade;
[0043] Biphenyl bisphenol: Aladdin, analytical grade;
[0044] Hydroquinone: Aladdin, analytical grade;
[0045] Bisphenol A: Aladdin, analytical grade;
[0046] Bisphenol fluorene: Aladdin, analytical grade;
[0047] Anhydrous potassium carbonate: Xilong Chemical Plant, analytical grade;
[0048] N-Methylpyrrolidone: Aladdin, analytical grade;
[0049] Xylene: Aladdin, analytical grade;
[0050] 3,6-Dioxa-1,8-octanedithiol (DOT): Macklin, analytical grade;
[0051] Trimethylolpropane tris(3-mercaptopropionate) (TMP): Macklin, analytical grade;
[0052] Pentaerythritol tetrakis-3-mercaptopropionate (PTP): Macklin, analytical grade;
[0053] 1-Hydroxycyclohexylphenyl ketone: Macklin, analytical grade;
[0054] Acetone: Fuyu Fine Chemical Co., Ltd., analytical grade; other raw materials can be obtained from public commercial channels.
[0055] Preparation Example 1 A method for preparing a side chain cross-linked naphthalene biphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE532), comprising:
[0056] In a 100 ml three-necked flask equipped with a mechanical stirrer, a water separator, and a nitrogen inlet, 2.3814 g (0.01 mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.8505 g (0.006 mol) of diallyl bisphenol A (DABPA), 1.3449 g (0.004 mol) of hexafluorobisphenol A (6F-BPA), 4 g of anhydrous potassium carbonate, and 9.3 ml of N,N-dimethylacetamide (DMAc) and 15mL toluene were introduced with N2 and refluxed at 130°C for 2h. After the toluene was evaporated, the mixture was cooled to room temperature, 6.6822g (0.02mol) of decafluorobiphenyl was added, and then the temperature was raised to 130°C for reaction for 5h until the viscosity of the system no longer increased. The obtained polymer was precipitated in ethanol, crushed, washed and dried to obtain side chain cross-linked naphthylene biphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE532); the yield was 91%.
[0057] Preparation Example 2 A method for preparing a side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE541). The difference between Preparation Example 2 and Preparation Example 1 is that 2.3814g (0.01mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 2.4673g (0.008mol) of diallyl bisphenol A (DABPA), and 0.6725g (0.002mol) of hexafluorobisphenol A (6F-BPA) are added, and the rest are the same as in Preparation Example 1 to obtain side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE541); the yield is 85%.
[0058] Preparation Example 3 A method for preparing a side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE523). The difference between Preparation Example 3 and Preparation Example 1 is that 2.3814g (0.01mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.2336g (0.004mol) of diallyl bisphenol A (DABPA), and 2.0174g (0.006mol) of hexafluorobisphenol A (6F-BPA) are added, and the rest are the same as in Preparation Example 1 to obtain side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE523); the yield is 87%.
[0059] Preparation Example 4 A method for preparing a side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE514). The difference between Preparation Example 4 and Preparation Example 1 is that 2.3814g (0.01mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 0.6168g (0.002mol) of diallyl bisphenol A (DABPA), and 2.6898g (0.008mol) of hexafluorobisphenol A (6F-BPA) are added, and the rest are the same as in Preparation Example 1 to obtain side chain cross-linked naphthobiphenyl hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE514); the yield is 88%.
[0060] The H NMR spectra and DSC analysis diagrams of DA-AF-FPPE532, DA-AF-FPPE541, DA-AF-FPPE523 and DA-AF-FPPE514 are shown in Figure 1 and Figure 2 ,from Figure 1From the H-NMR spectrum, we can see that three proton peaks on the terminal allyl group on the polymer side chain appear at 6.06ppm, 5.08ppm and 3.55ppm, which proves that the photocurable group has been successfully introduced into the polymer; the proton peak of the peri-hydrogen of DHPZ appears at 8.6ppm, the proton peaks at 7.5-8.0ppm and 7.25ppm belong to DHPZ, and the proton peaks at 7.4ppm and 7.1ppm belong to 6F-BPA; this proves that the target polymer DA-AF-FPPE has been successfully prepared; Figure 2 From the differential scanning calorimetry analysis diagram, it can be seen that the glass transition temperatures are 199°C, 186°C, 211°C and 229°C respectively.
[0061] Preparation Example 5 A method for preparing a side chain cross-linked naphthalene biphenyl hydroquinone type polyfluoropolyarylether (DA-PQ-FPPE), comprising:
[0062] In a 100 ml three-necked flask equipped with a mechanical stirrer, a water separator, and a nitrogen inlet, 2.3814 g (0.01 mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.8505 g (0.006 mol) of diallyl bisphenol A (DABPA), 0.4404 g (0.004 mol) of hydroquinone (PQ), 4 g of anhydrous potassium carbonate, and 9.6 mL of N-methylpyrrolidone and 15mL of xylene were introduced with N2 and refluxed at 130°C for 2h. After the xylene was evaporated, the mixture was cooled to room temperature, 6.6822g (0.02mol) of decafluorobiphenyl was added, and then the temperature was raised to 130°C for reaction for 5h until the viscosity of the system no longer increased. The obtained polymer was precipitated in ethanol, crushed, washed and dried to obtain side-chain cross-linked poly(naphthalene biphenyl) hydroquinone type polyfluoropolyarylether (DA-PQ-FPPE) with a yield of 86%.
[0063] Preparation Example 6 A method for preparing a side chain cross-linked naphthalene biphenyl biphenol type polyfluoropolyarylether (DA-BP-FPPE), comprising:
[0064] In a 100 ml three-necked flask equipped with a mechanical stirrer, a water separator, and a nitrogen inlet, 2.3814 g (0.01 mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.8505 g (0.006 mol) of diallyl bisphenol A (DABPA), 0.7448 g (0.004 mol) of biphenyl (BP), 4 g of anhydrous potassium carbonate, and 9.6 mL of N-methylpyrrolidone and 15mL xylene were introduced with N2 and refluxed at 130°C for 2.5h. After the xylene was evaporated, the mixture was cooled to room temperature, 6.6822g (0.02mol) of decafluorobiphenyl was added, and then the temperature was raised to 130°C for reaction for 5h until the viscosity of the system no longer increased. The obtained polymer was precipitated in ethanol, crushed, washed and dried to obtain a main chain cross-linked naphthalene biphenyl diphenol type polyfluoropolyarylether (DA-BP-FPPE) with a yield of 83%.
[0065] Preparation Example 7 A method for preparing a side chain cross-linked naphthalene biphenyl bisphenol A type polyfluoropolyarylether (DA-BA-FPPE), comprising:
[0066] In a 100 ml three-necked flask equipped with a mechanical stirrer, a water separator, and a nitrogen inlet, 2.3814 g (0.01 mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.8505 g (0.006 mol) of diallyl bisphenol A (DABPA), 0.9132 g (0.004 mol) of bisphenol A (BA), 4 g of anhydrous potassium carbonate, and 9.6 mL of N-methylpyrrolidone and 15mL xylene were introduced with N2 and refluxed at 130°C for 2.5h. After the xylene was evaporated, the mixture was cooled to room temperature. 6.6822g (0.02mol) of decafluorobiphenyl was added, and then the temperature was raised to 130°C for reaction for 5h until the viscosity of the system no longer increased. The obtained polymer was precipitated in ethanol, crushed, washed and dried to obtain main chain cross-linked naphthalene biphenyl bisphenol A type polyfluoropolyarylether (DA-BA-FPPE) with a yield of 86%.
[0067] Preparation Example 8 A method for preparing a side chain cross-linked naphthalene biphenyl bisphenol fluorene type polyfluoropolyarylether (DA-BF-FPPE), comprising:
[0068] In a 100 ml three-necked flask equipped with a mechanical stirrer, a water separator, and a nitrogen inlet, 2.3814 g (0.01 mol) of 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one monomer (DHPZ), 1.8505 g (0.006 mol) of diallyl bisphenol A (DABPA), 1.4016 g (0.004 mol) of bisphenol fluorene (FBP), 4 g of anhydrous potassium carbonate, and 9.6 mL of N-methylpyrrolidone and 15mL xylene were introduced with N2 and refluxed at 130°C for 2.5h. After the xylene was evaporated, the mixture was cooled to room temperature. 6.6822g (0.02mol) of decafluorobiphenyl was added, and then the temperature was raised to 130°C for reaction for 5h until the viscosity of the system no longer increased. The obtained polymer was precipitated in ethanol, crushed, washed and dried to obtain the main chain cross-linked poly(naphthalene biphenyl) bisphenol fluorene polyfluoropolyarylether (DA-BF-FPPE) with a yield of 81%.
[0069] Example 1 A side-chain cross-linked polyfluoropolyarylether hexafluorobisphenol A-type low dielectric ink for 3D printing based on thiol-ene click chemistry, the preparation method of which is as follows:
[0070] 4 g (accounting for 80 wt % of the ink mixture) of the prepolymer side chain cross-linked hexafluorobisphenol A polyfluoropolyarylether (DA-AF-FPPE532) prepared in Preparation Example 1, 0.75 g (accounting for 15 wt % of the ink mixture) of 3,6-dioxa-1,8-octanedithiol (DOT), and 0.25 g (accounting for 5 wt % of the ink mixture) of 1-hydroxycyclohexylphenyl ketone were dissolved in 1.25 g of acetone solvent; they were fully mixed by magnetic stirring in a light-proof environment, and the system was bubbling by ultrasound and vacuum pumping, and the ink preparation was completed.
[0071] The ink was subjected to inkjet printing to obtain a cured material, wherein, in the inkjet molding, the curing program was set to cure for 40 seconds under ultraviolet light with a wavelength of 365 nm, and to cure at 80° C. for 60 minutes, 120° C. for 90 minutes, and 150° C. for 360 minutes, to obtain a cured material PPDAFE532.
[0072] Example 2
[0073] The difference between Example 2 and Example 1 is that 4 g of the prepolymer side chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE541) of Preparation Example 2 is added, and the rest is the same as Example 1 to prepare ink, and then the above ink is inkjet printed to obtain the solidified material PPDAFE541.
[0074] Example 3
[0075] The difference between Example 3 and Example 1 is that 4 g of the prepolymer side chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE523) of Preparation Example 3 is added, and the rest is the same as Example 1 to prepare ink, and then the above ink is inkjet printed to obtain the solidified material PPDAFE523.
[0076] Example 4
[0077] The difference between Example 4 and Example 1 is that 4 g of the prepolymer side chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether (DA-AF-FPPE514) of Preparation Example 4 is added, and the rest is the same as Example 1 to prepare ink, and then the ink is inkjet printed to obtain the solidified material PPDAFE514.
[0078] Example 5
[0079] The difference between Example 5 and Example 1 is that 4 g of the prepolymer side chain cross-linked poly(naphthalene biphenyl) hydroquinone type polyfluoropolyarylether (DA-PQ-FPPE) prepared in Preparation Example 5 is added, and the rest is the same as in Example 1 to prepare an ink, and then the ink is inkjet printed to obtain a cured material. In the inkjet printing, the curing program is set to cure for 20 seconds under ultraviolet light with a wavelength of 365 nm, and to cure at 80°C for 60 minutes, 120°C for 60 minutes, and 150°C for 360 minutes to obtain a cured material.
[0080] Example 6
[0081] The difference between Example 6 and Example 1 is that 4 g of the prepolymer side chain cross-linked naphthalene biphenyl biphenol type polyfluoropolyaryl ether (DA-BP-FPPE) prepared in Preparation Example 6 is added, and the rest is the same as in Example 1 to prepare ink, and then the ink is inkjet printed to obtain a cured material. In the inkjet printing, the curing program is set to cure for 30 seconds under ultraviolet light with a wavelength of 365 nm, and cure at 80°C for 60 minutes, 120°C for 60 minutes, and 150°C for 360 minutes to obtain a cured material.
[0082] Example 7
[0083] The difference between Example 7 and Example 1 is that 4 g of the prepolymer side chain cross-linked naphthalene biphenyl bisphenol A type polyfluoropolyarylether (DA-BA-FPPE) prepared in Preparation Example 7 is added, and the rest is the same as in Example 1 to prepare ink, and then the ink is inkjet printed to obtain a cured material. In the inkjet printing, the curing program is set to cure for 60 seconds under ultraviolet light with a wavelength of 365 nm, and cure at 80°C for 30 minutes, 120°C for 60 minutes, and 150°C for 420 minutes to obtain a cured material.
[0084] Example 8
[0085] The difference between Example 8 and Example 1 is that 4 g of the prepolymer side chain cross-linked naphthalene biphenyl bisphenol fluorene type polyfluoropolyaryl ether (DA-BF-FPPE) prepared in Preparation Example 8 is added, and the rest is the same as in Example 1 to prepare ink, and then the ink is inkjet printed to obtain a cured material, wherein the inkjet printing is set to cure for 15 seconds under ultraviolet light with a wavelength of 395 nm, and cure at 80°C for 60 minutes, 120°C for 60 minutes, and 150°C for 120 minutes to obtain a cured material.
[0086] Examples 9-10
[0087] The difference between Example 9-10 and Example 1 is that 3,6-dioxa-1,8-octanedithiol (DOT) in Example 1 is replaced by trimethylolpropane tris(3-mercaptopropionate) (TMP) and pentaerythritol tetrakis-3-mercaptopropionate (PTP), respectively, and the rest is the same as Example 1, and inks are prepared respectively.
[0088] The above inks were respectively subjected to inkjet printing to obtain cured materials, wherein in the inkjet printing, the curing program was set to cure for 40 seconds under ultraviolet light with a wavelength of 395 nm, and to cure at 80° C. for 30 minutes, 120° C. for 60 minutes, and 150° C. for 480 minutes, to obtain cured materials respectively.
[0089] Performance Testing
[0090] The side chain cross-linked polyfluoropolyarylether low dielectric ink for 3D printing based on thiol-ene click chemistry prepared in Examples 1-10 of the present invention was formed by inkjet printing to obtain a cured material. The cured material was a film with a length of 20 cm, a width of 15 cm and a thickness of 60 μm. The film was subjected to dynamic thermomechanical analysis test (specific test conditions: DMA test: dynamic mechanical thermal analysis (DMA) measurement was performed using a TA Q800 instrument with a frequency of 1 Hz and a heating rate of 3°C / min), tensile performance test (specific test conditions: using an AnInstron-5869 machine, a load of 500 N, a strain rate of 2 mm / min, and an effective tensile length of the sample of 20 mm and a width of 6 mm), and dielectric performance test (specific test conditions: the dielectric properties were measured using an Aglient E4980A impedance analyzer, and the dielectric constant and dielectric loss in the frequency range of 0.001-10 GHz at 30°C were recorded). The test results are shown in Table 1.
[0091] Figure 3The tensile-displacement diagram of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked 3D printing bisphenol A type polyfluoropolyarylether low dielectric ink (DA / DOT) for 3D printing based on thiol-ene click chemistry prepared in Examples 1-4 of the present invention shows that the tensile test process is good.
[0092] Figure 4 The tensile strength and elongation at break graph of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked 3D printing bisphenol A-type polyfluoropolyarylether low dielectric ink (DA / DOT) for 3D printing based on thiol-ene click chemistry prepared in Examples 1-4 of the present invention. It can be seen from the figure that when the monomers DHPZ:DABPA:6F-BPA in the prepolymer are 5:3:2, the tensile strength can reach a maximum of 59 MPa, the maximum stretching film amount can reach 1375 MPa, and the elongation at break is 9%.
[0093] Figure 5 The dynamic thermomechanical analysis diagram of the cured material PPDAFE obtained by inkjet printing of the side-chain cross-linked hexafluorobisphenol A type polyfluoropolyarylether low dielectric ink (DA / DOT) for 3D printing based on thiol-ene click chemistry prepared in Examples 1-4 of the present invention, the glass transition temperatures of the cured materials (determined by tanδ of the material) are 187°C, 184°C, 201°C, and 208°C, respectively, and increase with the increase of the hexafluorobisphenol A content in the cured material.
[0094] Table 1 shows the performance test results of the cured materials obtained by inkjet printing of the polyfluoropolyarylether low dielectric ink for 3D printing based on thiol-ene click chemistry prepared in Examples 1-10.
[0095] Table 1
[0096]
[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A low dielectric ink for 3D printing based on thiol-ene click chemistry, characterized in that: The raw materials of the low dielectric ink include: 70wt%-80wt% ink mixture, and the balance is organic solvent; wherein, by mass percentage, the ink mixture includes: 80wt%-90wt% prepolymer, 5wt%-15wt% diluent monomer, and 5wt%-10wt% initiator; The prepolymer is a side-chain cross-linked polyfluorophenylene phthalate poly(arylether) having a structure shown in Formula I: Formula I; n=10, m=0~8, I=2~10; Ar One or more of; The diluent monomer is selected from one or more of 3,6-dioxa-1,8-octanedithiol, trimethylolpropane tris(3-mercaptopropionate), and pentaerythritol tetrakis-3-mercaptopropionate; The initiator is selected from one or two of 1-hydroxycyclohexyl phenyl ketone and 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone; The organic solvent is one or more of acetone, cyclohexanone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.
2. The low dielectric ink for 3D printing based on thiol-ene click chemistry according to claim 1, characterized in that: The low dielectric ink is formed by inkjet printing to obtain a solidified material; In the inkjet printing, the curing procedure is set to select 300-400nm wavelength light exposure for 5-60s, then heat to 80°C and keep warm for 30-120min, then heat to 120°C and keep warm for 30-120min, and then heat to 150°C and keep warm for 30-480min for thermal curing treatment.
3. The low dielectric ink for 3D printing based on thiol-ene click chemistry according to claim 2, characterized in that: The curing material has a glass transition temperature Tg of 140 to 220° C., a tensile strength of 40 to 65 MPa, an elongation at break of 7% to 20%, a dielectric constant of 2.51 to 2.90, and a dielectric loss of 0.006 to 0.
035.
4. A method for preparing a low dielectric ink for 3D printing based on thiol-ene click chemistry as claimed in claim 1, characterized in that: include: First, a prepolymer side chain cross-linked polyfluorophenyl naphthalene is prepared; then the prepolymer side chain cross-linked polyfluorophenyl naphthalene, a diluent monomer, and an initiator are added into an organic solvent, stirred to fully mix under light-proof conditions, and then subjected to a bubbling treatment to obtain an ink.
5. A method for preparing a low dielectric ink for 3D printing based on thiol-ene click chemistry as claimed in claim 4, characterized in that: The preparation method of the side chain cross-linked phthalazinone polyfluoro polyarylether comprises: adding 4-(4-hydroxyphenyl)-2,3-naphthyridin-1-one, diallyl bisphenol A, bisphenol monomer, alkaline catalyst and dehydrating agent into a polymerization solvent, heating up to reflux of the dehydrating agent under nitrogen conditions, cooling to room temperature after removing the dehydrating agent, and then adding decafluorobiphenyl and heating up to react to prepare the side chain cross-linked phthalazinone polyfluoro polyarylether.
6. The preparation method according to claim 5, characterized in that: The bisphenol monomer is selected from one or more of biphenyl bisphenol, hydroquinone, hexafluorobisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxybenzophenone, bisphenol A, and bisphenol fluorene; the molar ratio of the bisphenol monomer to 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A is 0-4:5:1-5; taking the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole, the molar ratio of the decafluorobiphenyl to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole is 1:0.95-1.
05.
7. The preparation method according to claim 5, characterized in that: The polymerization solvent is selected from one or more of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, and cyclopentane; taking the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole, the molar ratio of the polymerization solvent to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A is 3-5:
1.
8. The preparation method according to claim 5, characterized in that: The alkaline catalyst is selected from one or more of K2CO3, Na2CO3, CaCO3, and KF; taking the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A as a whole, the molar ratio of the alkaline catalyst to the bisphenol monomer and 4-(4-hydroxyphenyl)-2,3-diazine-1-one and diallyl bisphenol A is 1.05-2.5:
1.
9. The preparation method according to claim 5, characterized in that: The dehydrating agent is selected from one or both of xylene and toluene; the volume ratio of the dehydrating agent to the polymerization solvent is 0.3-2:
1.
10. The preparation method according to claim 5, characterized in that: The reaction temperature of adding decafluorobiphenyl and heating the reaction is 130-150°C, and the reaction time is 5-10h; The polymer obtained after the reaction is precipitated in ethanol, and then crushed, washed and dried to obtain a prepolymer side chain cross-linked polyfluorophenylene phthalate.
Citation Information
Patent Citations
Epoxy-containing, isocyanurate-modified silicone resin, photosensitive resin composition, photosensitive dry film, laminate, and pattern forming process
CN109422881A
Preparation method of photosensitive functional biphenyl diamine
CN111440115A
Thiol-ene printable resins for inkjet 3D printing
US20200123301A1