A lubricating ester-resistant PA composition and its preparation method and application

Through the synergistic effect of high-end amino PA resin and high molecular weight antioxidants, lubricating ester PA compositions were prepared, which solved the problem of performance decay of PA compositions under high heat and lubricating ester in the prior art, and achieved high temperature and lubrication Good mechanical properties maintained in the ester environment.

CN115584125BActive Publication Date: 2024-11-19KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211138492.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-19
Publication Date
2024-11-19
Estimated Expiration
2042-09-19

AI Technical Summary

Technical Problem

The existing PA compositions have decayed performance under the action of high heat and lubricating ester, which cannot meet the needs of high-speed rail and passenger cars.

Method used

The lubricating ester PA composition is prepared through the twin screw extrusion process using a high-end amino group content PA resin and a high-molecular weight antioxidant, which increases the high temperature and lubricating ester resistance of the composition.

Benefits of technology

After the lubricating ester resistance test at 1000h and 140°C, the tensile strength retention rate of the composition reaches more than 100%, the bending strength retention rate reaches more than 98%, and the impact retention rate of the cantilever beam notch is 78-94%, satisfying rail transit bearings Application requirements of cages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003853134520000051
    Figure BDA0003853134520000051
  • Figure BDA0003853134520000071
    Figure BDA0003853134520000071
  • Figure BDA0003853134520000081
    Figure BDA0003853134520000081
Patent Text Reader

Abstract

The present invention discloses a lubricating ester-resistant PA composition and its preparation method and application, belonging to the technical field of engineering plastics. The lubricating ester-resistant PA composition of the present invention comprises the following components by weight: 40 to 80 parts of PA resin, 10 to 50 parts of reinforcing fiber, and 0.1 to 3 parts of antioxidant, wherein the terminal amino content of the PA resin is ≥30mmol / kg, and the weight average molecular weight of the antioxidant is ≥600. The lubricating ester-resistant PA composition of the present invention uses a PA resin with a terminal amino content that is resistant to heat degradation as a base resin, and cooperates with a high molecular weight antioxidant, and has good heat-resistant and lubricating ester-resistant effects. After 1000h, 140°C lubricating ester resistance test, the tensile strength retention rate is maintained at more than 98%, the bending strength retention rate is maintained at more than 88%, and it has good toughness, and the cantilever beam notch impact retention rate is maintained at 78-94%, which can be widely used in the field of rail transit bearing retainers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of engineering plastics, and more specifically, to a lubricating ester-resistant PA composition and a preparation method and application thereof. Background Art

[0002] Polyamide 66 (PA66) is a widely used material in engineering plastics. It has excellent heat resistance, solvent resistance, mechanical and processing properties, and is widely used in electronics, rail transit, power tools, home appliances, sports equipment and other fields. In rail transit, bearings are essential components, and the bearing cage in the bearing plays the role of isolating and retaining the rolling element. During the operation of the bearing, the bearing cage will be subjected to great centrifugal force, impact and vibration, and friction will generate a lot of heat, which puts forward higher mechanical, wear and heat resistance requirements for the performance of the bearing cage. In addition, the bearing cage is also subject to the effects of chemical media such as lubricants, lubricant additives, organic solvents and coolants, so there are also high requirements for the solvent resistance of the bearing cage. At present, non-metallic cage materials can be made of nylon, phenolic tape, polytetrafluoroethylene and other materials. Among them, nylon materials have been widely used due to their balanced heat resistance, mechanical, wear resistance, cost and other advantages. However, due to the effects of high heat and lubricating esters, ordinary nylon will have a large performance attenuation and cannot meet the use requirements of high-speed rail, passenger car and other industries.

[0003] The prior art discloses a high-end amino-stabilized polyamide composition containing a copper compound, comprising: (A) a first raw material component that can undergo a polycondensation reaction to form an amide group; (B) a second raw material component that can react with the first raw material component (A) to form an amide group; (C) an organic copper component; and (D) an antioxidant, wherein the organic copper component (C) is mainly composed of a mixture of an organic copper salt and a halogen, wherein the organic copper component is added in an amount of 15 to 50 g per kilogram of solute in the above-mentioned salt solution. It aims to solve the technical defects of polyamide in terms of stability performance under light and heat conditions. By controlling the content of terminal amino and carboxyl groups on the polyamide molecular chain and synergizing with the above-mentioned organic copper component and antioxidant, the high-end amino-stabilized polyamide composition containing copper compounds obtained has outstanding thermal stability and effectively improves the phenomenon of discoloration of the material due to long-term exposure to high temperature. It can be used in a high-temperature environment. When used under long-term light or high temperature, it has outstanding stability and maintains excellent mechanical strength and appearance. However, it fails to improve the performance stability of the polyamide composition under high heat and lubricating esters. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects and shortcomings of existing PA compositions that show significant performance degradation under high heat and lubricating ester, and to provide a lubricating ester-resistant PA composition. The PA composition has a synergistic effect of a high-end amino-content PA resin that is resistant to thermal decomposition and a high-molecular-weight antioxidant, thereby significantly improving the high-temperature and lubricating ester resistance of the PA composition, and still has good mechanical properties after a lubricating ester resistance test at 140°C for 1000 hours.

[0005] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0006] A lubricating ester-resistant PA composition, comprising the following components in parts by weight:

[0007] PA resin 40-80 parts, reinforcing fiber 10-50 parts, antioxidant 0.1-3 parts,

[0008] The terminal amino group content of the PA resin is ≥30 mmol / kg, determined according to HG / T 4182-2012, and the weight average molecular weight of the antioxidant is ≥600.

[0009] Among them, it should be noted that:

[0010] The terminal amino group content of the PA resin of the present invention is tested according to the HG / T 4182-2012 standard.

[0011] Under high heat and lubricating ester conditions, the PA composition will experience significant performance degradation mainly because the antioxidant is extracted by the lubricating ester under high heat conditions, and nylon is easily degraded under high temperature conditions. The high heat lubricating ester causes nylon degradation, which in turn leads to a decrease in the mechanical properties of the PA composition.

[0012] The actual application of PA compositions often involves application scenarios that require contact with solvents. If the molecular weight of the antioxidant is too low, it is easy to be extracted by the solvent, affecting the stability of the PA combination system. Low molecular weight antioxidants are also prone to precipitation, frosting and other problems, which is not conducive to maintaining the stable compatibility of the PA combination system.

[0013] At the same time, the base resin in the PA composition of the present invention is a PA resin, and the terminal amino content of the PA resin is ≥30mmol / kg, and the determination method is HG / T 4182-2012. The terminal group structure is directly related to the molecular heat degradation resistance of the PA resin. The high-end amino PA resin has excellent degradation resistance. Thermal crosslinking at high temperature will release alkaline ammonia gas to slow down degradation, and the moderately generated crosslinked structure will further improve the performance. Ordinary PA high-temperature crosslinking will release water, further promoting the hydrolysis reaction of nylon. The lubricating ester-resistant PA composition of the present invention reduces the problem of antioxidant being extracted by the medium during use by using a high molecular weight extraction-resistant antioxidant. The high molecular weight antioxidant is used in combination with the high-end amino resin, which plays a significant synergistic role and can obtain a higher performance retention rate.

[0014] Preferably, the following components are included in parts by weight:

[0015] 50-70 parts of PA resin, 15-45 parts of reinforcing fiber, and 0.3-2.5 parts of antioxidant.

[0016] In order to further improve the high-heat lubricating ester resistance of the PA resin, preferably, the terminal amino group content of the PA resin is 50 to 80 mmol / kg, and the determination method is HG / T 4182-2012.

[0017] Preferably, the PA resin is PA66.

[0018] Preferably, the antioxidant is a hindered phenol antioxidant.

[0019] Further preferably, the antioxidant is a hindered phenol antioxidant with a weight average molecular weight of 700 to 1200. Increasing the molecular weight of the antioxidant is beneficial to improving its heat resistance and extraction resistance, but increasing the molecular weight will also cause the proportion of functional groups with antioxidant effects to decrease, the antioxidant effect to decrease, and the difficulty of synthesis and cost to increase. Therefore, it is necessary to comprehensively consider the balance between its basic efficacy and heat resistance and extraction performance. The weight average molecular weight of the antioxidant is preferably 700 to 1200.

[0020] In a specific embodiment, the antioxidant of the present invention can be one or more of antioxidant 1098, antioxidant 1790 or antioxidant 1010.

[0021] The reinforcing fiber of the present invention can be one or more of glass fiber, carbon fiber, organic fiber, mineral fiber or metal fiber.

[0022] The present invention also specifically protects a method for preparing a lubricating ester-resistant PA composition, comprising the following steps:

[0023] The PA resin and the antioxidant are mixed evenly, added into a twin-screw extruder for extrusion granulation, and reinforcing fibers are added by side feeding, and extrusion granulation is performed to obtain a lubricating ester-resistant PA composition.

[0024] Among them, it should be noted that:

[0025] In the preparation method of the lubricating ester-resistant PA composition of the present invention, side-feeding the reinforcing fibers is more conducive to increasing the fiber retention length and improving the performance.

[0026] In a specific embodiment, the twin-screw extrusion process is as follows:

[0027] Extrusion temperature: Zone 1 170-190°C, Zone 2 250-270°C, Zone 3 260-280°C, Zone 4 265-285°C, Zone 5 265-285°C, Zone 6 265-285°C, Zone 7 260-280°C, Zone 8 260-280°C, Zone 9 260-280°C;

[0028] The screw speed is 300-500 rpm.

[0029] The use of the lubricating ester-resistant PA composition of the present invention in the preparation of a bearing retainer is also within the protection scope of the present invention.

[0030] The present invention also specifically protects a bearing retainer, which is prepared from the lubricating ester-resistant PA composition of the present invention.

[0031] The bearings of rail transit need to have good mechanical property retention rate under high temperature and chemical medium lubricant in working state. The ester-resistant PA composition provided by the present invention has a tensile strength retention rate of more than 100% and a bending strength retention rate of more than 98% after 1000h and 140°C ester-resistant test under high temperature and ester. At the same time, it has good toughness and the cantilever beam notch impact retention rate is maintained at more than 89%, which fully meets the application performance requirements of rail transit bearing cages and can be widely used in the preparation of bearing cages and in the field of rail transit.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The lubricating ester-resistant PA composition of the present invention uses a PA resin with a terminal amino content that is resistant to heat degradation as a base resin. The terminal group structure is directly related to the molecular heat degradation resistance of the PA resin. The high-end amino PA resin has excellent degradation resistance. Thermal crosslinking at high temperature will release alkaline ammonia gas to slow down degradation. The moderately generated crosslinking structure will further improve the performance. At the same time, it cooperates with a high molecular weight extraction-resistant antioxidant to reduce the problem of the antioxidant being extracted by the medium during use. The high molecular weight antioxidant and the high-end amino resin are used in combination, which has a significant synergistic effect and can obtain a higher performance retention rate.

[0034] After a 1000h, 140°C ester resistance test, the ester-resistant PA composition of the present invention has a tensile strength retention rate of more than 98%, a flexural strength retention rate of more than 88%, good toughness, and a cantilever beam notch impact retention rate of 78-94%. The composition has good heat resistance and ester resistance, and can be widely used in the field of rail transit bearing retainers. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0036] The raw material information of the embodiments and comparative examples of the present invention are as follows:

[0037] PA66 resin:

[0038] PA66-1: EP-158, terminal amino content 50mmol / kg, Huafeng Group Co., Ltd.

[0039] PA66-2: EP-158NH, terminal amino content 80mmol / kg, Huafeng Group Co., Ltd.

[0040] PA66-3: PA66 EPR27, terminal amino content 40mmol / kg, Shenzhen Shenma Chemical Co., Ltd.;

[0041] PA66-4: PA66 EPR32, terminal amino content 25mmol / kg, Shenzhen Shenma Chemical Co., Ltd.;

[0042] PA66-5: Homemade, the terminal amino content is controlled by the content of hexamethylenediamine, the terminal amino content is 85mmol / kg, the preparation method is as follows:

[0043] (1) reacting 1,6-hexanediamine and 1,6-hexanediamine in a molar ratio of 0.92:1 in water to form a salt solution with a mass concentration of 50%, and adding 21.1 mmol of 1,6-hexanediamine per kilogram of solute in the formed salt solution;

[0044] (2) raising the temperature to 155° C. and the pressure to 0.25 MPa in a concentration kettle for 60 minutes to concentrate the polyamide mixed salt solution to a mass concentration of 75%;

[0045] (3) transferring the concentrated polyamide salt mixed solution to a high-pressure reactor, raising the pressure to 1.7 MPa and the temperature to 210° C. for 15 minutes; then raising the temperature to 265° C. and stabilizing the pressure at 1.85 MPa for 60 minutes; further raising the temperature to 280° C. and slowly decreasing the pressure to normal pressure for 60 minutes; reducing the pressure in the reactor to 0 MPa for 30 minutes, injecting nitrogen and increasing the pressure to 0.5 MPa, opening the valve at the bottom of the polymerization reactor, extruding the material strips from the orifice plate, and pelletizing to obtain the desired polyamide composition particles PA66-5;

[0046] PA6 resin: PA6 HY2800A, Haiyang Chemical Fiber, terminal amino content 43mmol / kg.

[0047] Antioxidants:

[0048] Antioxidant 1098, weight average molecular weight 637, manufacturer: BASF;

[0049] Antioxidant 1790, weight average molecular weight 700, manufacturer: Solvay;

[0050] Antioxidant 1010, weight average molecular weight 1178, manufacturer: Tianjin Lianlong;

[0051] Antioxidant Sumisorb 400, weight average molecular weight 438, manufacturer: Shanghai Yasuda Chemical Co., Ltd.;

[0052] Reinforcement fiber: Glass fiber ECS10-03-568H, China Jushi Co., Ltd.

[0053] Lubricating grease: Great Wall IV type railway vehicle rolling bearing lubricating grease, commercially available.

[0054] Examples 1 to 11

[0055] A lubricating ester-resistant PA composition, comprising the components shown in Table 1 below, in parts by weight:

[0056] Table 1. Composition of ester-resistant PA compositions of Examples 1 to 11

[0057]

[0058] The preparation method of the ester-resistant PA composition of the above-mentioned embodiments 1 to 11 comprises the following steps:

[0059] The PA resin and the antioxidant are mixed evenly, added into a twin-screw extruder for extrusion granulation, and reinforcing fibers are added by side feeding, and extrusion granulation is performed to obtain a lubricating ester-resistant PA composition.

[0060] Wherein, the twin-screw extrusion process is as follows:

[0061] Extrusion temperature: Zone 1 190℃, Zone 2 260℃, Zone 3 270℃, Zone 4 275℃, Zone 5 275℃, Zone 6 275℃, Zone 7 270℃, Zone 8 270℃, Zone 9 270℃;

[0062] The screw speed was 400 rpm.

[0063] Comparative Examples 1 to 4

[0064] A PA composition, in parts by weight, comprises the components shown in Table 2 below:

[0065] Table 2. Composition of PA compositions of Comparative Examples 1 to 4

[0066] Comparative Example 1 2 3 4 PA66-2 40 80 65 PA66-4 65 Antioxidant 1010 4 0.08 0.5 Antioxidant Sumisorb 400 0.5 Glass fiber ECS10-03-568H 10 50 25 25

[0067] The preparation method of the ester-resistant PA composition of Comparative Examples 1 to 4 comprises the following steps:

[0068] The PA resin and the antioxidant are mixed evenly, added into a twin-screw extruder for extrusion granulation, and reinforcing fibers are added by side feeding, and extrusion granulation is performed to obtain a lubricating ester-resistant PA composition.

[0069] Wherein, the twin-screw extrusion process is as follows:

[0070] Extrusion temperature: Zone 1 190℃, Zone 2 260℃, Zone 3 270℃, Zone 4 275℃, Zone 5 275℃, Zone 6 275℃, Zone 7 270℃, Zone 8 270℃, Zone 9 270℃;

[0071] The screw speed was 400 rpm.

[0072] Results

[0073] The performance stability of the grease-resistant PA compositions of Examples 1 to 11 and the PA compositions of Comparative Examples 1 to 4 under high heat and grease was tested, and the specific testing method is as follows:

[0074] The test method for high temperature resistant lubricating grease is as follows:

[0075] The granulated particles were injection molded into mechanical specimens at 290°C using an injection molding machine. The specimen size was prepared according to the ISO standard mechanical specimen. The mechanical specimen was completely immersed in lubricating grease and then placed in an oven for testing. The test conditions were 140°C and the test time was 1000 hours.

[0076] The high temperature resistance test method is as follows:

[0077] The granulated particles were injection molded into mechanical specimens at 290°C using an injection molding machine. The specimen size was prepared according to the ISO standard mechanical specimen, and then put into an oven for testing. The test conditions were 140°C and the test time was 1000h.

[0078] The tensile strength, flexural strength and Izod notched impact strength were tested before and after the high temperature resistance test and the high temperature resistant lubricating grease test, and the performance retention rate was calculated.

[0079] Retention rate 1 = performance after high temperature resistant lubricating grease test / performance before high temperature resistant lubricating grease test * 100%

[0080] Retention rate 2 = performance after high temperature resistance test / performance before high temperature resistance test*100%.

[0081] Among them, the tensile strength is tested according to ISO 527-2012 standard:

[0082] Bending strength is tested according to ISO 178-2019 standard:

[0083] Izod notched impact strength is tested according to ISO 180-2019 standard:

[0084] The specific test results before and after the high temperature resistant lubricating grease test are shown in Tables 3 and 4 below.

[0085] Table 3. Test results of Examples 1 to 11

[0086] Example 1 2 3 4 5 6 7 8 9 10 11 Tensile strength retention rate 1 / % 94 92 98 95 95 96 91 95 98 93 91 Bending strength retention rate 1 / % 92 91 93 92 90 93 88 92 95 91 88 Izod notch impact retention rate 1 / % 87 81 90 89 94 89 79 88 91 87 78

[0087] Table 4. Test results of comparative examples 1 to 4

[0088] Comparative Example 1 2 3 4 Tensile strength retention rate 1 / % 84 83 81 83 Bending strength retention rate 1 / % 85 83 80 84 Izod notch impact retention rate 1 / % 74 73 71 73

[0089] The specific test results before and after the high temperature resistance test are shown in Tables 5 and 6 below.

[0090] Table 5. Test results of Examples 1 to 11

[0091] Example 1 2 3 4 5 6 7 8 9 10 11 Tensile strength retention rate 2 / % 98 88 95 90 94 95 93 93 93 97 93 Bending strength retention rate 2 / % 96 83 92 85 91 92 89 90 89 96 89 Izod notched impact retention rate 2% 93 83 88 87 93 94 91 91 91 92 92

[0092] Table 6. Test results of comparative examples 1 to 4

[0093]

[0094]

[0095] It can be seen from Table 3 that the terminal amino content of PA in the ester-resistant PA compositions of Examples 1 to 11 of the present invention is all above 30 mmol / kg, and the terminal group structure is directly related to the molecular heat degradation resistance of the PA resin. The high-end amino PA resin has excellent degradation resistance, and thermal crosslinking at high temperature will release alkaline ammonia gas to slow down degradation. The moderately generated crosslinked structure will further improve the performance. At the same time, in Examples 1 to 11, by using a high molecular weight extraction-resistant antioxidant with a weight average molecular weight greater than 600, the problem of the antioxidant being extracted by the medium during use is reduced. The high molecular weight antioxidant is used in combination with the high-end amino resin, which has a significant synergistic effect. After being tested at 140°C for 1000h with high temperature resistant lubricating ester, it still has a good mechanical property retention rate, wherein the tensile strength retention rate is maintained at 91-98%, and the bending strength retention rate is maintained at more than 88%. At the same time, it has good toughness, and the cantilever beam notch impact retention rate is maintained at 78-94%, which fully meets the application performance requirements of rail transit bearing cages, and can be widely used in the preparation of bearing cages and in the field of rail transit.

[0096] From the test results of Comparative Examples 1 to 4 in Table 4, it can be seen that the good high temperature resistant lubricating ester effect cannot be achieved outside the protection scope of the present invention:

[0097] In Comparative Example 1, excessive antioxidant was added, and the tensile strength retention rate could not be achieved, and adding too much antioxidant would increase the manufacturing cost. In Comparative Example 2, too little antioxidant was added, and the tensile strength retention rate, bending strength retention rate and cantilever beam notched impact retention rate of the PA composition could not meet the requirements of the present invention. It can be seen from Comparative Examples 1 and 2 that the content of each component in the lubricating ester-resistant PA composition of the present invention is quite important, and the high-heat lubricating ester performance retention rate of the present invention can only be achieved within the synergistic dosage range of the present invention.

[0098] In comparative example 3, the PA resin is PA66-4, and the terminal amino group content is 25 mmol / kg, which is lower than 30 mmol / kg. In comparative example 4, the antioxidant is the antioxidant Sumisorb 400, and the weight average molecular weight is 438, which is lower than 600. Both cannot achieve the effect of the high temperature resistant lubricating ester of the present invention.

[0099] Similarly, it can be seen from Tables 5 and 6 that the amount of antioxidant added and the terminal amino content of PA have a certain influence on the high temperature resistance. It can also be seen from the comparative example that the PA composition has high temperature resistance but does not have good high temperature resistant lubricating ester performance.

[0100] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A lubricating ester-resistant PA composition, characterized in that: In parts by weight, it includes the following components: PA resin 40-80 parts, reinforcing fiber 10-50 parts, antioxidant 0.1-3 parts, The terminal amino content of the PA resin is ≥30mmol / kg, and the determination method is HG / T 4182-2012; The antioxidant is antioxidant 1790.

2. The ester-resistant PA composition according to claim 1, characterized in that: In parts by weight, it includes the following components: 50-70 parts of PA resin, 15-45 parts of reinforcing fiber, and 0.3-2.5 parts of antioxidant.

3. The ester-resistant PA composition according to claim 1, characterized in that: The terminal amino group content of the PA resin is 50 to 80 mmol / kg, and the determination method is HG / T 4182-2012.

4. The ester-resistant PA composition according to claim 1, characterized in that: The antioxidant is a hindered phenol antioxidant.

5. The ester-resistant PA composition according to claim 1, characterized in that: The reinforcing fiber is one or more of carbon fiber, organic fiber, mineral fiber or metal fiber.

6. A method for preparing the lubricating ester-resistant PA composition according to any one of claims 1 to 5, characterized in that: The steps include: The PA resin and the antioxidant are mixed evenly, added into a twin-screw extruder for extrusion granulation, and reinforcing fibers are added by side feeding, and extrusion granulation is performed to obtain a lubricating ester-resistant PA composition.

7. The method for preparing the ester-resistant PA composition according to claim 6, characterized in that: The twin-screw extrusion process is as follows: Extrusion temperature: Zone 1 170-190°C, Zone 2 250-270°C, Zone 3 260-280°C, Zone 4 265-285°C, Zone 5 265-285°C, Zone 6 265-285°C, Zone 7 260-280°C, Zone 8 260-280°C, Zone 9 260-280°C; The screw speed is 300-500 rpm.

8. Use of the lubricating ester-resistant PA composition according to any one of claims 1 to 5 in preparing a bearing retainer.

9. A bearing retainer, characterized in that: The bearing retainer is prepared from the lubricating ester-resistant PA composition according to any one of claims 1 to 5.