A method for preparing bismuth oxide thin film and reconfigurable photoelectric logic gate
Through the non-monotonic photovoltage characteristics of the bismuth oxide film, the reconfigurability of the photoelectric logic gate is realized, which solves the problem that the photoelectric logic gate device cannot realize the XOR gate operation, reduces the processing accuracy requirements and production costs, and is suitable for future data Handle complex needs.
Patent Information
- Application Number
- CN202211124468.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-15
Smart Images

Figure CN115612995B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of integrated circuits and processors, and in particular to a method for preparing a bismuth oxide thin film and a reconfigurable photoelectric logic gate based on the non-monotonic change of the bismuth oxide open-circuit photovoltage with light intensity. Background Art
[0002] Traditional complementary metal oxide semiconductor (CMOS) logic computing devices have followed Moore's Law in the past few decades, continuously reducing the size to increase the number of transistors to meet the increasing demand for data processing. It is expected that in the era of the Fourth Industrial Revolution and the Internet of Things, the amount of data will explode and even exceed the scope allowed by Moore's Law. Traditional CMOS logic computing devices will face serious limitations in calculating massive data sets. Compared with reducing device size and three-dimensional integration, the development of new reconfigurable logic gates is a very promising direction.
[0003] Photoelectric logic gates can be used for accurate and fast data processing and have attracted widespread attention. In particular, reconfigurable photoelectric logic gates can be programmed to flexibly switch between different logic gates on a single device, enabling more complex data operations and calculations with fewer components. Currently, reconfigurable photoelectric logic gates that can switch between basic logic gates such as AND gates, OR gates, and NOT gates have been reported. However, reconfigurable photoelectric logic gates that can achieve XOR operations are rarely reported.
[0004] XOR logic gates are not only an important part of data processing functions such as bit pattern recognition, data encryption, parity check and signal regeneration, but also a basic tool for synchronization, erasure and replacement in packet switching networks. The difficulty in realizing the operation of photoelectric XOR gates lies in that it takes into account both the output of 0 when the input is (0,0) and the output of 1 when the input is (1,0), but it is difficult to take into account the output of 0 when the input is (1,1), which is essentially a non-monotonic change. The output of current photoelectric logic gate devices changes monotonically with the input light intensity, so XOR gate operations cannot be realized. In some reports, XOR gate operations are realized using photocurrents in different directions, but it is necessary to judge the output result by judging the absolute value of the photocurrent, which increases the complexity of logical judgment. In addition, under a certain light intensity, the photocurrent increases with the increase of device size, so the logic gate based on the photocurrent signal has very high requirements for device processing accuracy. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art, provide a bismuth oxide thin film preparation method and a reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity, and design and manufacture a reconfigurable photoelectric logic gate by using the unique characteristics of bismuth oxide. By adjusting the input light intensity, without changing the threshold conditions, a single device can be used to realize programmable reconstruction of multiple logic gates such as XOR gate, AND gate, NAND gate, OR gate, NOR gate, NOT gate, and inhibit gate.
[0006] To achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, the present invention provides a method for preparing a bismuth oxide thin film, the method comprising the following steps:
[0008] (1) depositing bismuth on a conductive substrate to obtain a bismuth film, using bismuth metal as a target, controlling the sputtering power to 20-80 W, the deposition time to 15-900 s, the substrate rotation speed to 0-25 r / min, the substrate temperature to 300-620 K, the sputtering pressure to 0.7-3.5 Pa, and introducing argon as a carrier gas during the sputtering process, with a flow rate of 5-60 mL / min;
[0009] (2) The bismuth film prepared in step (1) is further calcined in air to obtain a bismuth oxide film.
[0010] Preferably, in the step (1), bismuth is deposited on a conductive substrate by magnetron sputtering to obtain a bismuth thin film.
[0011] Preferably, in step (2), the calcination temperature is controlled to be 450-720K, and the calcination is carried out in any one of a heating table, a high-temperature oven, and a tubular heating furnace.
[0012] In a second aspect, the present invention provides a reconfigurable photoelectric logic gate based on bismuth oxide open-circuit photovoltage that changes non-monotonically with light intensity, comprising a working electrode, wherein the working electrode is a bismuth oxide film deposited on a conductive substrate, and the bismuth oxide film is prepared by the above-mentioned preparation method.
[0013] Preferably, the reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity further includes an input light source, a modulator, a counter electrode, an electrolyte and an electrolytic cell; the input light source includes a first input light source and a second input light source;
[0014] The input light source and modulator are used to emit light to illuminate the same position of the working electrode as the input light;
[0015] The working electrode is fixed inside the electrolytic cell, and the electrolytic cell serves as a container for the electrolyte;
[0016] The counter electrode is fixed inside the electrolytic cell and will not block the light emitted by the input light source and the modulator.
[0017] Preferably, the conductive substrate is one of stainless steel, copper sheet, aluminum sheet, indium tin oxide glass, conductive silicon sheet, and fluorine-doped tin oxide glass.
[0018] Preferably, the counter electrode is one of a platinum sheet, a copper sheet, a silver / silver chloride electrode, and a calomel electrode.
[0019] Preferably, the input light source has a wavelength of 365-450 nm and a light intensity of 0.01-25 mW / cm 2 .
[0020] In a third aspect, the present invention provides a method for assembling a reconfigurable optoelectronic logic gate. The method is based on the above-mentioned reconfigurable optoelectronic logic gate, and the method comprises the following steps:
[0021] Using quartz glass as a light input window;
[0022] The working electrode is fixed inside the electrolytic cell, opposite to the quartz glass window, to ensure that the input light can irradiate the working electrode;
[0023] Fix the counter electrode inside the electrolytic cell and ensure that it does not block the optical path of the input light;
[0024] The three light sources are fixed respectively as the first input light source, the second input light source and the modulator, and the light path is adjusted so that the first input light source, the second input light source and the modulator irradiate the same position of the working electrode.
[0025] In a fourth aspect, the present invention provides a method for realizing logical calculation of a reconfigurable optoelectronic logic gate, wherein the reconfigurable optoelectronic logic gate is assembled by the above-mentioned assembly method, and the method comprises the following steps:
[0026] Inject electrolyte into the electrolytic cell, control the switch and light intensity of the first input light source, the second input light source and the modulator, and mark the on of the first input light source and the second input light source as 1, and the off of the first input light source as 0;
[0027] A voltmeter is used to detect the change in open circuit voltage at both ends of the working electrode and the counter electrode, and an open circuit voltage greater than a threshold is judged as 1, and a voltage less than the threshold is judged as 0;
[0028] By adjusting the light intensity of the first input light source, the second input light source and the modulator, arbitrary reconstruction of XOR gate, multi-input XOR gate, AND gate, NAND gate, OR gate, NOR gate, NOT gate and prohibition gate can be achieved on a single device without changing the threshold.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The bismuth oxide thin film prepared by the bismuth oxide thin film preparation method provided by the present invention discovered for the first time the phenomenon that the open-circuit photovoltage changes non-monotonically with the light intensity, and a reconfigurable photoelectric logic gate was designed and manufactured using this unique property of bismuth oxide; the reconfigurable photoelectric logic gate can achieve programmable reconstruction of multiple logic gates such as XOR gate, AND gate, NAND gate, OR gate, NOR gate, NOT gate, and inhibit gate by adjusting the input light intensity without changing the threshold conditions using a single device.
[0031] In addition, the magnetron sputtering coating technology used to prepare bismuth oxide thin films facilitates large-scale and low-cost production of devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic diagram of a reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with light intensity provided by an embodiment of the present invention;
[0033] Figure 2 A curve diagram showing the variation of the open circuit voltage of a reconfigurable optoelectronic logic gate with light intensity based on the non-monotonic variation of the open circuit photovoltage of bismuth oxide with light intensity provided by an embodiment of the present invention;
[0034] Figure 3 It is the signal output of the XOR gate;
[0035] Figure 4 It is the signal output of the three-input XOR gate;
[0036] Figure 5 is the signal output of the AND gate;
[0037] Figure 6 It is the signal output of the NAND gate;
[0038] Figure 7 It is the signal output of the OR gate;
[0039] Figure 8 It is the signal output of the NOR gate;
[0040] Fig. 9 The signal output for disabling the gate. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0042] Example 1
[0043] See also Figure 1As shown, the reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity provided in this embodiment mainly includes an input light source, a modulator 3, a working electrode 4, a counter electrode 5, an electrolyte and an electrolytic cell; the input light source includes a first input light source 1 and a second input light source 2
[0044] The input light source and modulator 3 are used to emit light to illuminate the same position of the working electrode as the input light; the working electrode is fixed inside the electrolytic cell, and the electrolytic cell serves as a container for the electrolyte; the pair of electrodes are fixed inside the electrolytic cell and will not block the light emitted by the input light source and modulator.
[0045] Specifically, the input light source and modulator wavelength is 405nm, the working electrode is bismuth oxide deposited on a stainless steel substrate, and the counter electrode is a silver / silver chloride electrode. Of course, the input light source and modulator wavelength is 365-450nm, and the light intensity is 0.01-25mW / cm 2 Within the range.
[0046] The preparation of the working electrode includes the following steps:
[0047] (1) A bismuth film was obtained by depositing bismuth on a stainless steel substrate by magnetron sputtering, using bismuth metal as a target, the sputtering power was controlled to be 40 W, the deposition time was controlled to be 120 s, the substrate rotation speed was controlled to be 20 r / min, the substrate temperature was controlled to be 370 K (Kelvin temperature), the sputtering pressure was controlled to be 1.0 Pa, and argon was introduced as a carrier gas during the sputtering process, and its flow rate was controlled to be 30 mL / min;
[0048] (2) The bismuth film prepared in step (1) is further calcined in air to obtain a bismuth oxide film. The calcination temperature is controlled to 620K and the calcination is performed on a heating table.
[0049] Example 2
[0050] Refer to Example 1, except for the preparation of the working electrode.
[0051] The preparation of the working electrode includes the following steps:
[0052] (1) A bismuth film was obtained by depositing bismuth on a stainless steel substrate by magnetron sputtering, using bismuth metal as a target, the sputtering power was controlled to 80 W, the deposition time was controlled to 120 s, the substrate rotation speed was controlled to 15 r / min, the substrate temperature was controlled to 420 K, the sputtering pressure was controlled to 1.5 Pa, and argon was introduced as a carrier gas during the sputtering process, and its flow rate was controlled to 25 mL / min;
[0053] (2) The bismuth film prepared in step (1) is further calcined in air to obtain a bismuth oxide film. The calcination temperature is controlled to be 570K and the calcination is performed on a heating table.
[0054] Example 3
[0055] Refer to Example 1, except for the preparation of the working electrode.
[0056] The preparation of the working electrode includes the following steps:
[0057] (1) A bismuth film was obtained by depositing bismuth on a stainless steel substrate by magnetron sputtering, using bismuth metal as a target, the sputtering power was controlled to be 20 W, the deposition time was controlled to be 360 s, the substrate rotation speed was controlled to be 10 r / min, the substrate temperature was controlled to be 320 K, the sputtering pressure was controlled to be 0.8 Pa, and argon was introduced as a carrier gas during the sputtering process, and its flow rate was controlled to be 20 mL / min;
[0058] (2) The bismuth film prepared in step (1) is further calcined in air to obtain a bismuth oxide film. The calcination temperature is controlled to 520K and the calcination is performed on a heating table.
[0059] Example 4
[0060] This embodiment provides an assembly method of a reconfigurable photoelectric logic gate, wherein the reconfigurable photoelectric logic gate is the reconfigurable photoelectric logic gate described in any one of Embodiments 1-3, and specifically comprises the following steps:
[0061] 1) Use 1mm thick quartz glass as the light input window;
[0062] 2) Fix the working electrode inside the electrolytic cell, opposite to the quartz glass window, to ensure that the input light can irradiate the working electrode;
[0063] 3) Fix the counter electrode inside the electrolytic cell and ensure that it does not block the optical path of the input light;
[0064] 4) Fix three light sources separately as the first input light source, the second input light source and the modulator, and adjust the light paths so that they illuminate the same position of the working electrode.
[0065] Experimental Example 1
[0066] 1. Obtain the curve of photovoltage changing with light intensity
[0067] Using a two-electrode system, after assembling the working electrode obtained in Example 4 above, add electrolyte into the electrolytic cell, and connect a voltmeter to the working electrode and the counter electrode. Irradiate the working electrode with light of different intensities, and record the curve of open circuit photovoltage changing with light intensity, such as Figure 2As shown. When the light intensity is low, the open-circuit photovoltage increases with the light intensity, and then as the light intensity increases, the open-circuit photovoltage reaches a maximum value, and then the light intensity continues to increase, and it is found that the open-circuit photovoltage decreases with the increase of light intensity. In other words, the bismuth oxide thin film prepared by the bismuth oxide thin film preparation method provided by the present invention shows a non-monotonic change trend in the open-circuit photovoltage with the increase of light intensity, while the current classical theory believes that the open-circuit photovoltage is proportional to the logarithm of the light intensity, and there is no similar report of non-monotonic change of photovoltage with the increase of light intensity in the relevant literature. It can be seen that the present invention is the first to discover the phenomenon that the open-circuit photovoltage changes non-monotonicly with the light intensity, and uses this unique property of bismuth oxide to design and manufacture a reconfigurable photoelectric logic gate.
[0068] Experimental Example 2
[0069] 1. Implement XOR gate
[0070] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize the XOR gate.
[0071] Taking advantage of the fact that the open-circuit photovoltage of bismuth oxide changes non-monotonically with light intensity, the XOR gate operation is realized. Specifically, the light intensity of the modulator is set to 0.11mW / cm2, the light intensity of the first input light source is 5.21mW / cm2, and the light intensity of the second input light source is 5.21mW / cm2. The input light is turned on as 1 and turned off as 0. The output threshold is 535mV, that is, the output open-circuit photovoltage is greater than 535mV and is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the XOR gate are shown in the figure below. Figure 3 As shown, the two are consistent, indicating the successful construction of the XOR gate.
[0072] 2. Implement multi-input XOR gate
[0073] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize a multi-input XOR gate.
[0074] The current multi-input XOR gate is not a true "same 0, different 1". Cui Jianguo and others used traditional electronic logic circuits to design a multi-input XOR gate that achieves true "same 0, different 1", but its structure is very complex and not reconfigurable, which limits its practical application. In this patent, by adjusting the input light intensity and the modulator light intensity, a true "same 0, different 1" multi-input XOR gate can be achieved with a single device.
[0075] Take the three-input XOR gate as an example. Specifically, set the light intensity of the modulator to 0.11mW / cm2, the light intensity of the first input light source to 3.83mW / cm2, the light intensity of the second input light source to 3.83mW / cm2, and the light intensity of input 3 to 3.83mW / cm2. Set the input light on as 1 and off as 0. Set the output threshold to 535mV, that is, the output open-circuit light voltage greater than 535mV is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the three-input XOR gate are as follows: Figure 4 As shown, the two are consistent, indicating the successful construction of the three-input XOR gate. For the four-input XOR gate, it is only necessary to change the light intensity of the first input light source-4 to 2.61mW / cm2, and for the five-input XOR gate, it is only necessary to change the light intensity of the first input light source-5 to 2.09mW / cm2.
[0076] 3. Implement AND gate
[0077] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize the AND gate.
[0078] Specifically, the light intensity of the modulator is set to 0.11mW / cm2, the light intensity of the first input light source is set to 0.13mW / cm2, and the light intensity of the second input light source is set to 0.13mW / cm2. The input light is turned on as 1 and turned off as 0. The output threshold is set to 535mV, that is, the output open-circuit light voltage is greater than 535mV and is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the AND gate are shown in the figure below. Figure 5 As shown, the two are consistent, indicating that the AND gate is successfully constructed.
[0079] 4. Implementing NAND Gate
[0080] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize the NAND gate.
[0081] Specifically, the light intensity of the modulator is set to 0.99mW / cm2, the light intensity of the first input light source is 5.21mW / cm2, and the light intensity of the second input light source is 5.21mW / cm2. The input light is turned on as 1 and turned off as 0. The output threshold is 535mV, that is, the output open circuit light voltage is greater than 535mV and is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the NAND gate are as follows: Figure 6 As shown, the two are consistent, indicating that the NAND gate is successfully constructed.
[0082] 5. Implement OR gate
[0083] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize the OR gate.
[0084] Specifically, the light intensity of the modulator is set to 0.11mW / cm2, the light intensity of the first input light source is set to 0.51mW / cm2, and the light intensity of the second input light source is set to 0.51mW / cm2. The input light is turned on as 1 and turned off as 0. The output threshold is set to 535mV, that is, the output open-circuit light voltage is greater than 535mV and is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the OR gate are as follows: Figure 7 As shown, the two are consistent, indicating that the OR gate is successfully constructed.
[0085] 6. Implement NOR gate and NOT gate
[0086] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to realize NOR gate and NOT gate.
[0087] Specifically, the light intensity of the modulator is set to 0.99mW / cm2, the light intensity of the first input light source is set to 10.45mW / cm2, and the light intensity of the second input light source is set to 10.45mW / cm2. The input light is recorded as 1 when it is on and 0 when it is off. The output threshold is recorded as 535mV, that is, the output open-circuit light voltage is recorded as 1 when it is greater than 535mV and as 0 when it is less than 535mV. The signal output and truth table of the NOR gate are shown in Figure 8. The two are consistent, indicating that the NOR gate is successfully constructed. As long as the double input of the NOR gate is changed to a single input, a NOT gate can be obtained.
[0088] 7. Implement NOR gate and NOT gate
[0089] By adjusting the input light intensity and the modulator light intensity, the logic gate is reconstructed to achieve a disable gate.
[0090] Specifically, the light intensity of the modulator is set to 0.11mW / cm2, the light intensity of the first input light source is set to 0.51mW / cm2, and the light intensity of the second input light source is set to 11.31mW / cm2. The input light is turned on as 1 and turned off as 0. The output threshold is set to 535mV, that is, the output open-circuit light voltage is greater than 535mV and is recorded as 1, and less than 535mV is recorded as 0. The signal output and truth table of the inhibit gate are shown in the figure below. Fig. 9 As shown, the two are consistent, indicating that the forbidden gate is successfully constructed.
[0091] In summary, the present invention has developed a reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity. By adjusting the input light intensity, without changing the threshold conditions, a single device can be used to realize the programmable reconstruction of various logic gates such as XOR gate, AND gate, NAND gate, OR gate, NOR gate, NOT gate, and inhibit gate. Because the open-circuit voltage is independent of the device size and is an intrinsic property of the photoelectric material, the photoelectric logic gate signal based on the open-circuit voltage signal of the present invention does not change with the device size, which greatly reduces the device processing accuracy requirements and is expected to significantly reduce the device processing cost. Compared with traditional electronic logic gates, the photoelectric logic gate proposed in the present invention is expected to achieve more complex operations and calculations with fewer components due to its flexible and diverse programmable reconstruction characteristics, showing great application prospects in the upcoming era of the Internet of Things with explosive growth of information.
[0092] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable ordinary technicians in the field to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made based on the essence of the content of the present invention should be included in the protection scope of the present invention.
Claims
1. A reconfigurable optoelectronic logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with light intensity, characterized in that: The method comprises a working electrode, wherein the working electrode is a bismuth oxide film deposited on a conductive substrate, and the bismuth oxide film is prepared by the following method: (1) depositing bismuth on a conductive substrate to obtain a bismuth film, using bismuth metal as a target, controlling the sputtering power to 20-80 W, the deposition time to 15-900 s, the substrate rotation speed to 0-25 r / min, the substrate temperature to 300-620 K, the sputtering pressure to 0.7-3.5 Pa, and introducing argon as a carrier gas during the sputtering process, with a flow rate of 5-60 mL / min; (2) further calcining the bismuth film prepared in step (1) in air to obtain a bismuth oxide film; The reconfigurable optoelectronic logic gate further includes an input light source, a modulator, a counter electrode, an electrolyte, and an electrolytic cell; the input light source includes a first input light source and a second input light source; The input light source and modulator are used to emit light to illuminate the same position of the working electrode as the input light; The working electrode is fixed inside the electrolytic cell, and the electrolytic cell serves as a container for the electrolyte; The counter electrode is fixed inside the electrolytic cell and will not block the light emitted by the input light source and the modulator.
2. The reconfigurable photoelectric logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity as claimed in claim 1, characterized in that: The conductive substrate is one of stainless steel, copper sheet, aluminum sheet, indium tin oxide glass, conductive silicon sheet, and fluorine-doped tin oxide glass.
3. The reconfigurable optoelectronic logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity as claimed in claim 1, characterized in that: The counter electrode is one of a platinum sheet, a copper sheet, a silver / silver chloride electrode, and a calomel electrode.
4. The reconfigurable optoelectronic logic gate based on the non-monotonic change of the open-circuit photovoltage of bismuth oxide with the light intensity as claimed in claim 1, characterized in that: The input light source has a wavelength of 365-450nm and a light intensity of 0.01-25mW / cm 2 .
5. A method for assembling a reconfigurable optoelectronic logic gate, the method being based on the reconfigurable optoelectronic logic gate according to claim 1, characterized in that: The method comprises the following steps: Using quartz glass as a light input window; The working electrode is fixed inside the electrolytic cell, opposite to the quartz glass window, to ensure that the input light can irradiate the working electrode; Fix the counter electrode inside the electrolytic cell and ensure that it does not block the optical path of the input light; The three light sources are fixed respectively as the first input light source, the second input light source and the modulator, and the light path is adjusted so that the first input light source, the second input light source and the modulator irradiate the same position of the working electrode.
6. A method for realizing logical calculation of a reconfigurable optoelectronic logic gate, wherein the reconfigurable optoelectronic logic gate is assembled by the assembly method according to claim 5, characterized in that: The method comprises the following steps: Inject electrolyte into the electrolytic cell, control the switch and light intensity of the first input light source, the second input light source and the modulator, and mark the on of the first input light source and the second input light source as 1, and the off of the first input light source as 0; A voltmeter is used to detect the change in open circuit voltage at both ends of the working electrode and the counter electrode, and an open circuit voltage greater than a threshold is judged as 1, and a voltage less than the threshold is judged as 0; By adjusting the light intensity of the first input light source, the second input light source and the modulator, arbitrary reconstruction of XOR gate, multi-input XOR gate, AND gate, NAND gate, OR gate, NOR gate, NOT gate and prohibition gate can be achieved on a single device without changing the threshold.
Citation Information
Cited By
Size-insensitive all-solid-state photoelectric exclusive-OR logic gate
CN122577874A