A chemical plating activator and its preparation method and application

By using metal nanoparticles such as copper, nickel, cobalt as electroless plating activators as catalysts, the problems of poor stability and high cost of Pd/Sn colloid activators are solved, and the cost reduction and efficiency improvement of the electroless plating process are achieved, and non-conductive are given The substrate conductivity is suitable for a variety of electronic fields.

CN115537788BActive Publication Date: 2024-11-01SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211043224.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-29
Publication Date
2024-11-01
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

The existing Pd/Sn colloid activators have poor stability and high cost in long-term use, which limits the development of electroless plating processes and is difficult to achieve a future development direction of high performance and low cost.

Method used

Using metal nanoparticles such as copper, nickel, cobalt as catalysts, combined with surfactant and reducing agent, electroless plating activators are prepared by liquid phase reduction method, used for metallization treatment of insulating substrates, replacing precious metal palladium, reducing production costs and Improve stability.

Benefits of technology

The stability and catalytic performance of the electroless plating activation liquid are improved, the production cost is reduced, the process steps are simplified, the uniformity and efficiency of the plating are improved, and the conductivity of the non-conductive substrate is given. It is suitable for microelectronics, electromagnetic shielding, etc. field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115537788B_ABST
    Figure CN115537788B_ABST
Patent Text Reader

Abstract

The present invention discloses a chemical plating activator and a preparation method and application thereof, wherein the chemical plating activator comprises a water solvent, and metal nanoparticles dissolved in the water solvent, a surfactant and a reducing agent, wherein the metal nanoparticles are one or more of copper nanoparticles, nickel nanoparticles, cobalt nanoparticles, platinum nanoparticles and alloy nanoparticles composed of at least two metals of copper, nickel, cobalt and platinum. The present invention uses copper, nickel, cobalt and the like instead of precious metal palladium as a catalyst, which not only reduces the production cost, but also gives the chemical plating activator a good stability and catalytic performance. The chemical plating activator is a uniform and stable colloid, which can remain in its original state after long-term sealed storage at room temperature; the chemical plating activator can achieve the effect of bright plating in a plating solution at a certain temperature in a few minutes, which greatly improves the production efficiency; the chemical plating activator can achieve metal or alloy plating on a substrate, giving the non-conductive substrate conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of activators, and in particular to a chemical plating activator and a preparation method and application thereof. Background Art

[0002] In recent years, electronic products have been developing rapidly towards being lighter, thinner, faster and more portable. The speed requirements for integrated circuits are also getting faster and faster, and the size is getting smaller and smaller. The width of the copper wire inside the printed circuit board is getting narrower and narrower, reaching the sub-micron level. Chemical copper plating technology can achieve conductive interconnection between insulating printed circuit boards, and is an indispensable key technology in the development of integrated circuits. Moreover, energy devices such as lithium-ion batteries, such as composite current collectors that use polymers as cores and metal layers on the surface, can not only improve the specific capacity and specific energy of energy devices, but also improve their safety and reduce costs. Compared with surface metallization such as vacuum sputtering, chemical plating surface metallization has lower costs, more uniform metal layer thickness, and is easier to mass produce. In the chemical plating process, the activation step of the insulating substrate is very important in the entire chemical plating process. The performance of the activator directly affects the performance of the coating and the cost of the chemical plating metallization process. The activators currently used on the market are mainly Pd / Sn colloids. However, the Sn on the surface of the metal Pd particles is 2+ The layer is easily oxidized to Sn during long-term chemical plating. 4+ , which will greatly reduce the long-term stability and activity of the activation solution. In addition, the Pd / Sn colloidal activation solution needs to be pre-impregnated before activation and degummed after activation, which increases the complexity of the chemical plating process steps; most importantly, the precious metal Pd resources are limited and expensive, which greatly increases the production cost of the chemical plating process, restricting the further development of chemical plating in the electronics industry, and is not in line with the future development direction of chemical plating towards high performance and low cost.

[0003] Developing high-performance, low-cost chemical plating catalysts to replace the commercially expensive colloidal palladium activation solution is in line with the future development direction of electronic manufacturing, and is also conducive to improving the efficiency of chemical plating and reducing the production cost of chemical plating in actual production. Therefore, the existing technology still needs to be improved and developed. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an activator for chemical plating and a preparation method and application thereof, aiming to solve the problems of high price and poor stability of existing Pd-based catalysts.

[0005] The technical solution of the present invention is as follows:

[0006] A chemical plating activator includes a water solvent, and metal nanoparticles, a surfactant and a reducing agent dissolved in the water solvent. The metal nanoparticles are one or more of copper nanoparticles, nickel nanoparticles, cobalt nanoparticles, platinum nanoparticles and alloy nanoparticles composed of at least two metals of copper, nickel, cobalt and platinum.

[0007] The chemical plating activator comprises, by weight percentage, 5-50% of metal nanoparticles, 1-30% of surfactant, 1-30% of reducing agent, and the remainder is water.

[0008] The chemical plating activator, wherein the surfactant is one or more of Brij 35, Tween 20 and PVP.

[0009] The chemical plating activator, wherein the reducing agent is one or more of sodium hypophosphite, sodium borohydride, potassium borohydride, hydrazine hydrate, formaldehyde, and acetaldehyde.

[0010] A method for preparing a chemical plating activator, comprising the steps of:

[0011] Adding a surfactant into a water solvent to obtain a surfactant protection solution;

[0012] dispersing a metal nanoparticle precursor salt in the surfactant protection solution to obtain a mixed solution;

[0013] An aqueous solution containing a reducing agent is added dropwise to the mixed solution at room temperature, and the metal nanoparticle precursor salt is reduced to metal nanoparticles under the action of the reducing agent to obtain the chemical plating activator.

[0014] The invention discloses an application of a chemical plating activator, wherein the chemical plating activator is used for plating a metal layer on the surface of an insulating substrate.

[0015] The application of the chemical plating activator, wherein the step of using the chemical plating activator for plating a metal layer on the surface of an insulating substrate comprises:

[0016] Immersing the insulating substrate in the chemical plating activator for activation treatment to obtain an activated substrate;

[0017] The activated substrate is rinsed with deionized water and then immersed in a metal plating solution for chemical plating to complete the metal plating on the surface of the activated substrate.

[0018] The application of the chemical plating activator, wherein, before immersing the insulating substrate in the chemical plating activator for activation treatment, further comprises the steps of:

[0019] Cleaning the insulating substrate to obtain a cleaned insulating substrate;

[0020] The cleaned insulating substrate is placed in an aqueous solution containing dichromate, sodium hydroxide or potassium permanganate for roughening treatment to obtain a roughened insulating substrate.

[0021] The application of the chemical plating activator, wherein the activation treatment temperature is 20-80°C, and the time is 1-30min; the chemical plating treatment temperature is 20-80°C, and the time is 1-30min.

[0022] In the application of the chemical plating activator, the insulating substrate is one of a polymer substrate, a ceramic substrate and a silicon substrate.

[0023] Beneficial effects: The present invention provides a chemical plating activator and a preparation method and application thereof. The present invention adopts low-cost copper, nickel, cobalt, etc. instead of precious metal palladium as a catalyst, which not only reduces the production cost, but also gives the chemical plating activation solution excellent stability and catalytic performance. The chemical plating activation solution is a uniform and stable colloid, which can remain in its original state after long-term sealed storage at room temperature; the chemical plating activator can achieve the effect of bright coating in a plating solution at a certain temperature in a few minutes, greatly improving the production efficiency; the chemical plating activator can realize the plating of metal or alloy on the substrate, giving the non-conductive substrate conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Tyndall effect of the obtained colloid activation solution.

[0025] Figure 2 Pictures of ABS before (left) and after (right) copper plating.

[0026] Figure 3 Schematic diagram of the metallographic microscope of the copper layer after polymer copper plating.

[0027] Figure 4 This is the resistance test of ABS after copper plating.

[0028] Figure 5 Schematic diagram of metallographic microscope before and after the hundred-grid test of ABS after copper plating.

[0029] Figure 6 Pictures of a polymer without chemical plating (left) and a polymer after cobalt plating (right).

[0030] Figure 7 This is a metallographic microscope image of the polymer surface coating after cobalt plating.

[0031] Figure 8 Schematic diagram of metallographic microscope before and after the polymer hundred grid test before and after cobalt plating. DETAILED DESCRIPTION

[0032] The present invention provides a chemical plating activator and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] The invention provides a chemical plating activator, which comprises a water solvent, and metal nanoparticles, a surfactant and a reducing agent dissolved in the water solvent. The metal nanoparticles are one or more of copper nanoparticles, nickel nanoparticles, cobalt nanoparticles, platinum nanoparticles and alloy nanoparticles composed of at least two metals of copper, nickel, cobalt and platinum.

[0034] The present invention adopts low-cost copper, nickel, cobalt and platinum instead of precious metal palladium as catalysts, which not only reduces the production cost but also gives the chemical plating activation solution excellent stability and catalytic performance. The chemical plating activation solution is a uniform and stable colloid, which can remain in its original state after long-term sealed storage at room temperature; the chemical plating activator can achieve the effect of bright plating in a plating solution at a certain temperature for a few minutes, greatly improving the production efficiency; the chemical plating activator can realize the plating of metals or alloys on substrates such as polymers, ceramics, silicon, etc., and give conductivity to non-conductive substrates, and can be applied to the fields of microelectronic conductive interconnection, electromagnetic shielding, thermal conductivity and heat dissipation, energy device current collector, etc.

[0035] In some embodiments, the chemical plating activator includes, by weight percentage, 5-50% of metal nanoparticles, 1-30% of a surfactant, 1-30% of a reducing agent, and the remainder is water.

[0036] In some embodiments, the surfactant is one or more of Brij 35, Tween 20 and PVP, but is not limited thereto.

[0037] In some embodiments, the reducing agent is one or more of sodium hypophosphite, sodium borohydride, potassium borohydride, hydrazine hydrate, formaldehyde, and acetaldehyde, but is not limited thereto.

[0038] In some embodiments, a method for preparing an electroless plating activator is also provided, comprising the steps of:

[0039] S10, adding a surfactant into an aqueous solvent to obtain a surfactant protection solution;

[0040] S20, dispersing the metal nanoparticle precursor salt in the surfactant protection solution to obtain a mixed solution;

[0041] S30, adding an aqueous solution containing a reducing agent to the mixed solution in a dropwise manner at room temperature, wherein the metal nanoparticle precursor salt is reduced to metal nanoparticles under the action of the reducing agent, thereby obtaining the chemical plating activator.

[0042] The preparation method of the chemical plating activator provided by the present invention is simple to operate and easy to implement, and the prepared chemical plating activator has low production cost, and the chemical plating activator is endowed with excellent stability and catalytic performance. The chemical plating activator is a uniform and stable colloid, and can remain in its original state after long-term sealed storage at room temperature; the chemical plating activator can achieve the effect of bright plating in a plating solution at a certain temperature for a few minutes, greatly improving the production efficiency; the chemical plating activator can realize the plating of metal or alloy on a substrate, and endow a non-conductive substrate with conductivity.

[0043] In some embodiments, an application of a chemical plating activator is also provided, wherein the chemical plating activator is used to plate a metal layer on the surface of an insulating substrate, which specifically comprises the steps of:

[0044] Cleaning the insulating substrate to obtain a cleaned insulating substrate;

[0045] placing the cleaned insulating substrate into an aqueous solution containing dichromate, sodium hydroxide or potassium permanganate for roughening treatment to obtain a roughened insulating substrate;

[0046] The roughened insulating substrate is immersed in the chemical plating activator for activation treatment to obtain an activated substrate, wherein the activation treatment temperature is 20-80° C. and the time is 1-30 min;

[0047] The activated substrate is rinsed with deionized water and then immersed in a metal plating solution for chemical plating to complete the metal plating on the surface of the activated substrate. The temperature of the chemical plating treatment is 20-80° C. and the time is 1-30 minutes.

[0048] In this embodiment, the insulating substrate is one of a polymer substrate, a ceramic substrate and a silicon substrate, but is not limited thereto. For example, if copper is plated on the surface of the insulating substrate, the metal plating solution is a copper plating solution, and the copper plating solution includes: potassium sodium tartrate tetrahydrate, disodium ethylenediaminetetraacetic acid dihydrate, cupric sulfate pentahydrate, potassium ferrocyanide, sodium hydroxide and formaldehyde, wherein the concentration of sodium hydroxide is 0.015-0.030 g / ml, the concentration of potassium sodium tartrate tetrahydrate is 0.015-0.030 g / ml, the concentration of cupric sulfate pentahydrate is 0.015-0.030 g / ml, the concentration of disodium ethylenediaminetetraacetic acid dihydrate is 0.02-0.040 g / ml, and the concentration of potassium ferrocyanide is 0.015-0.030 g / ml. The concentration of potassium chloride is 0.001-0.002g / ml, and the concentration of formaldehyde is 0.95ml dissolved in 10ml water; if the metal cobalt is plated on the surface of the insulating substrate, the metal plating solution is a cobalt-phosphorus plating solution, which includes cobalt sulfate heptahydrate, sodium hypophosphite monohydrate, trisodium citrate, boric acid and sodium hydroxide, wherein the concentration of cobalt sulfate heptahydrate is 20-30mg / mL, the concentration of sodium hypophosphite monohydrate is 30-50mg / mL, the concentration of trisodium citrate is 15-30mg / mL, the concentration of boric acid is 20-30mg / mL, and the concentration of sodium hydroxide is 30-50mg / mL.

[0049] The chemical plating activator provided by the present invention can achieve the effect of bright plating in a plating solution at a certain temperature in a few minutes, greatly improving production efficiency; the chemical plating activator can achieve metal or alloy plating on a substrate, giving conductivity to a non-conductive substrate.

[0050] The present invention will be further explained below by means of specific embodiments:

[0051] Example 1

[0052] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 660μl of H2PtCl6·6H2O (0.1g / ml) solution and 0.037g of Cu(NO3)2·6H2O to the above mixed solution, stir magnetically for 30min, and ultrasonically for 30min; weigh 0.01g of NaBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of NaBH4 to the above mixed solution and stir for 60min to obtain a colloid activation solution.

[0053] Next, the roughened ABS substrate was immersed in a 60°C colloidal activation solution for 5 minutes, and then the activated ABS was rinsed with deionized water, and then immersed in a 60°C copper plating solution for copper plating for 5 minutes. After the copper plating was completed, it was rinsed with deionized water to obtain copper-plated ABS.

[0054] Figure 1 The Tyndall effect of the obtained colloid activated solution, from which it can be judged that the obtained is a colloid activated solution;

[0055] Figure 2 The following are pictures of ABS before (left) and after (right) copper plating. It can be seen that a bright and uniform copper layer is formed on the surface of the ABS after copper plating.

[0056] Figure 3 This is a metallographic microscope diagram of the copper layer after ABS copper plating, from which it can be seen that the copper layer is uniform and dense;

[0057] Figure 4 This is the resistance test of the copper-plated ABS. It can be seen that the resistance of the copper-plated layer on the ABS is: 0.3Ω;

[0058] Figure 5 This is a metallographic microscope diagram of ABS after copper plating before and after the hundred-grid test. It can be seen that the copper layer still exists after the hundred-grid test, indicating that the copper layer has strong adhesion.

[0059] Example 2

[0060] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 0.037g of Co(NO3)2·6H2O to the above mixed solution, stir magnetically for 30min, and ultrasonicate for 30min; weigh 0.01g of NaBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of NaBH4 to the above mixed solution and stir for 60min to obtain a cobalt colloid activation solution.

[0061] Next, the roughened ABS substrate was immersed in a 50°C cobalt colloid activation solution for 5 minutes, and then the activated ABS was rinsed with deionized water, and then immersed in a 80°C cobalt plating solution for 5 minutes. After the cobalt plating was completed, it was rinsed with deionized water to obtain the cobalt-plated ABS.

[0062] Figure 6 The following are pictures of ABS without chemical plating (left) and ABS after cobalt plating (right). It can be seen that after chemical cobalt plating, the surface of ABS is covered with a layer of gray cobalt.

[0063] Figure 7 This is a metallographic microscope image of the ABS surface coating after cobalt plating, from which we can see that the cobalt layer is uniform and dense;

[0064] Figure 8This is a schematic diagram of the metallographic microscope before and after the ABS hundred-grid test before and after cobalt plating. It can be seen that the cobalt layer still exists after the hundred-grid test, indicating that the cobalt layer has strong adhesion.

[0065] Example 3

[0066] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 1.85g of Cu(NO3)2·6H2O (molar ratio 1:50) to the above mixed solution, stir magnetically for 30min, and ultrasonicate for 30min; weigh 0.01g of NaBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of NaBH4 to the above mixed solution and stir for 60min to obtain a copper colloid activation solution.

[0067] Next, the roughened PET substrate was immersed in a 60°C colloidal activation solution for 5 minutes, and then the activated PET was rinsed with deionized water, and then immersed in a 60°C copper plating solution for copper plating for 5 minutes. After the copper plating was completed, it was rinsed with deionized water to obtain a copper-plated PET.

[0068] Example 4

[0069] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 1.85g of Ni(NO3)2·6H2O to the above mixed solution, stir magnetically for 30min, and ultrasonicate for 30min; weigh 0.01g of KBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of KBH4 to the above mixed solution and stir for 60min to obtain a colloid activation solution.

[0070] Next, the roughened PI substrate was immersed in a 30°C colloidal activation solution for 30 minutes, and then the activated PI was rinsed with deionized water, and then immersed in a 70°C nickel plating solution for nickel plating for 5 minutes. After the nickel plating was completed, it was rinsed with deionized water to obtain nickel-plated PI.

[0071] Example 5

[0072] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 521μl of H2PtCl6·6H2O (0.1g / ml) solution and 1.85g of Cu(NO3)2·6H2O (molar ratio 1:50) to the above mixed solution, stir magnetically for 30min, and ultrasonicate for 30min; weigh 0.01g of NaBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of NaBH4 to the above mixed solution and stir for 60min to obtain a colloid activation solution.

[0073] Next, the roughened PET substrate was immersed in a 25°C colloidal activation solution for 5 minutes, and then the activated PET was rinsed with deionized water, and then immersed in a 70°C nickel plating solution for copper plating for 5 minutes. After the nickel plating was completed, it was rinsed with deionized water to obtain nickel-plated PET.

[0074] Example 6

[0075] Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 260.5μl of H2PtCl6·6H2O (0.1g / ml) solution and 1.85g of Ni(NO3)2·6H2O to the above mixed solution, stir magnetically for 30min, and ultrasonically for 30min; weigh 0.01g of NaBH4 and dissolve it in 50ml of deionized water and stir evenly; under vigorous stirring, add 50ml of H2O containing 0.01g of NaBH4 to the above mixed solution and stir for 60min to obtain a colloid activation solution.

[0076] Next, the roughened ABS substrate was immersed in a colloidal activation solution at 80°C for 5 minutes, and then the activated ABS was rinsed with deionized water, and then immersed in a cobalt plating solution at 80°C for copper plating for 5 minutes. After the plating was completed, it was rinsed with deionized water to obtain cobalt-plated ABS.

[0077] In summary, the present invention uses a liquid phase reduction method to reduce the above-mentioned metal precursor into a nano-metal colloidal activator, and then applies the colloidal catalyst to a non-conductive substrate for chemical metal plating. The pre-treated substrate is immersed in a plating solution for chemical plating. Since the functional activator contains a nano-particle catalyst that catalyzes chemical plating, once chemical plating is initiated, the deposited metal layer will further self-catalyze chemical plating, and ultimately the metallization of the non-conductive substrate can be achieved.

[0078] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. Application of a chemical plating activator in plating a metal layer on the surface of an insulating substrate, It is characterized in that The insulating substrate is immersed in a chemical plating activator for activation treatment to obtain an activated substrate; The activated substrate is rinsed with deionized water and then immersed in a metal plating solution for chemical plating to complete the metal plating on the surface of the activated substrate; The chemical plating activator is prepared by the following preparation method: Weigh 0.110g of Brij 35 and add it to 100ml of deionized water, heat and stir to dissolve; add 109μl of Tween 20 to the above solution and stir evenly; add 660μl of H 2 PtCl 6 6H 2 O solution and 0.037 g Cu(NO 3 ) 2 6H 2 O, magnetic stirring for 30 min, ultrasonic for 30 min; weigh 0.01 g NaBH 4 Dissolve in 50 ml of deionized water and stir evenly; under vigorous stirring, add 0.01 g NaBH 4 50ml H 2 O is added dropwise to the mixed solution and stirred for 60 min to obtain the chemical plating activator; Among them, the H 2 PtCl 6 6H 2 The concentration of O solution is 0.1g / ml.

2. The use of the chemical plating activator according to claim 1, It is characterized in that Before the insulating substrate is immersed in a chemical plating activator for activation treatment, the method further comprises the following steps: Cleaning the insulating substrate to obtain a cleaned insulating substrate; The cleaned insulating substrate is placed in an aqueous solution containing dichromate, sodium hydroxide or potassium permanganate for roughening treatment to obtain a roughened insulating substrate.

3. The use of the chemical plating activator according to claim 1, It is characterized in that The temperature of the activation treatment is 20-80°C, and the time is 1-30 minutes; the temperature of the chemical plating treatment is 20-80°C, and the time is 1-30 minutes.

4. Use of the chemical plating activator according to any one of claims 1 to 3, It is characterized in that The insulating substrate is a polymer substrate.