A laser brazing method for compensation net

By using a special stainless steel porous compensation mesh in the welding of automobile panels, the problems of uneven welds and leakage in non-standard welding are solved, the welding performance and yield are improved, and the welding needs of high-strength automobile panels are met.

CN115635156BActive Publication Date: 2024-10-18CHINA FAW CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211251974.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2024-10-18
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

The non-standard welding between the car roof and the side panel has problems such as low yield and leakage of solder in the laser brazing process. It is difficult to meet the welding needs of high-strength automobile panels. It is difficult to improve the welding seam with existing technology. Yield and welding performance.

Method used

A special stainless steel metal porous compensation net is used. After stamping, grinding, alkali cleaning and ultrasonic cleaning, the compensation net is clamped in the weld, and its adsorption effect on the solder is used to limit the flow of the solder to form a solder- Compensation net-sandwich structure of solder improves welding performance.

Benefits of technology

It significantly improves the yield of laser brazing of automobile panels, enhances the tensile strength of the weld, reduces production costs, avoids the formation of uneven welds and pores, and improves the welding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115635156B_ABST
    Figure CN115635156B_ABST
Patent Text Reader

Abstract

The present invention specifically relates to a method for laser brazing of compensation mesh. The method comprises the following steps: S1, preparing a stainless steel metal compensation mesh: selecting a stainless steel thin plate strip, forming a compensation mesh with a specific aperture by one-time stamping, and cutting it into the required width and length; grinding the two sides of the compensation mesh with sandpaper, then washing it with a high-pressure water gun, then alkaline washing, and finally ultrasonically cleaning it in alcohol, drying it, and placing it in a constant temperature drying oven for standby use. S2, splicing and pressing the automobile brazing material plates to maintain a certain gap, placing the stainless steel metal compensation mesh in the middle of the gap, and using a clamping device to ensure that the compensation mesh is in a central upright state, and then laser brazing is performed at a given power and wire feeding speed. Laser welding is enhanced by physical means, and the opening in the middle of the compensation mesh also effectively avoids uneven distribution of the brazing material on both sides, and improves the tensile strength of the weld, effectively preventing the formation of pores during welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular to a compensation net laser brazing method. Background Art

[0002] At present, the mainstream connection methods between the car roof and the side panel are resistance spot welding and laser brazing. Among them, resistance spot welding is that the spot welding electrode applies and maintains a certain pressure on the workpiece to be welded, and the heat generated by the current during the stable contact process increases the temperature to form a weld point. Laser brazing is a brazing technology that uses laser as a heat source to heat the brazing material, so that the welding wire is fully melted to form a high-temperature liquid metal that infiltrates into the joints of the welded parts to achieve a good combination between the workpieces. Compared with traditional resistance spot welding, laser brazing has the advantages of low production cost, fast production speed, and beautiful products. Therefore, laser welding is the main connection method on the market.

[0003] In view of the many advantages of laser brazing, it is currently used in the welding of thin plates of various types of base materials or welding with high strength requirements in the market, especially in industrial applications between galvanized automotive steel plates. However, compared with the laser brazing of standard plates, the non-standard welding between the car roof and the side panels places higher requirements on laser brazing. Special-shaped welds place higher requirements on the flow properties of the brazing material and the clamping and joining stability of the welding base material during the laser brazing process. However, the current production technology level is limited, and laser welding between automotive plates often has problems such as low yield and weld brazing material leakage. At the same time, higher base material performance also places higher requirements on weld performance.

[0004] The national intelligent manufacturing vision plan puts forward lightweight and high-strength requirements for automobile manufacturing, which also makes the welding process of automobile welds urgently need more stringent technical standards. The current welding foundation can no longer meet the welding requirements of high-strength automobile plates. Therefore, improving the weld yield and welding performance has become a major problem in current automobile manufacturing.

[0005] The published Chinese invention application CN113547214A "A laser welding process for lightweight aluminum alloys for new energy vehicles" mentions a welding method that adds rare earth elements accounting for 0.01% of the mass of the aluminum alloy into the weld. This method can make the rare earth elements evenly distributed in the weld, thereby improving the weld strength.

[0006] Chinese invention patent CN110587135A "Welding method for laser tailor-welded plate welds to prevent stamping cracking" provides a welding method using prefabricated welding plates with a thickness of 0.5-3.0 mm. This method can make two types of plates exist in the welding position, improve the elongation and strength of the plate after welding, and avoid cracking during stamping of automobile plates.

[0007] However, both of the above two methods have certain limitations and encounter certain difficulties in the actual production process. It is also difficult to achieve high-efficiency production, and the production cost will also be greatly increased. Summary of the invention

[0008] In order to solve the problems of low yield rate, weld collapse, irregularity and leaking during the welding process of automobile plates, this study proposes a method of adding a porous compensation mesh for laser welding of automobile plates. The porous metal compensation mesh is used to limit the flow of brazing material and effectively compensate for the uneven weld caused by unstable clamping, effectively improving the yield rate of laser brazing of automobile plates and significantly improving its welding performance.

[0009] The present invention provides a compensation mesh laser brazing method, the method comprising the following steps:

[0010] S1. Preparation of stainless steel compensation mesh: Select stainless steel sheet strip, and form it into a compensation mesh with a specific aperture by one-time stamping, and cut it into the required width and length; grind both sides of the compensation mesh with sandpaper, then rinse it with a high-pressure water gun, then perform alkaline washing, and finally perform ultrasonic cleaning in alcohol, blow dry and place it in a constant temperature drying oven for use.

[0011] S2. The automobile brazing material plates are spliced ​​and pressed to maintain a certain gap, the stainless steel metal compensation mesh is placed in the middle of the gap, and a clamping device is used to ensure that the compensation mesh is in the middle and upright state, and then laser brazing is performed at a given power and wire feeding speed.

[0012] Furthermore, the stamping pressure used in step S1 is 5 tons, and fixed die stamping is adopted.

[0013] Furthermore, the given thickness of the stainless steel strip described in step S1 is 0.05 mm to 0.075 mm, the diameter of the punching hole during stamping is 0.1 mm to 0.2 mm, and the mesh spacing of the compensation net is 0.2 mm to 0.3 mm.

[0014] Furthermore, the types of sandpaper in step S1 include 800#, 1200# and 2000# water-abrasive sandpaper.

[0015] Furthermore, the impact pressure of the high-pressure water gun described in step S1 is 10 MPa, which is a porous jet.

[0016] Furthermore, the alkaline washing time in step S1 is 5 min to 10 min, the washing agent used is 5% to 8% sodium hydroxide aqueous solution, and the ultrasonic cleaning time is 10 min to 20 min.

[0017] Furthermore, in step S2, the gap between the solder plates is maintained at 0.1 mm to 0.2 mm.

[0018] Furthermore, the brazing material for laser brazing in step S2 is CuSi3 welding wire, and the wire diameter is 1 mm to 1.6 mm.

[0019] Furthermore, the clamping device described in step S2 is a triangular wedge with the same material and specification as the stainless steel metal compensation mesh, the top angle of the wedge is 15° to 30°, and the long right-angle side is 1mm to 2mm.

[0020] Furthermore, the given power described in step S2 is 1800W to 2200W, the welding speed is 1.2m / min to 2.2m / min, the wire feeding speed is consistent with the welding speed, and the laser spot diameter is 0.2mm to 0.4mm.

[0021] The beneficial effects of the present invention are as follows: the automobile roof compensation mesh welding method provided by the present invention adds a special compensation mesh to the center of the weld and fixes it with a clamping device. The compensation mesh with a specific aperture size and opening distribution has a good adsorption effect on the solder and can effectively limit the flow of the solder, reduce the probability of welding leakage, and thus improve the yield rate and reduce costs.

[0022] The welding method provided by the present invention forms a multi-layer reinforced welding structure of brazing filler metal-compensation net-brazing filler metal between the automobile roof and the side panel. Laser welding is enhanced by physical means, and the opening in the middle of the compensation net also effectively avoids uneven distribution of brazing filler metal on both sides, improves the tensile strength of the weld, and effectively prevents the formation of pores during welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the cross section of the laser brazed stainless steel compensation mesh;

[0024] Figure 2 A schematic diagram of a clamping device used in the laser brazing process;

[0025] Figure 3 Schematic diagram of the weld cross section of the clamping device after using a compensation net for laser brazing;

[0026] Figure 4 This is a top view of the weld after laser brazing. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0029] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0030] The technical solution provided by the present invention is as follows: a compensation mesh laser brazing method that can significantly improve the brazing strength of high-strength automobile plates, characterized in that the weld has a special compensation mesh sandwich structure, specifically involving adding a layer of stainless steel compensation mesh with a specific thickness and aperture in the middle part of the weld on the basis of original laser brazing, and combining it with a specific welding process, which can effectively avoid problems such as leaking welds during the welding process. The embodiments of this technical solution are as follows.

[0031] Example 1

[0032] A compensation mesh laser brazing method that can significantly improve the brazing strength of high-strength automotive plates. By using a special compensation mesh and clamping device in the laser welding process, and matching it with a matching laser welding process, a sandwich reinforcement structure of brazing material-compensation mesh-brazing material is formed in the weld. The metal compensation mesh used is a 304 stainless steel thin plate strip of a given thickness, which is formed into a mesh material with a specific aperture by a single stamping, and then cut into a suitable width and length. After cutting, it is polished with 800#, 1200#, and 2000# water-abrasive sandpaper, cleaned with a high-pressure water gun porous jet with an impact pressure of 10MPa, and then alkaline washed in a 5% sodium hydroxide aqueous solution for 5 minutes, and finally ultrasonically cleaned for 20 minutes, and dried in an incubator.

[0033] The stamping pressure is 5 tons, fixed die stamping is used, the given thickness of the stainless steel strip is 0.05mm, the stamping hole is a small round hole with a diameter of 0.2mm, and the mesh spacing is 0.2mm. The schematic diagram is as follows Figure 1 As shown, circular apertures of the same size are evenly distributed on the entire stainless steel strip at a spacing of 0.2 mm.

[0034] The clamping device used is a triangular wedge with the same material and specifications as the compensation net. The top angle of the wedge is 30° and the long right angle side is 2mm. The schematic diagram is as follows Figure 2 As shown in the figure, it is made of the same specifications and materials as the compensation net, and has the same size circular hole in the middle. The laser brazing brazing material used in the laser brazing process is CuSi3 welding wire with a wire diameter of 1.6mm. The gap between the automobile plates during the welding process is 0.2mm. The laser power in the laser brazing process is 2200W, the welding speed is 2.2m / min, the wire feeding speed is consistent with the welding speed, and the laser spot diameter is 0.4mm.

[0035] The schematic diagram of the cross section of the weld at the clamping device after welding and the overall longitudinal section of the weld is as follows: Figure 3 As shown in the figure, the brazing material evenly penetrates into the mesh of the stainless steel compensation mesh and is tightly combined with the compensation mesh matrix to form a solid sandwich structure. At the same time, the existence of the compensation mesh hinders the infiltration of the brazing material, which can better prevent the brazing material from leaking out of the gap. The metal porous compensation mesh is parallel to the connecting end faces of the car roof and side panels and spreads evenly, which allows the brazing material to evenly penetrate and wrap the metal porous compensation mesh on the premise of good bonding with the matrix on both sides, forming a uniformly distributed circular infiltration structure. This special connection layer containing a metal porous compensation mesh and an ellipsoidal pore structure can effectively reduce the concentration of thermal stress and mechanical stress during the brazing temperature rise and fall and service process, and achieve the purpose of strengthening and toughening the welding parts of the automobile plate. According to the tensile strength test analysis, the tensile strength of the weld reached 390.5MPa, which is 30% higher than the tensile strength of the automobile plate welded by the same process without the metal mesh.

[0036] Example 2

[0037] The difference between this embodiment and Example 1 is that the metal porous compensation mesh is adjusted from a circle to a square with a side length of 0.2 mm, and the rest of the technical solutions are the same as those of Example 1. Due to the surface tension of the solder droplet, even if the opening is square, the droplet still forms a circle after passing through the compensation mesh, which results in a certain gap between the solder and the square hole after solidification, and the square hole is not completely filled.

[0038] After tensile strength test, the tensile strength of the square hole compensation mesh reached 375.4MPa, which is 25% higher than that of the automobile plate without metal mesh. It is also effective in preventing solder leakage, but due to the gaps between the mesh holes, the solder and the compensation mesh are not tightly combined, resulting in a certain degree of strength loss.

[0039] Example 3

[0040] Considering that the aperture will have a certain impact on the tensile strength, and the production difficulty of different apertures is also different, this embodiment provides compensation meshes with different apertures, and the apertures of the round hole compensation meshes are 0.1mm, 0.3mm, 0.4mm and 0.5mm respectively. The remaining parameters, production process and welding process are the same as those in Example 1. The solder infiltrates the round holes of the compensation mesh more evenly, but a small amount of internal pores appear in the large-aperture embodiment 0.5mm, which is not allowed in the production standard, and in the small-aperture embodiment 0.1mm, it is found that there are many unfilled or unfilled pores in the compensation mesh, resulting in pores in the weld, which is also not allowed.

[0041] By conducting tensile strength tests on the 0.1mm, 0.3mm, 0.4mm and 0.5mm round hole compensation meshes of the embodiments, the tensile strength of the 0.3mm round hole compensation mesh is 372.4MPa, which is closer to Example 2, and is 24% higher than the tensile strength of the automobile plate welded with the same process without the metal mesh; the tensile strength of the 0.4mm round hole compensation mesh is 360.4MPa, which is 20% higher than the tensile strength of the automobile plate welded with the same process without the metal mesh; the tensile strength of the 0.5mm round hole compensation mesh is significantly reduced to 330.4MPa, which is only 10% higher than the tensile strength of the automobile plate welded with the same process without the metal mesh; the tensile strength of the 0.1mm round hole compensation mesh is 381.6MPa, which is 27% higher than the tensile strength of the automobile plate welded with the same process without the metal mesh. In general, the reinforcement effect of the metal compensation mesh mainly depends on the stainless steel material of the compensation mesh itself. After the aperture is enlarged, the material area of ​​the metal compensation mesh is reduced, so the tensile strength is also reduced, but at the same time, the aperture cannot be too small. Since the solder itself has a certain viscosity and surface tension, a too small aperture will result in no solder infiltration in some of the pores of the compensation mesh, affecting the quality.

[0042] Example 4

[0043] Compared with Example 1, this embodiment modifies the welding process and reduces the laser power in the laser brazing process to 1800W. The welding speed is 1.2m / min, the wire feeding speed is consistent with the welding speed, and the laser spot diameter is 0.2mm. Lowering the welding speed and the spot diameter can make the brazing material fully melt and fully penetrate into the compensation mesh. The more thoroughly melted brazing material will also combine more thoroughly with the compensation mesh, thereby improving the weld quality and yield rate.

[0044] After the tensile strength test, although the welding speed was reduced after adjusting the laser welding process, the overall tensile strength was improved, and the tensile strength was 405.3MPa, which was 35% higher than that of the original laser welding process without the compensation net. However, the production speed was reduced by 25% compared with the laser welding process of Example 1. Therefore, in the actual application of the present invention, it is necessary to comprehensively consider product quality and production speed.

[0045] The above is only a preferred embodiment of the present invention, and does not limit the form of the present invention. Any person skilled in the art can use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A compensation mesh laser brazing method, characterized in that: The method comprises the following steps: S1. Preparation of stainless steel compensation mesh: Select stainless steel sheet strip, and form it into a compensation mesh with a specific aperture by one-time stamping, and cut it into the required width and length; polish both sides of the compensation mesh with sandpaper, then rinse it with a high-pressure water gun, then perform alkaline washing, and finally perform ultrasonic cleaning in alcohol, blow dry and place it in a constant temperature drying oven for use; S2. The automobile brazing material plates are spliced ​​and pressed to maintain a certain gap, the stainless steel metal compensation mesh is placed in the middle of the gap, and a clamping device is used to ensure that the compensation mesh is in the middle and upright state, and then laser brazing is performed at a given power and wire feeding speed; The clamping device is a triangular wedge with the same material and specification as the stainless steel metal compensation mesh, the top angle of the wedge is 15° to 30°, and the long right-angle side is 1mm to 2mm.

2. The compensation mesh laser brazing method according to claim 1, characterized in that: The stamping pressure used in step S1 is 5 tons, and fixed die stamping is adopted.

3. The compensation mesh laser brazing method according to claim 1, characterized in that: The given thickness of the stainless steel sheet strip described in step S1 is 0.05 mm to 0.075 mm, the diameter of the punching hole during punching is 0.1 mm to 0.2 mm, and the mesh spacing of the compensation net is 0.2 mm to 0.3 mm.

4. The compensation mesh laser brazing method according to claim 1, characterized in that: The types of sandpaper in step S1 include 800#, 1200# and 2000# water-abrasive sandpaper.

5. The compensation mesh laser brazing method according to claim 1, characterized in that: The impact pressure of the high-pressure water gun described in step S1 is 10 MPa, which is a porous jet.

6. The compensation mesh laser brazing method according to claim 1, characterized in that: The alkaline washing time in step S1 is 5 min to 10 min, the washing agent used is 5% to 8% sodium hydroxide aqueous solution, and the ultrasonic cleaning time is 10 min to 20 min.

7. The compensation mesh laser brazing method according to claim 1, characterized in that: In step S2, the gap between the solder plates is maintained at 0.1 mm to 0.2 mm.

8. The compensation mesh laser brazing method according to claim 1, characterized in that: The brazing material for laser brazing in step S2 is CuSi3 welding wire, and the wire diameter is 1 mm to 1.6 mm.

9. The compensation mesh laser brazing method according to claim 1, characterized in that: The given power described in step S2 is 1800W to 2200W, the welding speed is 1.2m / min to 2.2m / min, the wire feeding speed is consistent with the welding speed, and the laser spot diameter is 0.2mm to 0.4mm.

Citation Information

Patent Citations

  • Welding method for stamping cracking prevention of welding seam of laser tailor-welded blank

    CN110587135A

  • Laser welding process for light aluminum alloy of new energy automobile

    CN113547214A

  • Laser brazing clearance compensation method

    CN101862874A

  • Laser welding method

    CN102139412A