A multi-metal catalyst for the synthesis of polyetheramines and a preparation method thereof

By adjusting the pore size of multi-metal catalysts and carriers, the polyetheramine synthesis process is optimized, which solves the problems of insufficient activity and conversion rate of existing catalysts and achieves high-efficiency, low-energy consumption and environmentally friendly polyetheramine synthesis effects.

CN115608374BActive Publication Date: 2024-10-29FUJIAN YUECHUN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210923977.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-02
Publication Date
2024-10-29
Estimated Expiration
2042-08-02

AI Technical Summary

Technical Problem

Existing polyetheramine synthesis catalysts have deficiencies in catalytic activity, selectivity and conversion rate, and the process consumes high energy, causing environmental hazards and high costs.

Method used

Multi-metal catalysts are used, including carriers, first metals (such as Ni, Cu, Co, etc.) and noble metals (such as Pt, Rh, etc.), to improve catalytic activity and selectivity through different sizes and electronic effects, and to adjust the pore size and The calcination step was optimized to produce a catalyst with high conversion and selectivity.

Benefits of technology

It significantly improves the conversion rate and selectivity of the polyetheramine synthesis reaction, reduces process energy consumption, reduces pollution, controls production costs, and achieves efficient catalytic effects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the field of synthesis technology, and specifically to a multi-metal catalyst for the synthesis of polyetheramines and a preparation method thereof; the present invention utilizes different effects after the combination of multiple metals in the catalyst, such as size effect, electronic effect, lattice strain effect, structural effect, etc., and further significantly improves the catalytic activity, selectivity and stability of the catalyst through the use of a carrier and the limitation of its pore size, thereby promoting the synthesis reaction of polyetheramines; the conversion rate and selectivity of the catalyst for the reaction in the synthesis process are further improved in combination with the setting of process parameters, the preparation process is simple, energy consumption is low, pollution is low, the conversion rate of polyetheramines is high, and the selectivity of primary amines in the product is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of synthesis technology, C08G65 / 48, and specifically to a multi-metal catalyst for the synthesis of polyetheramines and a preparation method thereof. Background Art

[0002] Polyetheramine, also known as amino-terminated polyether, is a class of polyoxyalkylene compounds whose main molecular chain is polyether and whose terminal is capped by amino group (generally containing polyamino group, primary amino group, secondary amino group). At present, the main synthesis methods of polyetheramine include leaving group method, polyether nitrile alkylation method, aminobutyric acid ester method, catalytic reduction amination method, etc. The catalytic reduction amination method has advanced technology, few side reactions, and meets environmental protection requirements. It has become the focus of research by scientific and technological workers at home and abroad; in this method, polyether polyol is mostly used as the reaction raw material, dehydrogenated under the catalyst, and reacted with ammonia through different treatment methods to convert the terminal hydroxyl group of polyether polyol into the corresponding amino group or amine group. Because the amino group or amine group at the end of the polyether skeleton can react with a variety of reactive groups, and because the presence of ether bonds in the polyether chain makes it soluble in a variety of organic substances, polyetheramine is widely used in the industrial field. However, the difficulty and key to the synthesis process of polyetheramine lies in the selection and preparation of catalysts. The catalytic activity, selectivity and conversion rate of existing polyetheramine synthesis catalysts still have a lot of room for improvement.

[0003] CN101982482A discloses a method for preparing polyetheramine using an amorphous alloy catalyst. A large amount of strong alkaline solution is required in the preparation process of the catalyst, which has certain environmental risks, and the conversion rate of the catalyst to polyetheramine is still not high.

[0004] CN108014821B discloses a catalyst for synthesizing polyetheramines, a preparation method and application thereof, wherein the active component NiO of the catalyst contains 5-10wt%, Au2O3 contains 0.5-1.5wt%, and SeO2 contains 0.1-0.5wt%. However, the preparation process of the catalyst requires a relatively high temperature, even up to 1500°C, and the process energy consumption is relatively high. Summary of the invention

[0005] The present invention aims to improve the deficiencies of the prior art and provides a multi-metal catalyst for the synthesis of polyetheramines and a preparation method thereof.

[0006] Firstly, the present invention provides a multi-metal catalyst for the synthesis of polyetheramines, wherein the multi-metal catalyst comprises a carrier, a first metal and a second metal.

[0007] Furthermore, the first metal is one or more of Ni, Cu, Co, Fe, Zn, Ba, Ca, Mn, Al, Mo, Ti, Cr, and lanthanide metals.

[0008] Furthermore, the second metal is a noble metal, and the addition of the noble metal can improve the selectivity and conversion rate of the polyetheramine synthesis reaction.

[0009] The atomic radius of the first metal in the multi-metal catalyst is relatively small, while the atomic radius of the second metal is relatively large. Metals of different sizes promote each other's dispersion. Under the size effect, the active sites of the multi-metal catalyst are more exposed; the incorporation of lattices between different metals will enhance their electronic and structural effects, and may also improve the stability of the catalyst during subsequent calcination; therefore, multi-metal catalysts promote the reaction of polyether polyols with liquid ammonia due to the many effects they have (such as size effect, electronic effect, lattice strain effect, structural effect, etc.), thereby improving the conversion rate and selectivity of the polyetheramine synthesis reaction.

[0010] Furthermore, in terms of the mass percentage of the multi-metal catalyst, the first metal content in the multi-metal catalyst is 20-45%, and the second metal content is 0.1%-0.8%.

[0011] The first metal has good rapid adsorption and activation properties for H, but the similarity in radius and electronic structure may cause the first metal to shield some active sites during preparation. The second metal is added to improve the dispersibility, catalytic activity and stability of the metal catalyst through different effects. However, when the second metal is added in excessive amounts, the structural stability of the catalyst will be reduced. In addition, the second metal is a precious metal and is relatively expensive. Large-scale use will also greatly increase the production cost. In order to obtain a better catalytic effect of the multi-metal catalyst while ensuring a certain cost, the content of the first metal and the second metal in the multi-metal catalyst needs to be controlled.

[0012] Furthermore, the carrier is one of silicon compounds, metal oxides, porous carbon materials, glass fibers, hollow ceramic balls, and diatomaceous earth.

[0013] The above carriers have a large number of voids and a large specific surface area, which can provide crystal growth sites for the first metal and the second metal and better disperse the multiple metals; in addition, the huge specific surface area of ​​these carriers can also adsorb polyether polyols and liquid ammonia during the synthesis of polyetheramines, accelerating the catalytic reaction.

[0014] Furthermore, the carrier is one of silicon carbide, silicon oxide, metal oxide, activated carbon, graphene, glass fiber, hollow ceramic ball, and diatomaceous earth.

[0015] Furthermore, the carrier is a metal oxide.

[0016] Furthermore, the metal oxide is Al2O3, TiO2, O 13 One or more of V6.

[0017] Furthermore, Al2O3 in the metal oxide is β-Al2O3 or γ-Al2O3.

[0018] Furthermore, the pore size of the metal oxide is 65-120 angstroms. By limiting the pore size of the carrier metal oxide, the adsorption and diffusion degree of the carrier on the first metal precursor and the first metal precursor therein can be adjusted. Moreover, the pore size will also affect the adsorption and diffusion of the polyether amine synthesis raw material polyether polyol and liquid ammonia on the carrier surface, thereby affecting the catalytic effect of the catalyst on the synthesis of polyether amine; when the pore size is too small, the first metal and the second metal will have overlapping growth on the carrier surface, causing some active sites to be shielded, and in the subsequent synthesis reaction, there is not much space for the reactants to diffuse to its surface, the synthesis reaction speed is greatly reduced, and the conversion rate is also reduced.

[0019] In a preferred embodiment, when the pore size of the metal oxide is 100 angstroms, the prepared multi-metal catalyst exhibits the best conversion rate for the synthesis reaction of polyetheramines; and when the pore size of the metal oxide is 160 angstroms, the conversion rate of this catalyst for polyetheramines is significantly reduced. It is speculated that: when the pore size is too large, the dispersion of the growth of the first metal and the second metal on the carrier surface is too strong, and the lattice effect and structural effect produced by the mutual influence between them will also be reduced.

[0020] Secondly, the present invention provides a method for preparing a multi-metal catalyst for the synthesis of polyetheramines, the steps being as follows:

[0021] S1. Mix the solution of the first metal precursor with the carrier, impregnate it, and then calcine it to obtain an intermediate 1.

[0022] S2. The intermediate 1 is mixed with a solution of a second metal precursor, impregnated, and then calcined to obtain an intermediate 2.

[0023] S3. Reducing the intermediate 2 gives a multimetal catalyst.

[0024] Furthermore, in step S1, the volume ratio of the first metal precursor solution to the carrier is 2:1-1:2.

[0025] The carrier skeleton supports the lattice growth of the multi-metal catalyst, disperses and increases its active sites, increases the strength of the multi-metal catalyst, and further improves the catalytic ability and stability of the catalyst. However, when the amount is too much, the dispersion of the first metal and the second metal on the carrier surface is too strong, which will reduce the lattice effect and structural effect between them.

[0026] Preferably, in step S1, the volume ratio of the first metal precursor solution to the carrier is 1:1.

[0027] Furthermore, the metal cation in the first metal precursor is Ni 2+ , Cu 2+ 、Co 2+ , Fe 3+ 、Zn 2+ , Ba 2+ , Ca 2+ , Mn 2+ 、Al 3+ 、Mo 2+ 、Ti 4+ Cr 3+ , one or more of the lanthanide metal cations.

[0028] Furthermore, the first metal precursor is one or more of Ni(NO3)2, NiCl2, Cu(NO3)2, CuCl2, Co(NO3)2, CoCl2, Fe(NO3)3, FeCl3, Zn(NO3)2, ZnCl2, Ba(NO3)2, BaCl2, Ca(NO3)2, CaCl2, Mn(NO3)2, MnCl2, Al(NO3)2, Mo(NO3)2, Ti(NO3)4, La(NO3)3, La(NO3)3, Ce(NO3)3, CeCl3, Cr(NO3)3, and CrCl3.

[0029] Furthermore, the first metal precursor is one or more of Ni(NO3)2, Cu(NO3)2, Co(NO3)2, Fe(NO3)3, Zn(NO3)2, Ba(NO3)2, Ca(NO3)2, Mn(NO3)2, Mo(NO3)2, Ti(NO3)4, La(NO3)3, La(NO3)3, Ce(NO3)3, and Cr(NO3)3.

[0030] Furthermore, the dipping process in step S1 is performed 2 or 3 times.

[0031] Preferably, the dipping process in step S1 is performed twice.

[0032] Furthermore, in step S1, the calcination temperature is 350-600° C., and the calcination time is 5-12 hours.

[0033] Preferably, in step S1, the calcination temperature is 450° C. and the calcination time is 8 hours.

[0034] Furthermore, in step S2, the second metal precursor is any one or more of AgNO3, Rh(NO3)2, Pt(NO3)2, PtCl2, Pd(NO3)2, PdCl2, Ru(NO3)3, and RuCl3.

[0035] Furthermore, in step S2, the second metal precursor is any one or more of AgNO3, Rh(NO3)2, Pt(NO3)2, Pd(NO3)2, and Ru(NO3)3.

[0036] Furthermore, in step S2, the calcination temperature is 400-550° C., and the calcination time is 8-12 hours.

[0037] Preferably, in step S2, the calcination temperature is 450° C. and the calcination time is 10 h.

[0038] Furthermore, in step S3, the reduction temperature is 200-500° C., and the reducing substance is H 2 .

[0039] Preferably, the reduction temperature in step S3 is 400°C.

[0040] The multi-metal catalyst provided by the present invention exhibits excellent conversion rate and selectivity for the synthesis reaction of polyetheramine, and the synthesis steps are as follows:

[0041] (1) In a hydrogen environment, the polyether polyol raw material and liquid ammonia are fully mixed in proportion.

[0042] (2) The mixed material contacts the catalyst to undergo a catalytic amination reaction, the reactants are separated into gas and liquid, and the raw ammonia is recovered and then post-processed.

[0043] In the step (1), the mass ratio of the polyether polyol raw material to the liquid ammonia is (1-8):1, and in the step (2), the reaction temperature is 160-250° C. and the reaction pressure is 4-15 MPa.

[0044] Beneficial effects:

[0045] The present invention utilizes different effects after the combination of multiple metals in the catalyst, such as size effect, electronic effect, lattice strain effect, structural effect, etc., and further significantly improves the catalytic activity, selectivity and stability of the catalyst by using a carrier and limiting its pore size, thereby promoting the synthesis reaction of polyetheramine; combined with the setting of process parameters, the conversion rate and selectivity of the catalyst to the reaction in the synthesis process are further improved, the preparation process is simple, energy consumption is low, pollution is low, the conversion rate of polyetheramine is high, and the selectivity of primary amines in the product is high. DETAILED DESCRIPTION

[0046] Example

[0047] Example 1

[0048] A multi-metal catalyst for synthesizing polyetheramine comprises a carrier, a first metal and a second metal.

[0049] According to the mass percentage of the multi-metal catalyst, the first metal is Ni 21.7% and Cu 12.8%, the second metal is Pt 0.18%, and the carrier is γ-Al2O3 with a pore size of 120 angstroms and a pore volume of 0.8 cm 3 / g.

[0050] The preparation method of the multi-metal catalyst is as follows:

[0051] Preparation of the first metal precursor solution: weigh 190 g Ni(NO3)2·6H2O and 95 g Cu(NO3)2·6H2O and add them into 500 mL deionized water to dissolve.

[0052] Preparation of the second metal precursor solution: Weigh 5 g of Pt(NO3)2, add 300 mL of deionized water to dissolve, and set aside.

[0053] S1. Mix the solution of the first metal precursor with the carrier, impregnate it, and then calcine it to obtain an intermediate 1:

[0054] Take 250g of γ-Al2O3 carrier and dry it at 110℃ for 10h, add the solution of the first metal precursor dropwise into the carrier for the first impregnation, dry the carrier at 110℃ for 12h after the impregnation, perform the second and third impregnations in the same way as the previous operation, dry the carrier at 110℃ for 12h and then calcine at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the solution of the first metal precursor to the carrier during the impregnation process is 1:1.

[0055] S2. Mix the intermediate 1 and the solution of the second metal precursor, impregnate, and then calcine to obtain the intermediate 2:

[0056] 100 mL of the second metal precursor solution was slowly added dropwise to the intermediate 1 for impregnation, and then dried at 110° C. for 12 h and calcined at 450° C. for 10 h to obtain the intermediate 2.

[0057] S3. Reducing the intermediate 2 to obtain a multimetal catalyst:

[0058] 100 mL of intermediate 2 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 400°C.

[0059] Example 2

[0060] A multi-metal catalyst for synthesizing polyetheramine comprises a carrier, a first metal and a second metal.

[0061] According to the mass percentage of the multi-metal catalyst, the first metal is Ni 11%, Cu 5.1%, Cr 5.9%, the second metal is Pt 0.8%, and the carrier is γ-Al2O3 with a pore size of 65 angstroms and a pore volume of 0.7 cm 3 / g.

[0062] The preparation method of the multi-metal catalyst is as follows:

[0063] Preparation of the first metal precursor solution: weigh 100 g Ni(NO3)2·6H2O, 45 g Cu(NO3)2·6H2O, and 50 g Cr(NO3)3·9H2O and add them into 500 mL deionized water to dissolve.

[0064] Preparation of the second metal precursor solution: Weigh 20 g of Pt(NO3)2, add 300 mL of deionized water to dissolve, and set aside.

[0065] S1. Mix the solution of the first metal precursor with the carrier, impregnate it, and then calcine it to obtain an intermediate 1:

[0066] Take 250g of γ-Al2O3 carrier and dry it at 110℃ for 10h, add the solution of the first metal precursor dropwise into the carrier for the first impregnation, dry the carrier at 110℃ for 12h after the impregnation, perform the second impregnation according to the same operation as the previous time, dry the carrier at 110℃ for 12h and then calcine at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the solution of the first metal precursor to the carrier during the impregnation process is 1:1.

[0067] S2. Mix the intermediate 1 and the solution of the second metal precursor, impregnate, and then calcine to obtain the intermediate 2:

[0068] 100 mL of the second metal precursor solution was slowly dripped into the intermediate 1 for impregnation, and then dried at 110° C. for 12 h and calcined at 350° C. for 12 h to obtain the intermediate 2.

[0069] S3. Reducing the intermediate 2 to obtain a multimetal catalyst:

[0070] 100 mL of intermediate 2 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 300°C.

[0071] Example 3

[0072] A multi-metal catalyst for synthesizing polyetheramine comprises a carrier, a first metal and a second metal.

[0073] According to the mass percentage of the multi-metal catalyst, the first metal is Ni 20.8%, Cu 12.9%, Cr 2.2%, the second metal is Pt 0.18%, and the carrier is γ-Al2O3 with a pore size of 100 angstroms and a pore volume of 0.8 cm 3 / g.

[0074] The preparation method of the multi-metal catalyst is as follows:

[0075] Preparation of the first metal precursor solution: weigh 190 g Ni(NO3)2·6H2O, 95 g Cu(NO3)2·6H2O, and 20 g Cr(NO3)3·9H2O and add them into 50 mL deionized water to dissolve.

[0076] Preparation of the second metal precursor solution: Weigh 5 g of Pt(NO3)2, add 300 mL of deionized water to dissolve, and set aside.

[0077] S1. The solution of the first metal precursor is mixed with the carrier, impregnated and then calcined to obtain intermediate 1: 250g of γ-Al2O3 carrier is dried at 110℃ for 10h, the solution of the first metal precursor is added dropwise to the carrier for the first impregnation, after the impregnation is completed, the carrier is dried at 110℃ for 12h, and the second impregnation is performed according to the same operation as the previous time. The carrier is dried at 110℃ for 12h and then calcined at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the first metal precursor solution to the carrier during the impregnation process is 1:1.

[0078] S2. Mix the intermediate 1 and the solution of the second metal precursor, impregnate, and then calcine to obtain the intermediate 2:

[0079] 100 mL of the second metal precursor solution was slowly added dropwise to the intermediate 1 for impregnation, and then dried at 110° C. for 12 h and calcined at 450° C. for 10 h to obtain the intermediate 2.

[0080] S3. Reducing the intermediate 2 to obtain a multimetal catalyst:

[0081] 100 mL of intermediate 2 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 400°C.

[0082] Comparative Example 1

[0083] A multi-metal catalyst for synthesizing polyetheramine comprises a carrier, a first metal and a second metal.

[0084] According to the mass percentage of the multi-metal catalyst, the first metal is Cu 17.1%, the second metal is Pt 0.17%, and the carrier is γ-Al2O3 with a pore size of 100 angstroms and a pore volume of 0.8 cm 3 / g.

[0085] The preparation method of the multi-metal catalyst is as follows:

[0086] Preparation of the first metal precursor solution: Weigh 95 g of Cu(NO3)2·6H2O and add it into 500 mL of deionized water to dissolve.

[0087] Preparation of the second metal precursor solution: Weigh 5 g of Pt(NO3)2, add 300 mL of deionized water to dissolve, and set aside.

[0088] S1. The first metal precursor is mixed with the carrier, impregnated and then calcined to obtain an intermediate 1:

[0089] Take 250g of γ-Al2O3 carrier and dry it at 110℃ for 10h, add the solution of the first metal precursor dropwise into the carrier for the first impregnation, dry the carrier at 110℃ for 12h after the impregnation, perform the second impregnation according to the same operation as the previous time, dry the carrier at 110℃ for 12h and then calcine at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the solution of the first metal precursor to the carrier during the impregnation process is 1:1.

[0090] S2. Mix the intermediate 1 and the solution of the second metal precursor, impregnate, and then calcine to obtain the intermediate 2:

[0091] 100 mL of the second metal precursor solution was slowly added dropwise to the intermediate 1 for impregnation, and then dried at 110° C. for 12 h and calcined at 450° C. for 10 h to obtain the intermediate 2.

[0092] S3. Reducing the intermediate 2 to obtain a multimetal catalyst:

[0093] 100 mL of intermediate 2 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 400°C.

[0094] Comparative Example 2

[0095] A multi-metal catalyst for synthesizing polyetheramines comprises a carrier and a first metal.

[0096] According to the mass percentage of the multi-metal catalyst, the first metal is Ni 20.1%, Cu 13.2%, and the carrier is γ-Al2O3, with a pore size of 100 angstroms and a pore volume of 0.8 cm 3 / g.

[0097] The preparation method of the multi-metal catalyst is as follows:

[0098] Preparation of the first metal precursor solution: weigh 190 g Ni(NO3)2·6H2O and 95 g Cu(NO3)2·6H2O and add them into 500 mL deionized water to dissolve.

[0099] S1. Mix the solution of the first metal precursor with the carrier, impregnate it, and then calcine it to obtain an intermediate 1:

[0100] Take 250g of γ-Al2O3 carrier and dry it at 110℃ for 10h, add the first metal precursor dropwise into the carrier for the first impregnation, dry the carrier at 110℃ for 12h after impregnation, perform the second impregnation according to the same operation as the previous time, dry the carrier at 110℃ for 12h and then calcine at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the solution of the first metal precursor to the carrier during the impregnation process is 1:1.

[0101] S2. Reduction of intermediate 1 to obtain a multimetallic catalyst:

[0102] 100 mL of intermediate 1 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 400°C.

[0103] Comparative Example 3

[0104] A multi-metal catalyst for synthesizing polyetheramine comprises a carrier, a first metal and a second metal.

[0105] According to the mass percentage of the multi-metal catalyst, the first metal is Ni 19.8%, Cu 12.5%, Cr 3.4%, the second metal is Pt 0.15%, and the carrier is γ-Al2O3 with a pore size of 160 angstroms and a pore volume of 0.9 cm 3 / g.

[0106] The preparation method of the multi-metal catalyst is as follows:

[0107] Preparation of the first metal precursor solution: weigh 190 g Ni(NO3)2·6H2O, 95 g Cu(NO3)2·6H2O, and 20 g Cr(NO3)3·9H2O and add them into 500 mL deionized water to dissolve.

[0108] Preparation of the second metal precursor solution: Weigh 5 g of Pt(NO3)2, add 300 mL of deionized water to dissolve, and set aside.

[0109] S1. The first metal precursor is mixed with the carrier, impregnated and then calcined to obtain an intermediate 1:

[0110] Take 750g of γ-Al2O3 carrier and dry it at 110℃ for 10h, add the solution of the first metal precursor dropwise into the carrier for the first impregnation, dry the carrier at 110℃ for 12h after the impregnation, perform the second impregnation according to the same operation as the previous time, dry the carrier at 110℃ for 12h and then calcine at 450℃ for 8h to obtain intermediate 1; wherein the volume ratio of the solution of the first metal precursor to the carrier during the impregnation process is 3:1.

[0111] S2. Mix the intermediate 1 and the solution of the second metal precursor, impregnate, and then calcine to obtain the intermediate 2:

[0112] 100 mL of the second metal precursor solution was slowly added dropwise to the intermediate 1 for impregnation, and then dried at 110° C. for 12 h and calcined at 450° C. for 10 h to obtain the intermediate 2.

[0113] S3. Reducing the intermediate 2 to obtain a multimetal catalyst:

[0114] 100 mL of intermediate 2 was placed in a reactor and hydrogen (pressure 2 bar, flow rate 100 L / h) was introduced for reduction for 12 h at a reduction temperature of 400°C.

[0115] For the multi-metal catalysts prepared in the above examples, the types and contents of metals therein were detected by inductively coupled plasma emission spectrometry.

[0116] The Ni(NO3)2·6H2O was purchased from Shandong Desheng New Materials Co., Ltd. with a purity of 98%; the Cu(NO3)2·6H2O was purchased from Shanghai Chengxin Industrial Co., Ltd. with a purity of 99%; the Cr(NO3)3·9H2O was purchased from Shanxi Xinyufeng Technology Co., Ltd.; Mn(NO3)2 and Pt(NO3)2 were both purchased from Shanghai Yien Chemical Technology Co., Ltd. with item numbers R000531 and R054754 respectively; and γ-Al2O3 was purchased from Benyu Metal Materials Co., Ltd.

[0117] Performance testing method:

[0118] The multi-metal catalyst prepared in the above examples is used for the synthesis reaction of polyetheramine in a fixed bed continuous process, and the steps are as follows:

[0119] (1) Under a hydrogen environment, a polyether polyol raw material (weight average molecular weight of 2000, purchased from Dow Chemical, catalog number 001) and liquid ammonia were fully mixed at a mass ratio of 2:1, and the flow rates of the polyether polyol and liquid ammonia into the reactor were 100 g / h and 50 g / h, respectively.

[0120] (2) The mixed material is contacted with the catalyst to undergo a catalytic amination reaction at a reaction temperature of 200° C. and a reaction pressure of 60 kg. The reactants are separated into gas and liquid, and the raw ammonia is recovered and then post-processed.

[0121] Gas chromatography was used to analyze the composition and content of the polyetheramine synthesis reaction products and to determine the reaction conversion rate and selectivity.

[0122] Performance test results:

[0123] Table 1

[0124] Sample No. Reaction conversion rate Purity of primary amine in the reaction product Example 1 99.5% 99.9% Example 2 98.2% 99.6% Example 3 99.9% 99.8% Comparative Example 1 48.2% 99.9% Comparative Example 2 92.8% 95.8% Comparative Example 3 78.2% 98.1%

Claims

1. Application of a multi-metal catalyst in the synthesis of polyetheramines in a fixed bed continuous process, It is characterized in that Here are the steps: (1) In a hydrogen environment, the polyether polyol raw material and liquid ammonia are fully mixed at a mass ratio of 2:1, and the flow rates of the polyether polyol and liquid ammonia into the reactor are 100 g / h and 50 g / h respectively; (2) The mixed material is contacted with the catalyst to undergo a catalytic amination reaction at a reaction temperature of 200°C and a reaction pressure of 60 kg. The reactants are separated into gas and liquid, and the raw ammonia is recovered and then post-processed; The polyether polyol raw material has a weight average molecular weight of 2000 and is purchased from Dow Chemical, item number 001; The multi-metal catalyst comprises a carrier, a first metal and a second metal; In terms of the mass percentage of the multi-metal catalyst, the first metal is Ni 20.8%, Cu 12.9%, Cr 2.2%, the second metal is Pt 0.18%, and the carrier is γ-Al 2 O 3 , with a pore size of 100 angstroms and a pore volume of 0.8 cm 3 / g; The preparation method of the multi-metal catalyst for the synthesis of polyetheramines comprises the following steps: S1. The solution of the first metal precursor is mixed with the support and then impregnated and calcined to obtain an intermediate 1; S2. The intermediate 1 is mixed with a solution of a second metal precursor and then impregnated and calcined to obtain an intermediate 2; S3. Reducing the intermediate 2 to obtain a multimetal catalyst; In step S1, the volume ratio of the first metal precursor to the carrier is 2:1-1:2; The dipping process in step S1 is 2 or 3 times; In step S1, the calcination temperature is 350-600° C. and the calcination time is 5-12 hours.

2. Use of a multi-metal catalyst according to claim 1 in the synthesis of polyetheramines in a fixed bed continuous process, Features The reduction temperature in step S3 is 200-500°C.

Citation Information

Patent Citations

  • Method for preparing polyether amine by adopting amorphous alloy catalyst

    CN101982482A

  • A catalyst for the synthesis of polyetheramines, its preparation method and application

    CN108014821B

  • Catalyst applied to amination of polyether polyol, preparation method thereof and method for preparing polyether amine by using catalyst

    CN106669731A

  • Preparation method of coupled nano composite noble metal catalyst of activated alumina carrier