Method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry

Through inductively coupled plasma emission spectroscopy and microwave digestion technology, the problem of low detection efficiency of 19 elements in sponge titanium and titanium alloys is solved, and fast and accurate detection is achieved, cost is reduced, and the loss of silicon is effectively avoided. Improve detection sensitivity.

CN115586175BActive Publication Date: 2024-11-15PANXI VANADIUM & TITANIUM INSPECTION & TESTING INST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211184019.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-15
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

The prior art cannot quickly and accurately detect the content of 19 trace elements in sponge titanium and titanium alloys, and the detection efficiency is low and there is a problem that element detection does not meet the industry's needs.

Method used

The inductively coupled plasma emission spectroscopy was used to treat the samples through microwave digestion technology, using hydrochloric acid, hydrofluoric acid, nitric acid and perchloric acid as solvents, combined with multi-spectral fitting technology and standard curve method, optimize the equipment parameters to simultaneously measure the sponge The content of 19 elements in titanium and titanium alloys.

Benefits of technology

It realizes rapid and accurate detection of 19 elements in titanium sponge and titanium alloy, improves detection efficiency, reduces labor and material costs, solves the problem of loss of silicon under hydrofluoric acid solvent, and enhances the detection of low-content elements. Sensitivity and detection ability of high content elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for measuring the contents of 19 elements in titanium sponge and titanium alloy by inductively coupled plasma emission spectrometry, and belongs to the technical field of nonferrous metal material detection. The invention uses hydrochloric acid, hydrofluoric acid, nitric acid and perchloric acid as solvents, adopts microwave digestion technology to process samples, uses Ar420.073 line as internal standard, uses high-purity titanium (titanium ≥ 99.98%) as matrix matching, combines MSF, adopts standard curve method for quantitative analysis, optimizes equipment parameters, eliminates the mutual influence of matrix and each detection element in a targeted manner, and establishes a method for determining the contents of 19 elements (iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium and copper) in titanium sponge and titanium alloy by inductively coupled plasma emission spectrometry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal material detection, and specifically relates to a method for measuring the contents of 19 trace elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectroscopy. Background Art

[0002] At present, the domestic demand for high-end titanium sponge and titanium materials has experienced explosive growth, while the foreign market demand for domestic general industrial titanium sponge and titanium materials is weak.

[0003] The reasons for the low quality of titanium sponge and titanium materials in my country, in addition to scientific and technological innovation, technical processes and other factors, accurate and efficient detection technology is also one of the important factors. First, the detection efficiency is low due to the excessive dispersion of inspection standards. In the current domestic standard methods for the detection of titanium sponge and titanium alloys (GB / T 4698.1-28), there are 18 detection method standards for the detection of 19 chemical components such as iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium, and copper. If multiple elements are measured at the same time, it will take a lot of time and the detection cycle will be long. This is inconsistent with the current production of high-quality titanium sponge and titanium alloys. Efficient and rapid detection needs. Secondly, some element detection standards no longer meet the current industry detection needs. For example, according to the requirements of the new national standard for titanium sponge (GB / T 2524-2019), the quality grade in the standard is 0. A The silicon content of titanium sponge impurities is ≤0.01%, while the lower limit of determination in GB / T 4698.3-2017 "Chemical Analysis Methods for Titanium Sponge, Titanium and Titanium Alloys - Determination of Silicon Content by Molybdenum Blue Photometry" is 0.010%, which can no longer meet the inspection requirements of the new standard. GB / T 4698.21 uses direct current arc atomic emission spectrometry (DCP-AES) to detect the 10 chemical components of manganese, chromium, nickel, aluminum, molybdenum, tin, vanadium, yttrium, copper and zirconium in titanium alloys. The detection element range is 0.001-0.2%. There are two main problems. First, the detection method uses powder state sample injection, and the chipped sample needs to be acidified first, carbonized with graphite powder at high temperature, and then ground into powdered sample for detection. The processing process is complicated and brings in a certain amount of impurities, resulting in many uncertainties in the test results. Second, the detection method lacks the detection of multiple added elements, such as the detection of vanadium and aluminum in titanium alloy TC4.

[0004] SN / T 3910-2014 "Determination of manganese, chromium, nickel, aluminum, molybdenum, tin, vanadium and copper in sponge titanium, titanium and titanium alloys - Inductively coupled plasma emission spectrometry" can simultaneously measure eight elements such as manganese, chromium and nickel in titanium alloys. Although it can improve the detection efficiency to a certain extent compared with the GB / T4698 series, some elements that are difficult to detect, such as silicon and boron, are not included in the detection range of the method. Although the standard YS / T 1262-2018 "Determination of multi-element content of sponge titanium, titanium and titanium alloys - Inductively coupled plasma atomic emission spectrometry" can simultaneously measure multiple elements, it cannot determine neodymium in titanium alloys. In addition, the sample pretreatment in this standard is dissolved in an open beaker, and the dissolution temperature should not exceed 70°C, which is difficult to control. In addition, in an open beaker, hydrochloric acid and hydrofluoric acid react violently with the titanium alloy sample after being added, and the solution temperature will rise rapidly, which can easily lead to silicon loss.

[0005] At present, foreign countries with more advanced titanium industry technology generally use ICP-AES method to detect impurity metal elements in sponge titanium. However, except for the standard methods of photometry and atomic spectroscopy absorption, no standard methods and patents for ICP-AES method for measuring 19 elements such as silicon, boron, zirconium, yttrium, niobium, tantalum, ruthenium, neodymium, tungsten, etc. in sponge titanium and titanium alloys have been found in relevant countries, so the detailed operation process is not very clear. ASTM E2994-16 published by the United States uses Spark Atomic Emission Spectrometry (Spark-AES) and Glow Discharge Atomic Emission Spectrometry (GD-AES) to analyze 11 elements in titanium and titanium alloys, but does not involve elements such as niobium, tantalum, boron, and tungsten. The ASTM E2371-21 standard provides a method for determining 19 elements in titanium and titanium alloys using ICP-AES or DCP-AES. This standard uses hydrochloric acid + hydrofluoric acid + nitric acid mixed acid dissolution, pure titanium as the matrix, and provides reference analysis lines, linear ranges, and the average and precision of several laboratory tests for each element. However, this method cannot detect neodymium (Nd) because F- and Nd 3+ The formation of NdF3 which is insoluble in HCl and HNO3 causes the Nd detection result to be low. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for accurately and quickly detecting 19 kinds of medium and trace elements in titanium sponge and titanium alloy.

[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for measuring the content of 19 elements in sponge titanium and titanium alloys by inductively coupled plasma emission spectroscopy, comprising the following steps:

[0008] a. Sample digestion: weigh 0.20g ± 0.0001g of sample, place it in a microwave digestion tank, add 15.0mL hydrochloric acid, 5.0mL hydrofluoric acid, 2.0mL nitric acid, 0.5mL perchloric acid, place the digestion tank in a microwave digestion instrument, digest according to the set conditions, and take it out and cool it to room temperature after digestion is completed;

[0009] b. Volume adjustment: The solution treated in step a was diluted to 100 mL with pure water to obtain solution 1 for measuring elements with a content of ≤1.0%; 10 mL of solution 1 was diluted to 100 mL with pure water to obtain solution 2 for measuring elements with a content of >1.0%;

[0010] c. Drawing a standard curve: prepare standard curve solutions with element content ≤1.0% and element content>1.0% respectively, and then introduce them into an inductively coupled plasma spectrometer for measurement according to the instrument detection conditions to draw a standard curve;

[0011] d. Establish the detection method: According to the instrument operation manual, reasonably select the instrument detection conditions, select the Ar420.073 line as the internal standard, and establish the instrument detection method;

[0012] e. Sample testing: Solution 1 and solution 2 obtained in step b are respectively introduced into an inductively coupled plasma spectrometer and tested according to the instrument detection conditions, and the contents of 19 elements including iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium and copper in sponge titanium and titanium alloy are determined according to the standard curve.

[0013] In the above step a, the hydrochloric acid is a 1:1 hydrochloric acid solution, the hydrofluoric acid is a 1:1 hydrofluoric acid solution, the nitric acid is a 1:1 nitric acid solution, and the perchloric acid is a perchloric acid solution with a concentration of 70%.

[0014] In the above step a, the setting conditions are: initial temperature 40°C, maintained for 5 minutes, heated to 120°C at 8°C / min, and maintained for 15 minutes.

[0015] In the above step b, a 100 mL polyethylene volumetric flask was used for volume adjustment.

[0016] In the above step c, the preparation method of the standard curve solution with an element content of ≤1.0% is as follows: take 6 portions of pure titanium (0.20 g ± 0.0001 g each), digest them according to the sample digestion process in step a, transfer them to a 100 mL polyethylene volumetric flask, add the corresponding single element standard solution of the element according to the concentration of the standard curve point, and then dilute to 100 mL with pure water to obtain a standard curve solution with an element content of ≤1.0%.

[0017] In the above step c, the preparation method of the standard curve solution with an element content of >1.0% is as follows: take 0.20g±0.0001g of pure titanium, digest it according to the sample digestion process in step a, transfer it to a 100mL polyethylene volumetric flask, dilute it to 100mL with pure water, take 10mL therefrom and add it to 6 100mL polyethylene volumetric flasks, add the corresponding single element standard solution of the element according to the concentration of the standard curve point, and then dilute it to 100mL with pure water to obtain a standard curve solution with an element content of >1.0%.

[0018] In the above steps c, d, and e, the setting conditions are: analysis power 1300 W, pump speed 1.5 mL / min, plasma flow rate 15 L / min, auxiliary gas flow rate 0.2 L / min, nebulizer flow rate 0.55 L / min, and observation distance 15 mm.

[0019] The beneficial effects of the present invention are as follows: the content of impurity elements in titanium sponge is generally low (0.01%-0.30%), while the content of each element in titanium alloy varies greatly (0.01%-47.0%). Due to the large content difference, the standard curve range is also different, so the national standards are measured separately. The inductively coupled plasma emission spectrometer used in the present invention has high sensitivity (solving the detection requirements of low-content elements), and the observation method can select a suitable observation mode according to the different contents of the elements to be measured (solving the detection requirements of high-content elements), and then optimize the method parameters such as selecting a suitable sample amount, analyzing the spectrum, and appropriately diluting the high-concentration elements (which can meet the detection of high-content elements without affecting the detection sensitivity of low-content elements) and the appropriate background correction technology to solve the simultaneous detection of 19 elements with different content ranges.

[0020] At present, silicon in titanium sponge and titanium alloy is detected by silicon molybdenum blue spectrophotometry, but there is no inductively coupled plasma emission spectrometry, because titanium alloy is generally dissolved by hydrofluoric acid, and silicon in the sample reacts with hydrofluoric acid to easily generate silicon tetrafluoride (gas, easily volatilized from the solution), resulting in silicon loss. The present invention uses low-temperature microwave digestion technology to effectively solve the loss of silicon in hydrofluoric acid solvent, and realizes the detection of silicon by inductively coupled plasma emission spectrometry.

[0021] The invention uses hydrochloric acid, hydrofluoric acid, nitric acid and perchloric acid as solvents, adopts microwave digestion technology to process samples, uses Ar420.073 line as internal standard, uses high-purity titanium (titanium ≥ 99.98%) as matrix matching, combines MSF (multi-spectrum fitting technology), adopts standard curve method for quantitative analysis, optimizes equipment parameters, eliminates the mutual influence between the matrix and each detection element in a targeted manner, and establishes a method for determining the content of 19 elements (iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium and copper) in sponge titanium and titanium alloys by inductively coupled plasma emission spectrometry. DETAILED DESCRIPTION

[0022] The technical solution of the present invention can be specifically implemented in the following manner.

[0023] The method for measuring the contents of 19 elements in titanium sponge and titanium alloy by inductively coupled plasma emission spectrometry comprises the following steps:

[0024] a. Sample digestion: weigh 0.20g ± 0.0001g of sample, place it in a microwave digestion tank, add 15.0mL hydrochloric acid, 5.0mL hydrofluoric acid, 2.0mL nitric acid, 0.5mL perchloric acid, place the digestion tank in a microwave digestion instrument, digest according to the set conditions, and take it out and cool it to room temperature after digestion is completed;

[0025] b. Volume adjustment: The solution treated in step a was diluted to 100 mL with pure water to obtain solution 1 for measuring elements with a content of ≤1.0%; 10 mL of solution 1 was diluted to 100 mL with pure water to obtain solution 2 for measuring elements with a content of >1.0%;

[0026] c. Drawing a standard curve: prepare standard curve solutions with element content ≤1.0% and element content >1.0% respectively, and then measure them using an inductively coupled plasma spectrometer to draw a standard curve;

[0027] d. Establish the detection method: According to the instrument operation manual, reasonably select the instrument detection conditions, select the Ar420.073 line as the internal standard, and establish the instrument detection method;

[0028] e. Sample testing: Solution 1 and solution 2 obtained in step b are respectively introduced into an inductively coupled plasma spectrometer and tested according to the set conditions, and the contents of 19 elements including iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium and copper in sponge titanium and titanium alloy are determined according to the standard curve.

[0029] In the above step a, the hydrochloric acid is a 1:1 hydrochloric acid solution, the hydrofluoric acid is a 1:1 hydrofluoric acid solution, the nitric acid is a 1:1 nitric acid solution, and the perchloric acid is a perchloric acid solution with a concentration of 70%.

[0030] The 1:1 solution is a solution in which the volume ratio of solute to water is 1:1.

[0031] In the above step a, the setting conditions are: initial temperature 40°C, maintained for 5 minutes, heated to 120°C at 8°C / min, and maintained for 15 minutes.

[0032] In the above step b, a 100 mL polyethylene volumetric flask was used for volume adjustment.

[0033] In the above step c, the preparation method of the standard curve solution with an element content of ≤1.0% is as follows: 6 portions of pure titanium (0.20 g ± 0.0001 g each) are taken respectively, digested according to the sample digestion process in step a, and then transferred to a 100 mL polyethylene volumetric flask, and the corresponding single element standard solution of the element is added according to the standard curve point concentration, and then the volume is adjusted to 100 mL with pure water to obtain a standard curve solution with an element content of ≤1.0%, and the standard curve point concentration is shown in Table 1.

[0034] Table 1 Standard curve point concentrations of elements with content ≤ 1.0% (μg / mL)

[0035] Standard Points Measuring elements concentration Standard point 0 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 0 Standard point 1 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 0.2 Standard point 2 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 0.5 Standard point 3 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 2.0 Standard point 4 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 8.0 Standard point 5 Fe,Si,Mn,Mo,B,Al,Sn,Cr,V,Zr,Mg,Nb,Pd,Ni,Ta,W,Nd,Ru,Cu 20.0

[0036] In the above step c, the preparation method of the standard curve solution with an element content of >1.0% is as follows: take 0.20g±0.0001g of pure titanium, digest it according to the sample digestion process in step a, transfer it to a 100mL polyethylene volumetric flask, dilute it to 100mL with pure water, take 10mL therefrom and add it to 6 100mL polyethylene volumetric flasks, add the corresponding single element standard solution of the element according to the standard curve point concentration, and then dilute it to 100mL with pure water to obtain a standard curve solution with an element content of >1.0%, and the standard curve point concentration is shown in Table 2.

[0037] Table 2 Standard curve point concentrations of elements with content > 1.0% (μg / mL)

[0038]

[0039] In the above steps c, d, and e, the setting conditions are: analysis power 1300 W, pump speed 1.5 mL / min, plasma flow rate 15 L / min, auxiliary gas flow rate 0.2 L / min, nebulizer flow rate 0.55 L / min, and observation distance 15 mm.

[0040] Preferably, in the above step d, the conditions set in the inductively coupled plasma spectrometer are as shown in Table 3.

[0041] Table 3 Measurement conditions of elements in titanium sponge and titanium alloy

[0042]

[0043]

[0044] Inductively coupled plasma emission spectrometry has the advantages of simultaneous measurement of multiple elements and high sensitivity; according to the current product standards and grades of titanium sponge (GB / T 2425-2019) and titanium alloy (GB / T 3620.1-2016), there are 19 elements in total; currently, these 19 elements in titanium sponge and titanium alloy require 18 detection methods to complete. If multiple elements in titanium alloy are to be detected simultaneously, a lot of labor costs, material costs and time costs are consumed. The method of the present invention can simultaneously detect 19 elements in titanium sponge and titanium alloy, which not only improves the detection efficiency, but also greatly saves labor and material costs.

[0045] The inductively coupled plasma emission spectrometer has two optional observation modes: vertical and horizontal (vertical observation mode: less interference, smaller matrix effect and interference, especially for organic samples; also good detection limit for complex matrices. Horizontal observation mode: high sensitivity, good detection limit for simple samples); the current national standards (GB / T 4698 series, YS / T 1262-2018) use an open beaker to dissolve the sample for measuring the above elements in titanium alloys. In an open environment, the blank is easily contaminated by foreign impurities and is uncontrollable; while the method of the present invention uses a microwave digestion tank to digest the sample in a closed environment (the first application of microwave digestion technology to the field of sponge titanium and titanium alloy detection), and the sample blank is low and controllable (according to the detection limit calculation formula: DL (detection limit) = 3 × RSD (relative standard deviation of the blank intensity of the element to be measured) × BEC (background equivalent concentration of the element to be measured), it can be seen from the above formula that the lower the sample blank, the lower its RSD and BEC, and the lower the calculated element detection limit).

[0046] It can be understood by those skilled in the art that the method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry of the present invention uses quantitative values ​​to express the numerical values ​​of each process in the claims in order to ensure the clarity and simplicity of the technical solution. On the basis of the technical solution of the present invention, those skilled in the art increase or decrease proportionally to adjust the process parameters is also equivalent to the technical solution of the present invention, and can achieve the technical effect of the present invention, which also belongs to the protection scope of the present invention.

[0047] The technical solution and effects of the present invention are further illustrated below through practical examples.

[0048] Example

[0049] Example 1

[0050] 1. Accurately weigh 0.20±0.0001g of sample;

[0051] 2. Place the sample in a microwave digestion tank, add 15.0mL hydrochloric acid (1+1), 5.0mL (1+1) hydrofluoric acid, 2.0mL (1+1) nitric acid, and 0.5mL (concentrated) perchloric acid, place the digestion tank in a microwave digestion instrument, and digest according to the following heating program: initial temperature 40°C, maintain for 5 minutes, heat to 120°C at 8°C / min, maintain for 15 minutes, then cool to room temperature, take out and transfer to a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 1). For elements with a content of ≤1.0%, use solution 1 to measure directly on the instrument; for elements with a content of >1.0%, take 10mL from solution 1 and put it into a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 2), and use high-purity titanium as a blank along with the sample;

[0052] 3. Select the analytical method for the prepared sample solution and measure it with an inductively coupled plasma spectrometer;

[0053] 4. The test results are shown in Table 4.

[0054] Table 4 Statistics of the measurement results of four titanium alloy standard samples with different contents by this inventive method / %

[0055]

[0056]

[0057] Example 2

[0058] 1. Accurately weigh 0.20±0.0001g of sample (IARM 337A) (Comparison of results from different laboratories);

[0059] 2. Place the sample in a microwave digestion tank, add 15.0mL hydrochloric acid (1+1), 5.0mL (1+1) hydrofluoric acid, 2.0mL (1+1) nitric acid, and 0.5mL (concentrated) perchloric acid, place the digestion tank in a microwave digestion instrument, and digest according to the following heating program: initial temperature 40°C, maintain for 5 minutes, heat to 120°C at 8°C / min, maintain for 15 minutes, then cool to room temperature, take out and transfer to a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 1). For elements with a content of ≤1.0%, use solution 1 to measure directly on the instrument; for elements with a content of >1.0%, take 10mL from solution 1 and put it into a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 2), and use high-purity titanium as a blank along with the sample;

[0060] 3. Select the analytical method for the prepared sample solution and measure it with an inductively coupled plasma spectrometer;

[0061] 4. The test results are shown in Table 5:

[0062] Table 5 Statistics of comparison of measurement results in different laboratories / %

[0063]

[0064]

[0065] Example 3

[0066] 1. Accurately weigh 0.20±0.0001g of sample (IARM 269B and IARM 300B) (comparison of different detection methods);

[0067] 2. Place the sample in a microwave digestion tank, add 15.0mL hydrochloric acid (1+1), 5.0mL (1+1) hydrofluoric acid, 2.0mL (1+1) nitric acid, and 0.5mL (concentrated) perchloric acid, place the digestion tank in a microwave digestion instrument, and digest according to the following heating program: initial temperature 40°C, maintain for 5 minutes, heat to 120°C at 8°C / min, maintain for 15 minutes, then cool to room temperature, take out and transfer to a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 1). For elements with a content of ≤1.0%, use solution 1 to measure directly on the instrument; for elements with a content of >1.0%, take 10mL from solution 1 and put it into a 100mL polyethylene dissolving bottle, dilute to volume with pure water and mix well for use (solution 2), and use high-purity titanium as a blank along with the sample;

[0068] 3. Select the analytical method for the prepared sample solution and measure it with an inductively coupled plasma spectrometer;

[0069] 4. The test results are shown in Table 6:

[0070] Table 6 Comparison of different detection methods

[0071]

Claims

1. A method for measuring the content of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry, characterized in that The steps include: a. Sample digestion: weigh 0.20g ± 0.0001g sample, place it in a microwave digestion tank, add 15.0mL hydrochloric acid, 5.0mL hydrofluoric acid, 2.0mL nitric acid, 0.5mL perchloric acid, place the digestion tank in a microwave digestion instrument, digest according to the set conditions, and take it out and cool it to room temperature after digestion is completed; b. Volume adjustment: The solution treated in step a was diluted to 100 mL with pure water to obtain solution 1 for measuring elements with a content of ≤1.0%; 10 mL of solution 1 was diluted to 100 mL with pure water to obtain solution 2 for measuring elements with a content of >1.0%; c. Drawing a standard curve: prepare standard curve solutions with element content ≤1.0% and element content>1.0% respectively, and then introduce them into an inductively coupled plasma spectrometer for measurement according to the instrument detection conditions to draw a standard curve; d. Establish the detection method: According to the instrument operation manual, reasonably select the instrument detection conditions, select the Ar420.073 line as the internal standard, and establish the instrument detection method; e. Sample testing: Solution 1 and solution 2 obtained in step b are respectively introduced into an inductively coupled plasma spectrometer for testing according to the instrument detection conditions, and the contents of 19 elements including iron, silicon, manganese, molybdenum, boron, aluminum, tin, chromium, vanadium, zirconium, magnesium, niobium, palladium, nickel, tantalum, tungsten, neodymium, ruthenium and copper in sponge titanium and titanium alloy are determined according to the standard curve; In step a, the hydrochloric acid is a 1:1 hydrochloric acid solution, the hydrofluoric acid is a 1:1 hydrofluoric acid solution, the nitric acid is a 1:1 nitric acid solution, and the perchloric acid is a 70% perchloric acid solution; In step a, the setting conditions are: initial temperature 40°C, maintained for 5 minutes, heated to 120°C at 8°C / min, and maintained for 15 minutes.

2. The method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry according to claim 1, characterized in that: In step b, a 100 mL polyethylene volumetric flask was used to make up the volume.

3. The method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry according to claim 1, characterized in that: In step c, the preparation method of the standard curve solution with an element content of ≤1.0% is as follows: take 6 portions of 0.20g±0.0001g of pure titanium respectively, digest them according to the sample digestion process in step a, transfer them to a 100mL polyethylene volumetric flask, add the corresponding single element standard solution of the element according to the concentration of the standard curve point, and then dilute to 100mL with pure water to obtain a standard curve solution with an element content of ≤1.0%.

4. The method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry according to claim 1, characterized in that: In step c, the preparation method of the standard curve solution with an element content of >1.0% is as follows: take 0.20g±0.0001g of pure titanium, digest it according to the sample digestion process in step a, transfer it to a 100mL polyethylene volumetric flask, dilute it to 100mL with pure water, take 10mL therefrom and add it to 6 100mL polyethylene volumetric flasks, add the corresponding single element standard solution of the element according to the concentration of the standard curve point, and then dilute it to 100mL with pure water to obtain a standard curve solution with an element content of >1.0%.

5. The method for measuring the contents of 19 elements in titanium sponge and titanium alloys by inductively coupled plasma emission spectrometry according to claim 1, characterized in that: In steps c, d, and e, the instrument detection conditions are: analysis power 1300 W, pump speed 1.5 mL / min, plasma flow rate 15 L / min, auxiliary gas flow rate 0.2 L / min, nebulizer flow rate 0.55 L / min, and observation distance 15 mm.

Citation Information

Cited By

  • Method for determining element content in titanium alloy by inductively coupled plasma emission spectrometry

    CN121275724A