A method for controlling the ring formation of rotary kiln in metallurgical zinc-containing dust
By adding an appropriate amount of magnesium-containing materials to the metallurgical zinc-containing dust sludge, the melting point of the co-melt is increased, the ring formation problem of the rotary kiln is solved, the stable operation cycle of the kiln wall is extended, the fluidity of the kiln slag is improved, and the melting point of the metallurgical dust sludge is achieved. Efficient processing.
Patent Information
- Application Number
- CN202211294285.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-21
AI Technical Summary
In the existing technology, there is a problem of controlling the ring formation in the rotary kiln of metallurgical zinc-containing dust and sludge. In particular, the large amount of gas consumption, complex operation and high energy consumption make it difficult to effectively solve the ring formation problem.
By mixing metallurgical zinc-containing dust sludge and magnesium-containing materials in a certain proportion, the amount of magnesium-containing materials does not exceed 5%, drying, preheating, heating, and calcining in a rotary kiln. After high-temperature decomposition, the MgO content is greater than 40%. Increase the melting point of the co-melt and avoid loop formation.
It effectively increases the melting point of the co-melt from 1200℃ to 1400℃, reduces the adhesion of the co-melt inside the rotary kiln, extends the stable operation cycle of the kiln wall, improves the fluidity of the kiln slag, and maximizes the refining efficiency. Iron benefits.
Smart Images

Figure CN115558783B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling zinc-containing dust, and in particular to a method for controlling ring formation in a rotary kiln of metallurgical zinc-containing dust. Background Art
[0002] Metallurgical dust ash is one of the main solid wastes in the steel industry. In addition to iron, the content of heavy metals such as lead, zinc, and cadmium is quite considerable. If it can be recycled in a comprehensive manner, it will be a valuable secondary resource; if it is not handled carefully, it will become a heavy metal pollution source that cannot be ignored.
[0003] The dust ash produced by steel mills mainly includes blast furnace dust ash, converter dust ash, and sintering machine head electrostatic dust ash. The dust ash with high lead, zinc, and alkali metal content includes blast furnace bag ash, converter secondary ash, converter electrostatic dust ash, sintering electrostatic dust ash, etc. If the dust ash such as blast furnace bag ash is directly returned to the sintering process, the harmful elements of lead, zinc, and alkali metals will be repeatedly circulated and enriched into the blast furnace, which will affect the smooth operation of the blast furnace, cause the furnace wall to thicken or nodule, and affect the life of the first generation of furnaces. Direct export will have the risk of environmental pollution. It is urgent to develop the recovery and treatment process of zinc, potassium, lead, and other metals. At present, the main processes for treating metallurgical dust ash include rotary hearth furnace, small blast furnace smelting, rotary kiln, etc.
[0004] Patent CN201110053516.9 provides a roasting method for controlling the ring formation of a rotary kiln. This method has certain limitations on the combustion mode and is only effective for rotary kilns that use coal gas or natural gas as fuel. However, it is difficult to implement in actual production due to operational problems. Patent application number CN202210068387.9 provides a method for preventing the ring formation of an iron ore reduction rotary kiln. This method is mainly used for rotary kilns for iron ore reduction. This method requires more fans, is difficult to operate, and uses a mixture of air and coal gas. There are certain risks in the actual operation process. Patent application number CN 201710089189.X discloses a process for producing nickel-iron particles by reducing and roasting laterite nickel ore in a rotary kiln in one step. The process requires that the raw material MgO / SiO2≥0.54. When it is insufficient, magnesium supplements such as dolomite or magnesia are added to increase the overall melting point of the material, but it needs to be used in conjunction with a sulfiding agent. In fact, the sulfur ions decomposed in the sulfiding agent under high temperature conditions are enriched on the surface of the metal particles, thereby reducing the melting point and surface tension of the metal particles. However, after adding a sulfiding agent, sulfur residues are easily caused, and the sulfur dioxide content in the tail gas is greatly increased, which increases the load of subsequent desulfurization equipment and facilities. In the above inventions, coal gas is used to solve the problem of rotary kiln ring formation, resulting in large coal gas consumption, serious local high temperature burning of refractory materials, a large number of fans required, and high power. The ring formation problem can be alleviated to a certain extent, but there are also problems such as high energy consumption and large influence of operation. At present, there is little research on controlling the ring formation of zinc-containing dust and mud rotary kilns.
[0005] In summary, the prior art has the following problem: how to reduce the ring formation problem of zinc-containing dust and mud rotary kiln. Summary of the invention
[0006] The technical problem to be solved by the present invention is how to control the ring formation problem of zinc-containing dust and mud rotary kiln.
[0007] To achieve the above object, the present invention provides a method for controlling the ring formation of metallurgical zinc-containing dust and sludge rotary kiln, the method comprising the following steps:
[0008] Mix metallurgical zinc-containing dust and magnesium-containing materials in a certain proportion, with the amount of magnesium-containing materials not exceeding 5%;
[0009] The mixed material is fed into the rotary kiln, where it is dried, preheated, heated, and calcined;
[0010] After the magnesium-containing material is decomposed at high temperature in the rotary kiln, the MgO content in the magnesium-containing material is greater than 40%.
[0011] Specifically, the amount of magnesium-containing material added is controlled to be 3% to 5% of the total amount of zinc-containing dust and mud.
[0012] Specifically, the magnesium-containing material includes one or more of forsterite, dolomite, serpentine, light-burned dolomite, MgO concentrate powder, and magnesite.
[0013] Specifically, the metallurgical zinc-containing dust and magnesium-containing materials are mixed in a certain proportion, including:
[0014] If the moisture content of the mixed material is between 10 and 12%, no additional water is needed;
[0015] If the moisture content of the mixed material is less than 10%, add water.
[0016] Specifically, after the magnesium-containing material is decomposed at high temperature in a rotary kiln, the generated CaO content is less than 5%, the MgO content is greater than 40%, the SiO2 content is less than 5%, the Al2O3 content is less than 4%, and the S and P content are both less than 0.01%.
[0017] Specifically, the particle sizes of dolomite, serpentine, magnesite and light-burned dolomite are all no greater than 10 mm.
[0018] Specifically, the zinc-containing dust mud contains coke powder, converter dust fine ash, ore trough dust ash, and blast furnace bag dust ash.
[0019] Specifically, the carbon content of the coke powder is greater than 80%, and the total iron content of the converter dust removal fine ash is greater than 55%.
[0020] Specifically, the amount of magnesium-containing material added is controlled to be 4% of the total amount of zinc-containing dust and mud.
[0021] The advantages of the present invention are: the present invention can effectively increase the melting point of the eutectic from the original 1200°C to 1400°C by adding magnesium-containing raw materials. The maximum operating temperature of the rotary kiln for treating metallurgical dust and sludge does not exceed 1250°C (high temperature section), so at this operating temperature, the eutectic produced inside the rotary kiln is not melted and basically does not adhere to the kiln wall of the rotary kiln, thereby effectively controlling the ringing problem and ensuring a longer stable operation period of the rotary kiln.
[0022] The present invention not only effectively increases the MgO content of the slag by adding magnesium-containing raw materials, but also the MgO content of the slag finally entering the blast furnace charge reaches a certain level during the large circulation process of the steel plant, thereby improving the fluidity of the slag and maximizing the ironmaking efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A flow chart of a method for controlling ring formation in a rotary kiln of metallurgical zinc-containing dust and sludge provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The technical solution adopted by the present invention is: in the process of reducing zinc-containing dust and sludge, by adding a certain amount of MgO-containing material and increasing the magnesium oxide content in the raw material, the melting point of the eutectic can be effectively increased, thereby achieving the control of the ring formation of the rotary kiln of metallurgical zinc-containing dust and sludge.
[0026] The present invention provides a method for controlling the ring formation of metallurgical zinc-containing dust and sludge rotary kiln, such as Figure 1 As shown, the method comprises the following steps:
[0027] The metallurgical zinc-containing dust and magnesium-containing materials are mixed in a certain proportion, and the amount of magnesium-containing materials cannot exceed 5%; the above-mentioned MgO-containing materials are: forsterite, dolomite, serpentine, light-burned dolomite, MgO concentrate powder, magnesite, etc., one or two or more of which are mixed in a proportion greater than 0% by mass.
[0028] The mixed material is sent into the rotary kiln, where it is dried, preheated, heated and calcined; the calcination temperature is controlled at 1100-1300°C. The rotary kiln has a size of Φ4.5mX64m, an annual processing capacity of 200,000 tons of dust removal ash, and adopts a dry method.
[0029] After the magnesium-containing material is decomposed at high temperature in the rotary kiln, the MgO content in the magnesium-containing material is greater than 40%.
[0030] The amount of magnesium-containing material added is controlled to be 3% to 5% of the total amount of zinc-containing dust. Preferably, the amount of magnesium-containing material added is 5% of the total amount of zinc-containing dust. The best effect is achieved when the amount of magnesite powder added is 5%. At this time, the melting point of the eutectic can be increased from the original 1250°C to about 1400°C to 1450°C, effectively avoiding the formation of low-melting-point eutectic by zinc-containing dust during calcination.
[0031] The magnesium-containing material includes one or more of forsterite, dolomite, serpentine, light-burned dolomite, MgO concentrate powder, and magnesite.
[0032] Mix metallurgical zinc-containing dust and magnesium-containing materials in a certain proportion, including:
[0033] If the moisture content of the mixed material is between 10 and 12%, no additional water is needed;
[0034] If the water content of the mixed material is less than 10%, water is added. The above-mentioned magnesium-rich raw materials are mixed evenly with the zinc-containing dust mud. During mixing, whether water needs to be added is determined according to the water content of the zinc-containing dust mud. If the water content is between 10% and 12%, no additional water is required. If the water content is lower, water needs to be added. After mixing evenly, there is no need to make balls (granules), and the powder is directly fed into the rotary kiln for calcination.
[0035] After the magnesium-containing material is decomposed at high temperature in a rotary kiln, the generated CaO content is less than 5%, the MgO content is greater than 40%, the SiO2 content is less than 5%, the Al2O3 content is less than 4%, and the S and P content are both less than 0.01%.
[0036] The particle size of dolomite, serpentine, magnesite and light-burned dolomite is not greater than 10mm.
[0037] Zinc-containing dust mud contains coke powder, converter dust fine ash, ore trough dust ash, and blast furnace bag dust ash.
[0038] The carbon content of coke powder is greater than 80%, and the total iron content of converter dust removal fine ash is greater than 55%.
[0039] The amount of magnesium-containing material added is controlled to be 4% of the total amount of zinc-containing dust and mud.
[0040] The present invention can effectively increase the melting point of the eutectic from the original 1200°C to 1400°C by adding magnesium-containing raw materials. The maximum operating temperature of the rotary kiln for treating metallurgical dust and sludge does not exceed 1250°C (high temperature section). Therefore, at this operating temperature, the eutectic produced inside the rotary kiln is not melted and basically does not adhere to the wall of the rotary kiln, thereby effectively controlling the ringing problem and ensuring a longer stable operation period of the rotary kiln.
[0041] The present invention not only effectively increases the MgO content of the slag by adding magnesium-containing raw materials, but also the MgO content of the slag finally entering the blast furnace charge reaches a certain level during the large circulation process of the steel plant, thereby improving the fluidity of the slag and maximizing the ironmaking efficiency.
[0042] The following examples are only for further illustrating the present invention and are not intended to limit the present invention. Example 1
[0043] This embodiment provides a method for controlling the ring formation of metallurgical zinc-containing dust and sludge rotary kiln. Figure 1 As shown, the specific method is:
[0044] Batching and mixing: coke powder, converter dust fine ash, ore trough dust ash, blast furnace bag dust ash, magnesium-containing materials, and return materials from the settling chamber are mixed in a certain proportion into a drum mixer, and a certain amount of water is added for mixing to prevent dust; wherein, the magnesium-containing material is magnesite powder, and the MgO content is greater than 40%, and the particle size of the magnesium-containing material is less than 10% on an 8mm square hole sieve, and 0 on a 10mm square hole sieve; the fixed carbon content of the coke powder is greater than 80%; the total iron grade of the converter dust fine ash is greater than 55%, and the specific composition and proportion are shown in Table 1.
[0045] Table 1
[0046]
[0047] Reduction roasting: The mixed material is sent into the rotary kiln from the kiln tail. In the process of forward flow, the material in the rotary kiln undergoes several processes such as drying, preheating, heating, calcination (1100-1300℃), etc. The rotary kiln has a specification of Φ4.5mX64m and an annual processing capacity of 200,000 tons of dust ash (dry method).
[0048] Embodiment 2~7:
[0049] This embodiment provides a method for controlling the ringing of metallurgical zinc-containing dust and sludge rotary kiln, taking the same steps as in Example 1, except that the proportion of magnesium-containing materials used is different, that is, the addition amount is changed from 1% to 0%, 2%, 3%, 4%, 5%, and 6%, and the other conditions are the same. When the magnesium-containing material increases from 1% to 6%, the processing capacity of coke powder and converter dust removal fine ash increases, while the processing capacity of ore trough dust removal ash, blast furnace bag dust removal ash, and sedimentation chamber return material decreases. Table 2 shows the ingredients when the addition amount of magnesium-containing material is 5%.
[0050] Table 2
[0051]
[0052] When magnesite powder was not added to the initial batching, the rotary kiln for processing metallurgical zinc dust began to form serious rings after about 7 days of operation, and the kiln had to be stopped to treat the rings. When magnesite powder was added to the raw materials entering the kiln, the ring formation period of the rotary kiln was shown in Table 3, and when the amount of magnesite powder added was further increased (>5%), the ring formation time was no longer extended.
[0053] Table 3
[0054]
[0055] When the amount of magnesite powder is reduced (<5%), the ring formation problem of the rotary kiln cannot be significantly improved due to the reduction of the amount of magnesite powder, and the ring formation frequency is high; when the amount of dolomite is increased (>5%), the effect is almost the same as when the amount is 5%, and the ring formation cycle is basically about 30 days. Comprehensively considered, the increase in the amount of magnesite powder causes a decrease in the dust removal ash processing volume and increases the cost of purchasing magnesite powder. At the same time, it causes the grade of kiln slag to decrease, and the subsequent kiln slag enters the sintering, which brings different degrees of negative impact on the sintering, reduces the utilization coefficient and drum index of the sintering machine, increases the energy consumption of the sintering process, and the grade of the sintered ore is also affected to varying degrees. Therefore, the effect of magnesite powder is best when the amount is 5%. At this time, the melting point of the eutectic can be increased from the original 1250℃ to about 1400℃~1450℃, effectively avoiding the formation of low-melting-point eutectic by zinc-containing dust mud during the calcination process. It is beneficial to steelmaking and sintering. The magnesium oxide formed after the decomposition of magnesite powder is used as a slag-forming agent in steelmaking, enters the sintering ore and finally enters the blast furnace for ironmaking, which is beneficial to improving the fluidity of the slag. However, the amount of magnesium-containing raw materials cannot exceed 5%. A high magnesium oxide content will have different degrees of negative effects on subsequent sintering, reduce the utilization coefficient and drum index of the sintering machine, and increase energy consumption.
[0056] The present invention can effectively increase the melting point of the eutectic from the original 1200°C to 1400°C by adding magnesium-containing raw materials. The maximum operating temperature of the rotary kiln for treating metallurgical dust and sludge does not exceed 1250°C (high temperature section). Therefore, at this operating temperature, the eutectic produced inside the rotary kiln is not melted and basically does not adhere to the wall of the rotary kiln, thereby effectively controlling the ringing problem and ensuring a longer stable operation period of the rotary kiln.
[0057] The present invention not only effectively increases the MgO content of the slag by adding magnesium-containing raw materials, but also the MgO content of the slag finally entering the blast furnace charge reaches a certain level during the large circulation process of the steel plant, thereby improving the fluidity of the slag and maximizing the ironmaking efficiency.
[0058] The above description is only an illustrative embodiment of the present invention and is not intended to limit the scope of the present invention. The components of the present invention can be combined with each other without conflict, and any equivalent changes and modifications made by any technician in the field without departing from the concept and principle of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for controlling the ring formation of metallurgical zinc-containing dust and sludge rotary kiln, It is characterized in that The method comprises the following steps: The metallurgical zinc-containing dust and the magnesium-containing material are mixed in a certain proportion, and the amount of the magnesium-containing material added is controlled to be 3% to 5% of the total amount of the zinc-containing dust; the metallurgical zinc-containing dust and the magnesium-containing material are mixed in a certain proportion, including: If the moisture content of the mixed material is between 10 and 12%, no additional water is needed; If the water content of the mixed material is less than 10%, water is added; the zinc-containing dust mud contains coke powder, converter dust fine ash, ore trough dust removal ash and blast furnace bag dust removal ash, the carbon content of coke powder is greater than 80%, and the total iron grade of converter dust removal fine ash is greater than 55%; The magnesium-containing material includes one or more of dolomite, serpentine, light-burned dolomite and magnesite; The particle size of dolomite, serpentine, magnesite and light-burned dolomite shall not exceed 10 mm; The mixed material is fed into the rotary kiln, where it is dried, preheated, heated, and calcined; After the magnesium-containing material is decomposed at high temperature in the rotary kiln, the MgO content in the magnesium-containing material is greater than 40%; after the magnesium-containing material is decomposed at high temperature in the rotary kiln, the CaO content is less than 5%, the MgO content is greater than 40%, and the SiO 2 Content is less than 5%, Al 2 O 3 The content is less than 4%, and both S and P are less than 0.01%.
2. A method for controlling ring formation in a rotary kiln of metallurgical zinc-containing dust and sludge according to claim 1, It is characterized in that The amount of magnesium-containing material added is controlled to be 4%-5% of the total amount of zinc-containing dust and mud.
3. A method for controlling ring formation in a rotary kiln of metallurgical zinc-containing dust and sludge according to claim 1, It is characterized in that The magnesium-containing material is magnesite powder, the dosage of magnesite powder is 5%, the fixed carbon content of the coke powder is greater than 80%, and the total iron grade of the converter dust removal fine ash is greater than 55%.