A flexible piezoresistive sensor based on TPU / PAN blended conductive composite fiber film and its preparation method

Preparation of TPU/PAN blended conductive composite fiber membranes by electrospinning solves the problem of signal drift and hysteresis of flexible piezoresistive sensors at high temperatures, and realizes piezoresistive sensors with high sensitivity and thermal stability, improving the biocompatibility of the device and piezoresistive properties.

CN115560887BActive Publication Date: 2024-12-03ZHEJIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211139829.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-19
Publication Date
2024-12-03
Estimated Expiration
2042-09-19

AI Technical Summary

Technical Problem

Existing flexible piezoresistive sensors are prone to signal drift and hysteresis at high temperatures, and the mechanical properties of traditional bilayer materials lead to poor device stability, making it difficult to achieve high sensitivity and thermal stability.

Method used

The TPU/PAN blended conductive composite fiber membrane was prepared as a pressure-sensitive material by electrospinning. By forming a uniform conductive layer on the surface of the TPU/PAN blended fiber membrane, the thermal stability and piezoresistive properties of the composite material were improved.

Benefits of technology

A flexible piezoresistive sensor with signal stability and high sensitivity at high temperatures is realized, avoiding signal drift and hysteresis, and improving the biocompatibility and piezoresistive sensitivity of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115560887B_ABST
    Figure CN115560887B_ABST
Patent Text Reader

Abstract

The present invention discloses a flexible piezoresistive sensor based on a TPU / PAN blended conductive composite fiber membrane and a preparation method thereof. The sensor is made of a TPU / PAN blended conductive composite fiber membrane as a pressure-sensitive material. The TPU / PAN blended conductive composite fiber membrane is composed of a matrix material and a conductive phase, wherein the matrix material is a TPU / PAN blended fiber membrane, and the conductive phase is uniformly formed on the surface of the TPU / PAN blended fiber membrane. The present invention obtains a fiber membrane by blending TPU and PAN, and uses the blended fiber membrane as a matrix material and composites it with a conductive phase to obtain a conductive composite fiber membrane. The addition of PAN can greatly improve the thermal stability and piezoresistive performance of the conductive composite fiber membrane. The obtained fiber membrane has good biocompatibility, thermal stability, piezoresistive sensitivity, and resilience, and can avoid device signal drift or hysteresis due to excessively high temperature at working temperature, and is expected to obtain a flexible pressure sensor that can be used to measure pressure at higher temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of piezoresistive sensing and relates to a flexible piezoresistive sensor based on a TPU / PAN blended conductive composite fiber film and a preparation method thereof. Background Art

[0002] Flexible piezoresistive sensors are an important branch of flexible pressure sensors. Their sensing mechanism is that the resistance of the pressure-sensitive material inside the sensor changes with the external pressure, thereby converting the change of the external pressure signal into the change of the electrical signal. Therefore, the type and performance of the pressure-sensitive material are the top priorities in the design of flexible pressure sensors.

[0003] There are two main categories of piezoresistive materials that are currently being studied: semiconductor single-phase materials with different microstructures and conductive composite materials. Of the two, the latter generally has a wider sensitivity range and has received more attention. In the early days of piezoresistive material research, researchers dispersed conductive fillers in a polymer matrix, or mixed two or more conductive phases to form a percolation-type composite material. This type of piezoresistive material utilizes the difference in Young's modulus between the matrix and the conductive phase. Under load, the tunneling current changes to achieve a response to the pressure signal. Piezoresistive sensors based on this composite material often require large loads and deformations while enhancing the signal, making it difficult to obtain high sensitivity. At the same time, creep and plastic deformation are prone to occur, resulting in electrical signal drift and hysteresis.

[0004] In order to improve the sensitivity of piezoresistive sensors, researchers subsequently turned their attention to surface-coated piezoresistive materials. This material is made by coating the conductive phase on the surface of an elastomer with a microstructure. The surface microstructure will be compressed and deformed under external loads, which will change the contact resistance of the material surface in direct contact with the electrode, thereby achieving a response to the pressure signal. However, there are two problems with piezoresistive sensors using traditional double-layer materials: first, the Young's modulus of the surface conductive material shell is too high to deform, which limits the sensitivity; second, the mechanical properties of the two layers of material are mismatched, the surface layer is prone to cracking, and the interface shear stress is prone to yielding or interface debonding, which seriously affects the stability of the device and even causes failure. Conductive polymer composite materials can better solve this problem.

[0005] Conductive polymer composites (CPCs) refer to composite materials with certain electrical conductivity, which are made of surface insulating organic polymer materials as the matrix and other conductive materials by uniform diffusion composite, stacking composite and surface conductive film formation. CPCs materials not only have the characteristics of the polymer matrix itself, but also have the characteristics of conductive fillers. In addition, by improving its composite ratio and design method, the electrical and mechanical properties of the material can be adjusted to meet the use requirements.

[0006] The present invention proposes to use electrospinning to design the conductive polymer composite material into a fibrous geometric structure to prepare a nanofiber membrane, which has the characteristics of high porosity and high specific surface area, and is more conducive to loading more conductive fillers; its mesh structure is conducive to improving its piezoresistive performance. However, the current flexible piezoresistive sensors based on traditional elastomers such as PDMS relax significantly at the operating temperature, are prone to creep, and cause significant signal drift, affecting the stability of the device. Therefore, it is necessary to design a high Tg pressure-sensitive composite material, so that a material system with good thermal stability, high sensitivity and high compression resilience can be obtained. Summary of the invention

[0007] The purpose of the present invention is to address the deficiencies in the prior art and provide a flexible piezoresistive sensor based on a TPU / PAN blended conductive composite fiber membrane and a preparation method thereof. The composite fiber membrane has good biocompatibility, strain sensitivity, and resilience. The corresponding piezoresistive sensor has no signal drift or hysteresis, and a flexible piezoresistive sensor with high stability and low hysteresis can be obtained.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A flexible piezoresistive sensor based on TPU / PAN blended conductive composite fiber membrane is made of TPU / PAN blended conductive composite fiber membrane as pressure-sensitive material. The TPU / PAN blended conductive composite fiber membrane is composed of a matrix material and a conductive phase, wherein the matrix material is a TPU / PAN blended fiber membrane, and the conductive phase is uniformly formed on the surface of the TPU / PAN blended fiber membrane.

[0010] The preparation method of the TPU / PAN blended conductive composite fiber membrane comprises the following steps:

[0011] Using N,N-dimethylformamide (DMF) as solvent, weigh TPU raw material and dissolve it in DMF solution, stir and mix evenly, add PAN powder, heat and stir in a water bath to obtain a uniform and stable TPU / PAN spinning solution, and use electrospinning method to prepare TPU / PAN blended fiber membrane;

[0012] The TPU / PAN blended fiber membrane is completely immersed in a conductive phase (such as MXene) solution, ultrasonically treated at room temperature, taken out, washed with deionized water, and dried to form a uniform conductive layer on the TPU / PAN blended fiber membrane to obtain a TPU / PAN blended conductive composite fiber membrane.

[0013] In the above technical solution, further, the total mass concentration of the TPU / PAN spinning solution is 10wt%-20wt%, wherein the mass ratio of TPU to PAN is 1:9-1:1.

[0014] Furthermore, the electrospinning parameters are as follows: spinning voltage is 10KV-30KV, receiving drum speed is 400-600r / min, propulsion speed is 0.002mm / s, spinning distance is 6.5cm, and spinning time is 8h.

[0015] Furthermore, the conductive phase is MXene, and the conductive phase solution is prepared by dispersing MXene nanosheet powder in deionized water and adding sodium polyphosphate to mix.

[0016] Furthermore, the mass concentration of MXene in the MXene solution is 1-10 mg / ml, and the mass concentration of sodium polyphosphate is 1wt%-10wt%.

[0017] The beneficial effects of the present invention are:

[0018] The present invention obtains a fiber membrane by blending TPU and PAN, and uses the blended TPU and PAN as a matrix material to compound the blended fiber membrane with a conductive phase to obtain a conductive composite fiber membrane. The addition of PAN can greatly improve the thermal stability and piezoresistive properties of the conductive composite fiber membrane. The obtained fiber membrane has good biocompatibility, thermal stability, piezoresistive sensitivity, and resilience, and can avoid device signal drift or hysteresis due to excessively high temperature at working temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The SEM images of the conductive composite fiber membranes prepared by adding PAN in different proportions; a, pure PAN, b, TPU:PAN=1:9, c, TPU:PAN=3:7, d, TPU:PAN=1:1, e, TPU:PAN=7:3; f, TPU:PAN=9:1;

[0020] Figure 2 is the piezoresistive sensitivity curve of different conductive composite fiber membrane samples;

[0021] Figure 3 It is a schematic diagram of the piezoresistive rebound performance test;

[0022] Figure 4 It is the compression-rebound curve of the sample obtained in Example 1. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0024] The flexible piezoresistive sensor based on TPU / PAN blended conductive composite fiber membrane of the present invention is made of TPU / PAN blended conductive composite fiber membrane as a pressure-sensitive material. The fiber membrane obtained by blending TPU and PAN is used as a matrix material, and a composite conductive phase is formed on its surface. By introducing highly polar polyacrylonitrile (PAN) into the TPU flexible substrate system, because the glass transition temperature of PAN is much higher than that of TPU, it can not only fully activate the active sites on the surface of TPU, but also greatly prolong the relaxation time, optimize the stability of TPU in a high-temperature working environment, thereby effectively improving the piezoresistive performance of the obtained composite fiber membrane.

[0025] In the scheme of the present invention, the TPU / PAN blended fiber membrane is prepared by an electrostatic spinning method, wherein the spinning solution is N,N dimethylformamide (DMF) as a solvent, TPU is added and stirred and evenly mixed, and PAN powder is added, and the mixture is heated and stirred in a water bath at a constant temperature. The total mass concentration in the spinning solution is 10wt%-20wt%, wherein the mass ratio of TPU to PAN is 1:9-9:1, preferably not exceeding 1:1, and if it exceeds this range, the piezoresistive sensitivity of the obtained composite conductive fiber membrane will be greatly affected.

[0026] According to a specific example of the present invention, the conductive phase can be MXene or graphene, and the prepared TPU / PAN blended fiber membrane is completely immersed in the conductive phase solution, ultrasonically treated at room temperature, taken out and washed with deionized water, and dried to form a uniform conductive layer on the TPU / PAN blended fiber membrane to obtain a TPU / PAN blended conductive composite fiber membrane. When the conductive phase is MXene, the oxidation of MXene can be effectively prevented by adding sodium polyphosphate to the conductive phase solution.

[0027] Example 1

[0028] Using N,N-dimethylformamide (DMF) as solvent, a certain amount of TPU raw material particles were weighed at room temperature (20°C), dissolved in DMF solution, and mixed evenly using a high-speed mixer. A certain amount of PAN powder was added thereto, and the mixture was heated and stirred at a constant temperature in a water bath at 50°C to obtain a uniform and stable spinning solution with a concentration of 15wt%, wherein the mass ratio of TPU / PAN was 1:9.

[0029] TPU / PAN nanofiber membrane was prepared by electrospinning: 18KV high voltage positive electricity was connected to the needle (the voltage was adjusted according to the state during spinning to make the spindle line stable during spinning), and aluminum foil was attached to a roller with a rotation speed of 500r / min to ground the receiving device. During the spinning process, the solution in the syringe was pushed at a speed of 0.002mm / s, the spinning distance was 6.5cm, and the spinning time was 8h. The fiber membrane obtained by electrospinning was dried in an electric hot air drying oven at 60℃ for 24h to remove the solvent that was not completely volatilized.

[0030] Cut a 2cm×3.5cm fiber membrane from the obtained TPU / PAN nanofiber membrane, put it into a centrifuge tube, add MXene solution (MXene mass concentration is 4mg / ml, and contains sodium polyphosphate) to the centrifuge tube until the solution submerges the fiber membrane in the centrifuge tube, cover it and put it in a test tube rack, put it in an ultrasonic machine, add water to the ultrasonic machine until it submerges the liquid surface in the centrifuge tube, and ultrasonicate it at room temperature for 30 minutes. Take it out after half an hour, wash it in deionized water, and then use non-woven fabric to absorb the water on the surface of the fiber membrane, and then put the fiber membrane into a vacuum drying oven at 30°C and vacuum dry it for 12 hours. During the vacuum drying process, the MXene nanosheet layer forms a uniform conductive layer on the TPU / PAN fiber membrane. The MXene@TPU / PAN composite conductive fiber membrane is obtained, and the conductivity is measured to be 0.00794S / m.

[0031] Example 2

[0032] The same as Example 1, except that the mass ratio of TPU / PAN in the spinning solution is 3:7, and the measured conductivity is 0.0476 S / m.

[0033] Example 3

[0034] The same as Example 1, except that the mass ratio of TPU / PAN in the spinning solution is 1:1, and the measured conductivity is 0.0714 S / m.

[0035] Example 4

[0036] The same as Example 1, except that the mass ratio of TPU / PAN in the spinning solution is 7:3, and the measured conductivity is 0.00529 S / m.

[0037] Example 5

[0038] The same as Example 1, the only difference is that the mass ratio of TPU / PAN in the spinning solution is 9:1, and the measured conductivity is 0.00009 S / m.

[0039] Example 6

[0040] The same as Example 1, the only difference is that no PAN powder is added to the spinning solution, only TPU is added, and a MXene@TPU composite conductive fiber membrane is obtained, and the measured conductivity is 0.00537 S / m.

[0041] Example 7

[0042] The same as Example 1, except that the mass concentration of MXene in the MXene solution is 5 mg / ml.

[0043] Example 8

[0044] The same as Example 1, the only difference is that the MXene solution does not contain sodium polyphosphate.

[0045] Figure 1 is the SEM image of the composite conductive fiber membrane prepared in Examples 1-6, Figure 2 As for its corresponding piezoresistive sensitivity performance, it can be seen that with the increase of PAN ratio, the growth of MXene on TPU / PAN nanofiber membrane is more uniform. When the mass ratio of TPU to PAN does not exceed 1:1, it has excellent piezoresistive sensitivity and good electrical conductivity. Especially when the mass ratio of the two is 1:9, the MXene@TPU / PAN composite conductive fiber membrane has excellent piezoresistive sensitivity, which is more sensitive at 0-10kPa and can reach a sensitivity of 627.52kPa at 10kPa. -1 .

[0046] When the composite conductive fiber membrane prepared in Example 8 is exposed to the air, MXene is easily oxidized, thereby affecting the membrane stability and device performance. Because the surface of the MXene sheet is negatively charged and the edge is positively charged, oxidation occurs from the edge to the middle. By adding polyanion salt sodium polyphosphate (H2Na2O7P2), it can be adsorbed on the edge of MXene, thereby effectively preventing its oxidation. In addition, MXene@TPU nanofiber membranes were prepared by adding MXene solutions with different sodium polyphosphate concentrations. It was observed in SEM that as the concentration of the sodium polyphosphate solution increased, granular oxide TiO2 no longer appeared on the nanofibers, indicating that adding sodium polyphosphate to the MXene nanosheet solution can achieve the purpose of anti-oxidation treatment, which is beneficial to device stability.

[0047] The composite conductive fiber membrane prepared in the above example was subjected to a compression rebound test, specifically using the following method: Figure 3 The device shown is used to cut small discs with a diameter of 10 mm from the prepared composite conductive fiber membrane using a tablet press as a homemade electrode. A computer, a digital source meter, a homemade electrode, a carbon fiber plate, and a customized small iron block of equal height are used to perform compression rebound tests to obtain compression rebound curves of different samples. The digital source meter will collect the changes in system current over time. By loading and releasing the customized small iron block, the resistance of the small disc of the conductive fiber membrane changes, thereby changing the current collected by the digital source meter. After exporting the data through the computer, the compression rebound test curve can be obtained. By comparing the data, it was found that the sample without PAN (i.e., the MXene@TPU composite conductive fiber membrane obtained in Example 6) would experience severe signal drift and hysteresis, and could not achieve stable measurement of pressure;

[0048] The composite conductive fiber membrane prepared by the present invention has excellent piezoresistive sensitivity and compression resilience performance. Figure 4As shown in the figure, the compression rebound performance of the MXene@TPU / PAN composite conductive fiber membrane when the mass ratio of TPU:PAN is 1:9 is measured. It can be seen that the steps during loading and unloading tend to be horizontal, and the steps corresponding to each loading and unloading are almost flat. Whether it is the sensitivity or the accuracy of the composite fiber membrane's response to pressure after loading and unloading, it can be seen that the prepared MXene@TPU / PAN composite conductive fiber membrane has extremely excellent piezoresistive properties. In addition, the prepared TPU / PAN-based flexible piezoresistive sensor has good thermal stability, which can avoid the device signal from drifting seriously due to excessively high temperature at the working temperature.

Claims

1. A flexible piezoresistive sensor based on TPU / PAN blended conductive composite fiber film, characterized in that: The TPU / PAN blended conductive composite fiber membrane is used as a pressure-sensitive material. The TPU / PAN blended conductive composite fiber membrane is composed of a base material and a conductive phase, wherein the base material is a TPU / PAN blended fiber membrane, and the conductive phase is uniformly formed on the surface of the TPU / PAN blended fiber membrane. The preparation method of the TPU / PAN blended conductive composite fiber membrane comprises the following steps: Using N,N-dimethylformamide (DMF) as solvent, weighing TPU raw material and dissolving it in DMF solution, stirring and mixing evenly, adding PAN powder, heating and stirring in a water bath at a constant temperature, obtaining a uniform and stable TPU / PAN spinning solution, wherein the mass ratio of TPU to PAN is 1:9-1:1, and using an electrospinning method to prepare a TPU / PAN blended fiber membrane; The TPU / PAN blended fiber membrane is completely immersed in a conductive phase solution, ultrasonically treated at room temperature, taken out, washed with deionized water, and dried to form a uniform conductive layer on the TPU / PAN blended fiber membrane to obtain a TPU / PAN blended conductive composite fiber membrane, wherein the conductive phase is MXene, and the conductive phase solution is MXene nanosheet powder dispersed in deionized water, and sodium polyphosphate is added to mix.

2. The flexible piezoresistive sensor according to claim 1, characterized in that: The total mass concentration of the TPU / PAN spinning solution is 10 wt%-20 wt%.

3. The flexible piezoresistive sensor according to claim 1, characterized in that: The electrospinning parameters are as follows: spinning voltage is 10 kV-30 kV, receiving drum speed is 400-600 r / min, propulsion speed is 0.002 mm / s, spinning distance is 6.5 cm, and spinning time is 8 h.

4. The flexible piezoresistive sensor according to claim 1, characterized in that: The mass concentration of MXene in the conductive phase solution is 1-10 mg / ml, and the mass concentration of sodium polyphosphate is 1wt%-10 wt%.

Citation Information

Patent Citations

  • Flexible strain sensor based on MXenes / polymer conductive fiber composite membrane and preparation method of flexible strain sensor

    CN111043950A

  • Preparation method and application of novel rubber seed shell-based composite material

    CN113769716A