A recyclable high-strength and tough composite hydrogel and its preparation method and application

By using the composite technology of calcium phosphate oligomers, aramid nanofibers and polyvinyl alcohol in high-strength composite hydrogel, combined with layer-by-layer stacking and acid demineralization treatment, the balance problem of high strength and high toughness is solved and achieved It has achieved reversible cyclic regeneration of hydrogel and is suitable for the fields of soft robotics and biological tissue engineering.

CN115570859BInactive Publication Date: 2024-10-11ZHEJIANG UNIV
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202211115393.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-14
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN115570859B_ABST
    Figure CN115570859B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a recyclable high-strength and tough composite hydrogel: a water dispersion of CPO and ANF and a PVA aqueous solution are compounded to form a uniform slurry, an isotropic composite film is prepared by inorganic ion polymerization and self-assembly; the composite film is immersed in water to reach swelling equilibrium, directional stretching is performed until the internal structure of the film is reorganized, and the film is immersed in water again to reach swelling equilibrium, so as to obtain a hydrogel film with a hierarchical and orderly structure; the obtained hydrogel film is stacked layer by layer, and glue is used for interlayer bonding, and dried after applying instantaneous compressive stress, and immersed in water again to reach swelling equilibrium, so as to obtain a high-strength and tough bulk phase hydrogel as a recyclable high-strength and tough composite hydrogel. The hydrogel can achieve a balance between high strength and high toughness, has the characteristics of being recyclable, and can be applied to the preparation of non-disease diagnosis and treatment in the field of soft robot materials or biological tissue engineering materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-strength and tough soft materials, and particularly relates to a recyclable high-strength and tough composite hydrogel and a preparation method and application thereof. Background Art

[0002] Hydrogels are a class of soft materials composed of three-dimensional cross-linked polymer networks in an aqueous environment. They have been widely studied in the fields of energy (hydrogel electrolytes / electrodes), environment (water purification / collection), biomedicine (soft tissue repair / replacement, drug loading / release), and structural engineering materials (intelligent wearable electronics, soft robots). The nanostructure and mechanical properties of hydrogels are crucial to their applications. For example, natural muscle tissue (a biological hydrogel) is composed of abundant water (70-80wt%) and collagen fibers, etc. It has excellent tensile strength and high load-bearing capacity and can provide structural support for organisms. Its excellent mechanical properties are derived from its highly integrated and anisotropic hierarchical ordered structure. In contrast, ordinary synthetic single polymer hydrogels have relatively low strength and toughness due to their simple isotropic structure. Therefore, the introduction of double networks or nano-reinforced phases in single hydrogel networks to construct composite hydrogels and the introduction of multiple interactions (such as ionic / covalent cross-linking, hydrogen bonds, etc.) and complex hierarchical structures inside the hydrogels to improve the mechanical properties have been widely studied. However, high strength and high toughness are usually conflicting, and achieving both simultaneously in hydrogels has always been a huge challenge.

[0003] Inspired by the hierarchical ordered structure of muscle hydrogels and the multiple molecular interactions within nanocomposite hydrogels, high-strength and tough nanocomposite hydrogels with anisotropic hierarchical structures have received extensive attention and research. Applying electromagnetic fields, temperature fields or stress fields to nanocomposite hydrogels usually forms hierarchical ordered structures. Among them, the prestress-induced structural orientation strategy has been widely used in the preparation of anisotropic nanocomposite hydrogels due to its simple operation. However, since the prestress cannot act evenly on large-sized three-dimensional bulk hydrogels, this seriously limits its application. In addition, high-strength and tough composite hydrogels are usually chemically cross-linked, especially covalently cross-linked hydrogels. Once formed, the covalent bonds in them are difficult to break, so the prepared hydrogels are difficult to spontaneously degrade and recycle. With the extensive research and large-scale application of hydrogels in the future, the end products of hydrogels will undoubtedly cause waste of resources and environmental pollution, which is not conducive to the development of green economy and circular economy.

[0004] In recent years, ultra-small inorganic ion nanomaterials have shown great potential in constructing ultra-tough nanocomposites due to their small size effect. For example, the Chinese patent application with publication number CN110669231A discloses a high-toughness bionic muscle hydrogel material, which includes 10-40wt% calcium phosphate nanoclusters and 60-90wt% organic matter, wherein the organic matter includes PVA and sodium alginate, and the mass ratio of PVA to sodium alginate is 8:1-3:1. The invention also discloses a preparation method of a high-toughness bionic muscle hydrogel material and its application in the field of soft robots or biological tissue engineering. The bionic muscle hydrogel material provided by the invention has high strength and high toughness; the preparation method provided proposes a new preparation strategy for constructing an organic-inorganic composite hydrogel with a hierarchical and ordered structure, and the prepared muscle-like hydrogel has great application prospects in the fields of soft robots and biological tissue engineering. However, since the organic components PVA and sodium alginate that constitute the muscle-like hydrogel are both flexible long-chain molecular polymers, they can only form a two-phase ordered assembly of organic molecular chains and inorganic nanowires at the molecular and nanoscale by compounding with calcium phosphate nanoclusters; in addition, the sodium alginate molecules inside the muscle-like hydrogel are bound together with calcium phosphate through ionic bonds, and calcium alginate molecules will still exist under acidic conditions, making it impossible to achieve reversible recycling of the muscle-like hydrogel, which seriously limits the recycling and reuse of the hydrogel. Summary of the invention

[0005] The purpose of the present invention is to provide a recyclable high-strength and toughness composite hydrogel and a preparation method thereof, which can achieve a balance between high strength and high toughness and has the characteristics of recyclability; the present invention also provides the application of the recyclable high-strength and toughness composite hydrogel in the preparation of soft robot materials or biological tissue engineering materials in non-disease diagnosis and treatment.

[0006] The present invention provides the following technical solutions:

[0007] A method for preparing a recyclable high-strength and tough composite hydrogel, the preparation method comprising:

[0008] (1) Compounding a calcium phosphate oligomer (CPO) and an aqueous dispersion of aramid nanofibers (ANF) with a polyvinyl alcohol (PVA) aqueous solution to form a uniform slurry, and preparing an isotropic composite film by inorganic ion polymerization and self-assembly;

[0009] (2) immersing the composite film in water to reach swelling equilibrium, directional stretching until the internal structure of the film is reorganized, and immersing it in water again to reach swelling equilibrium, thereby obtaining a hydrogel film with a hierarchical and ordered structure;

[0010] (3) The single-layer hydrogel film prepared in step (2) is stacked layer by layer, bonded between layers with glue, dried after applying instantaneous compressive stress, and immersed in water again to achieve swelling equilibrium, thereby obtaining a high-strength and tough bulk hydrogel as a recyclable high-strength and tough composite hydrogel (also called high-strength and tough nanocomposite hydrogel).

[0011] The technical concept of the present invention is:

[0012] The organic main network is constructed with PVA aqueous solution, CPO with ultra-small size is used as the inorganic reinforcement phase, and ANF with high strength, high modulus and high stiffness is used as the organic reinforcement phase. It is compounded with PVA aqueous solution to form a uniform slurry, and an isotropic composite film is first prepared by inorganic ion polymerization and self-assembly. Among them, CPO is in situ polymerized in the PVA / ANF composite network to form one-dimensional ultrafine hydroxyapatite nanowires (HLs). The obtained composite film is then wet-stretched in water to a certain strain, so that the internal structure of the film is reorganized (the three one-dimensional components (one-dimensional PVA molecular chains, one-dimensional ANF and one-dimensional HLs) inside the film are orderly assembled into nanofibers). These nanofibers are further directionally assembled into a hydrogel fiber network on a macro scale.

[0013] Among them, PVA constitutes the main organic network structure of the composite film. In the process of forming the composite film, CPO gradually transforms into crystalline HLs through inorganic ion polymerization, and is combined with ANF and PVA molecular chains by hydrogen bonds. At the same time, hydrogen bonds are also formed between ANF and PVA, and finally multiple intermolecular hydrogen bonds are formed between PVA molecular chains, ANF and HLs.

[0014] Based on the CPO-induced organic-inorganic integration and synergistic toughening and prestress-induced structural orientation strategy, the prepared hydrogel film has multiple hydrogen bonds at the molecular scale and a hierarchical and ordered fiber network structure from the nano to macro scale, so the hydrogel exhibits excellent mechanical properties at the macro scale.

[0015] In order to further obtain a larger-sized three-dimensional bulk hydrogel, a layer-by-layer assembly and interlayer cross-linking strategy can be used, that is, the obtained hydrogel film is stacked layer by layer along the orientation, the layers are glued together, and then instantaneous stress is applied to strengthen the interlayer cross-linking. Finally, the obtained three-dimensional bulk sheet is naturally dried and immersed in water again to achieve water absorption equilibrium, and a large-sized, high-strength and tough three-dimensional bulk hydrogel is obtained.

[0016] In step (1), the preparation method of CPO is: triethylamine as a stabilizer, calcium salt as a calcium source, and phosphoric acid as a phosphorus source are added to an organic solvent to generate CPO; the concentration of calcium salt in the organic solvent is 0.001 to 0.1 mol L -1, keep the calcium-phosphorus molar ratio between 1 and 2, and the concentration of triethylamine between 0.02 and 1 mol L -1 .

[0017] The organic solvent is ethanol, ethylene glycol, glycerol and other organic solvents and mixed solvents thereof. The calcium salt solution reacts with phosphoric acid to produce CPO. The reaction temperature is about 25°C. First, CPO with ultra-small size (~1nm) is prepared as an inorganic reinforcement phase.

[0018] Preferably, the concentration of calcium salt is 0.02 to 0.05 mol L -1 , keep the calcium-phosphorus molar ratio between 1 and 1.67, and the concentration of triethylamine between 0.2 and 0.5 mol L -1 .

[0019] In step (1), the particle size of the CPO is 0.5 to 2.0 nm.

[0020] In step (1), the preparation method of ANF is as follows: using Kevlar fiber as raw material and using a saturated solution of potassium hydroxide (KOH) in dimethyl sulfoxide (DMSO) as solvent to perform deprotonation to achieve macroscopic fiber stripping and obtain ANF; wherein the mass ratio of Kevlar fiber to KOH is 0.2 to 2:1, and the mass ratio of DMSO to KOH is 1000 to 100:1.

[0021] Among them, ANF is used as the organic reinforcing phase.

[0022] Preferably, the mass ratio of Kevlar fiber to KOH is 0.5 to 1, and the mass ratio of DMSO to KOH is 500 to 200. The reaction temperature is about 25° C., and mechanical stirring is performed until a dark red viscous ANF solution is obtained, and then solvent exchange is performed with deionized water to obtain ANF.

[0023] In step (1), the feed ratio of the inorganic phase CPO to the organic phase PVA / ANF is 5-40wt%:60-95wt%; and the feed ratio of PVA to ANF is 6:1.

[0024] Among them, CPO is used to form a uniform slurry with ANF aqueous dispersion (concentration of 0.1-0.5wt%) and PVA aqueous solution (concentration of 1-10wt%). In this process, composite films with different strengths and toughness can be obtained by adjusting the amount of CPO added (5-40wt%).

[0025] Preferably, the concentration of the PVA aqueous solution is 1 to 5 wt %.

[0026] In step (2), the directional stretching is performed to a strain of 50 to 150%. The immersion in water is performed for 5 to 60 minutes. Preferably, the directional stretching is performed to a strain of 50 to 100%.

[0027] In step (3), the instantaneous compressive stress is 5 to 20 kPa. Preferably, the instantaneous compressive stress is 5 to 10 kPa.

[0028] In step (3), the glue is an emulsion obtained by mixing a PVA aqueous solution with CPO, and the mass percentage of CPO in the emulsion is 10 to 35 wt%.

[0029] The high-strength and tough composite hydrogel is sequentially demineralized by acid, dissolved by heating in water to obtain a uniform dispersion, and CPO is added to perform secondary inorganic ion polymerization and self-assembly to achieve reversible cyclic regeneration of the hydrogel.

[0030] Since the three components of the hydrogel are connected together by hydrogen bonds, the reversible recycling of the hydrogel can be achieved through acid demineralization, heating dissolution and redispersion, and subsequent secondary inorganic ion polymerization.

[0031] Specifically, the hydrogel film is immersed in a hydrochloric acid solution with a pH of 3.0, and the calcium phosphate minerals in the film will dissolve; then, the residual organic film phase is washed several times in deionized water, and then placed in 100°C boiling water and heated to dissolve to obtain a uniform dispersion; finally, CPO (5-40wt%) is added for secondary inorganic ion polymerization and self-assembly to achieve reversible cyclic regeneration of the hydrogel.

[0032] The present invention also provides a recyclable high-strength and tough composite hydrogel obtained by the above preparation method.

[0033] The present invention also provides an application of the above-mentioned recyclable high-strength and tough composite hydrogel in the field of preparing soft robot materials or biological tissue engineering materials for non-disease diagnosis and treatment.

[0034] Compared with the prior art, the present invention prepares a high-strength and tough nanocomposite hydrogel by in-situ inorganic ion polymerization of CPO in a polymer composite network composed of a one-dimensional PVA molecular chain and a one-dimensional ANF. In order to achieve a balance between high strength and high toughness, the present invention introduces ANF as an organic reinforcing phase into the PVA hydrogel matrix, and first constructs a PVA / ANF composite network. Then, CPO is in-situ polymerized in the PVA / ANF composite network as an inorganic reinforcing phase to form a one-dimensional ultrafine HLs. The organic PVA / ANF and the inorganic HLs form a complete structure from the molecular scale to the macroscopic scale to become an independent PVA / ANF / HL (PAHL) film. Subsequently, the obtained PAHL film is wet stretched in water to a strain of 100% to construct a hierarchical and ordered fiber structure. Due to the organic-inorganic integration and synergistic toughening induced by CPO, and the hierarchical and ordered fiber structure induced by prestress, the PAHL hydrogel film has excellent tensile strength (24.15±1.12MPa) and toughness (15.68±1.78MJ m -3 ), far exceeding the vast majority of single polymer hydrogels, dual / multi-network hydrogels and nanocomposite hydrogels. Through layer-by-layer assembly and interlayer crosslinking strategies, the present invention further prepares large-scale three-dimensional bulk hydrogels with excellent mechanical properties and significant energy absorption / dissipation capabilities.

[0035] In addition, since the prepared nanocomposite hydrogel has physical cross-linking properties and the inorganic mineral units inside the hydrogel can be dissolved under weakly acidic conditions, the reversible recycling of the hydrogel can be easily achieved by secondary polymerization of CPO in the PVA / ANF composite network, which lays the foundation for the sustainable large-scale production and application of the hydrogel. The high-strength and tough composite hydrogel based on the synergistic toughening of CPO and ANF provided by the present invention has important application prospects in the fields of soft robots, biological tissue engineering, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The scanning electron microscope image (left) and transmission electron microscope image (right) of the interior of the high-strength and tough composite hydrogel prepared in Example after drying.

[0037] Figure 2 Optical photograph of the high-strength and tough composite hydrogel film prepared in Example in water (left) and scanning electron microscope image of the interior after freeze-drying (right).

[0038] Figure 3 The high-strength and tough composite hydrogel film prepared in the example exhibits excellent flexibility (can be curled, twisted, knotted, and lifted heavy objects) and load-bearing capacity (lifting heavy objects and resisting impact).

[0039] Figure 4This is the tensile stress-strain curve of the high-strength and tough composite hydrogel film prepared in the example.

[0040] Figure 5 This is the cyclic tensile stress-strain curve of the high-strength and tough composite hydrogel film prepared in the example.

[0041] Figure 6 The high-strength and large-size bulk nanocomposite hydrogel material prepared in the example, and the prepared hydrogel strip also has excellent flexibility (bending, twisting) and load-bearing capacity.

[0042] Figure 7 Optical photographs of various stages of the reversible recycling process of the high-strength and tough composite hydrogel film prepared in the example, which undergoes acid demineralization, heating dissolution and dispersion, and subsequent secondary inorganic ion polymerization to achieve the reversible recycling of the hydrogel film.

[0043] Figure 8 This is the tensile stress-strain curve of the regenerated high-strength and tough composite hydrogel film prepared in the example.

[0044] Fig. 9 The process flow for preparing recyclable high-strength and tough composite hydrogels and the schematic diagram of the hierarchical and orderly structure inside the hydrogels. DETAILED DESCRIPTION

[0045] like Fig. 9 The figure shows the process flow of preparing recyclable high-strength and tough composite hydrogel and its internal network structure. CPO and ANF are used as inorganic and organic reinforcing phases, respectively, and composited with PVA aqueous solution. The composite film is prepared by inorganic ion polymerization and self-assembly strategy. The film is then immersed in deionized water for 5 to 60 minutes and stretched to a strain of 50 to 150%. The internal structure is reorganized from a disordered mesh structure to an ordered fiber network structure, and HLs form an ordered crystal array driven by PVA molecular chains and ANF.

[0046] Preparation of CPO: Prepare an ethanol solution of calcium chloride: 5.88 g of calcium chloride dihydrate was dissolved in 0.80 L of anhydrous ethanol, 110.90 mL of triethylamine was added, and the mixture was stirred for 30 min. Then, an ethanol solution of phosphoric acid (2.09 mL of phosphoric acid was dissolved in 80 mL of ethanol) was added, and the mixture was stirred vigorously for 12 h. A white gel was obtained by centrifugation, which was washed three times with ethanol, centrifuged, and dispersed in ethanol to prepare a concentration of 10 mg mL -1 CPO.

[0047] Preparation of ANF: First, prepare a DMSO solution of KOH, i.e., add 5.00 g of KOH into 1.00 L of DMSO to form a saturated solution. Then, cut 5.00 g of Kevlar fiber into pieces with scissors and transfer them to the saturated DMSO solution of KOH. Mechanically stir until the Kevlar fiber is completely dissolved to form a dark red viscous solution. Then transfer it to a 3.00 L beaker, add 2.00 L of boiling water, perform solvent exchange, and precipitate ANF. Then, wash it three times with deionized water to obtain an aqueous dispersion of ANF nanofibers (0.5 wt%).

[0048] Preparation of recyclable high-strength and tough composite hydrogel films:

[0049] (1) Take 60g of 0.5wt% ANF dispersion and add 60g of 3.0wt% PVA aqueous solution, stir vigorously for 30min to form a uniform dispersion. -1 The CPO was placed in a centrifuge tube and centrifuged at 6000 rpm for 5 min. The supernatant was discarded and the obtained CPO gel was added to the above dispersion and stirred vigorously for 3 h. Finally, the uniform slurry was transferred to a 12 cm × 12 cm culture dish, dried at room temperature, and finally peeled off from the culture dish to obtain a dry composite film.

[0050] (2) The film is immersed in water for 5 to 60 minutes to reach swelling equilibrium, and then taken out and directional stretched to a strain of 100% to obtain a hydrogel film.

[0051] (3) Spread the single-layer hydrogel film layer by layer, and pass a special glue between the layers (glue preparation: take 30mL of 10mg mL -1 The CPO was placed in a centrifuge tube and centrifuged at 6000rpm for 5 minutes. The supernatant was discarded and the obtained CPO gel was added to 30g PVA aqueous solution (3.0wt%), stirred evenly and part of the water was evaporated to form a glue with a certain viscosity and fluidity) to bond together. Then, an instantaneous compressive stress of 10kPa was applied to the bonded layered film bulk composite material to make the layers tightly connected. After natural drying, it was immersed in water again to reach swelling equilibrium, and a large-sized, high-strength and tough three-dimensional bulk hydrogel was obtained.

[0052] like Figure 1 As shown, the composite hydrogel film prepared in this embodiment has a highly ordered internal structure, and the ultrafine HLs, PVA molecular chains, and ANF are highly integrated together to form composite nanofibers.

[0053] like Figure 2 As shown, the composite nanofibers prepared in this example are orderly assembled into a macroscopic hydrogel film.

[0054] like Figure 3 As shown, the hydrogel film prepared in this embodiment has excellent toughness and can be curled and knotted arbitrarily; at the same time, it exhibits excellent load-bearing and impact resistance.

[0055] like Figure 4 As shown in Figure 2, the tensile strength of the hydrogel film prepared in this example is 24.15±1.12MPa, and the toughness is 15.68±1.78MJ m -3 , the elastic modulus is 18.56±7.13MPa.

[0056] like Figure 5 As shown, under cyclic stress, the hydrogel film prepared in this example exhibits excellent mechanical stability.

[0057] like Figure 6 As shown, in this embodiment, a large-sized bulk hydrogel material can be prepared through layer-by-layer assembly and interlayer cross-linking. The prepared hydrogel strip also has the ability to curl, twist, tie a knot, and carry loads.

[0058] like Figure 7 As shown, the high-strength and tough composite hydrogel prepared in this embodiment can achieve reversible cyclic regeneration of the hydrogel film after acid demineralization, heating dissolution and dispersion, and subsequent secondary inorganic ion polymerization. The specific method is: take 3g of dry gel fragments (the hydrogel fragments are placed in an 80°C drying oven until completely dry) and transfer them to 100mL of hydrochloric acid aqueous solution (pH=3.0) for 30 minutes, take them out, repeatedly wash with deionized water to remove residual acid, and then transfer them to 30mL of deionized water, heat to boiling, and stir vigorously until the gel fragments are completely broken up and a uniform dispersion is formed. Then add the evaporated water until 30mL, and add CPO (100mL, 10mg mL -1 ) and stir evenly to form a uniform slurry, and then realize secondary inorganic ion polymerization of CPO in the drying process to form an isotropic regenerated hydrogel film. In order to obtain a hierarchical and ordered nanocomposite structure, the regenerated hydrogel film is immersed in water again for 5 to 60 minutes to reach swelling equilibrium. After being taken out, it is directional stretched to a strain of 100% to obtain a regenerated hierarchical and ordered hydrogel film.

[0059] like Figure 8 As shown in Figure 2, the tensile strength, elastic modulus, and toughness of the regenerated hydrogel were 23.21 ± 2.59 MPa, 17.28 ± 5.94 MPa, and 14.76 ± 3.67 MJ m -3 , which is basically consistent with the original hydrogel.

Claims

1. A method for preparing a recyclable high-strength and tough composite hydrogel, characterized in that: The preparation method comprises: (1) Compounding a calcium phosphate oligomer (CPO) and an aqueous dispersion of aramid nanofibers (ANF) with a polyvinyl alcohol (PVA) aqueous solution to form a uniform slurry, and preparing an isotropic composite film by inorganic ion polymerization and self-assembly; (2) immersing the composite film in water to reach swelling equilibrium, directional stretching until the internal structure of the film is reorganized, and immersing it in water again to reach swelling equilibrium, thereby obtaining a hydrogel film with a hierarchical and ordered structure; (3) The hydrogel film prepared in step (2) is stacked layer by layer, bonded between layers with glue, dried after applying instantaneous compressive stress, and immersed in water again to achieve swelling equilibrium, thereby obtaining a high-strength and tough bulk hydrogel as a recyclable high-strength and tough composite hydrogel.

2. The method for preparing a recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: In step (1), the preparation method of CPO is: triethylamine as a stabilizer, calcium salt as a calcium source, and phosphoric acid as a phosphorus source are added to an organic solvent to generate CPO; the concentration of calcium salt in the organic solvent is 0.001 to 0.1 mol L -1 , keep the calcium-phosphorus molar ratio between 1 and 2, and the concentration of triethylamine between 0.02 and 1 mol L -1 ; The particle size of the CPO is 0.5 to 2.0 nm.

3. The method for preparing the recyclable high-toughness composite hydrogel according to claim 1, characterized in that: In step (1), the preparation method of ANF is as follows: using Kevlar fiber as raw material and using a saturated solution of potassium hydroxide (KOH) in dimethyl sulfoxide (DMSO) as solvent to perform deprotonation to achieve macroscopic fiber stripping and obtain ANF; wherein the mass ratio of Kevlar fiber to KOH is 0.2 to 2:1, and the mass ratio of DMSO to KOH is 1000 to 100:

1.

4. The method for preparing the recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: In step (1), the feed ratio of the inorganic phase CPO to the organic phase PVA / ANF is 5-40wt%:60-95wt%; and the feed ratio of PVA to ANF is 6:

1.

5. The method for preparing the recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: In step (2), the directional stretching is performed to a strain of 50 to 150%.

6. The method for preparing a recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: In step (3), the instantaneous compressive stress is 5 to 20 kPa.

7. The method for preparing a recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: In step (3), the glue is an emulsion obtained by mixing a PVA aqueous solution with CPO, and the mass percentage of CPO in the emulsion is 10 to 35 wt%.

8. The method for preparing a recyclable high-strength and tough composite hydrogel according to claim 1, characterized in that: The high-strength and tough composite hydrogel is sequentially demineralized by acid, dissolved by heating in water to obtain a uniform dispersion, and CPO is added to perform secondary inorganic ion polymerization and self-assembly to achieve reversible cyclic regeneration of the hydrogel.

9. A recyclable high-strength and tough composite hydrogel obtained by the preparation method according to any one of claims 1 to 8.

10. An application of the recyclable high-strength and tough composite hydrogel according to claim 9 in the field of preparing soft robotic materials or biological tissue engineering materials for non-disease diagnosis and treatment.

Citation Information

Patent Citations

  • High-toughness bionic muscle hydrogel material and preparation method and application thereof

    CN110669231A

  • Micron and nano material-enhancing bionic layered composite material and manufacturing method thereof

    CN102706219A

  • High-performance rubber composite material containing Kevlar nano-fibers and preparation method thereof

    CN108424563A

  • High-strength and high-tenacity organic-inorganic complex macroscale fiber and preparation and application thereof

    CN110117830A

  • Aramid nanofiber / polyvinyl alcohol / gold / conductive polyaniline composite film material and preparation method thereof

    CN110790967A