Method for forming coating, coating device, component and plasma reaction device
By using rare earth metal compounds and shielding ring separation technology, a corrosion-resistant coating with a quasi-single crystal structure is formed, which solves the problems of coating failure and particle contamination during the plasma etching process, improves corrosion resistance, and is suitable for advanced semiconductor processes.
Patent Information
- Application Number
- CN202211248078.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-12
AI Technical Summary
During the plasma etching process, the corrosion-resistant coating on the surface of the component body gradually fails, resulting in micro-particle contamination, which cannot meet the needs of advanced semiconductor manufacturing processes.
Rare earth metal compounds are used as corrosion-resistant coating materials. By setting up a shielding ring in the coating device, the formation of metal vapor and the chemical reaction of the coating compound are separated into two independent areas to form a corrosion-resistant coating with a quasi-single crystal structure. .
It improves the resistance to plasma physical bombardment and chemical corrosion, reduces the generation of tiny particles, and meets the higher requirements for corrosion resistance in advanced manufacturing processes.
Smart Images

Figure CN115637418B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for forming a coating, a coating device, components and a plasma reaction device. Background Art
[0002] In the field of integrated circuit manufacturing, plasma etching technology plays a key role. With the continuous improvement of the aspect ratio index in the plasma etching process, the plasma corrosion environment to which the components in the etching chamber are subjected is becoming increasingly harsh. The components in the plasma etching chamber are required to have higher resistance to plasma physical bombardment and chemical corrosion, and produce less tiny particle pollution and metal pollution sources, in order to further ensure the stability and repeatability of the etching equipment process.
[0003] In the existing technology, yttrium-containing (Y2O3, YF3, etc.) coatings gradually show ineffective micro-particle contamination in these advanced processes (5nm and below) and cannot better meet the process requirements. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the corrosion-resistant coating on the surface of the component body gradually fails and forms tiny particle pollution during the plasma etching process, so as to meet the needs of advanced semiconductor processes.
[0005] In order to achieve the above object, the present invention provides a coating device for forming a corrosion-resistant coating, comprising:
[0006] Vacuum chamber;
[0007] A first electrode is disposed on the top of the vacuum chamber, and a metal target is disposed below the first electrode;
[0008] A second electrode is disposed in the vacuum chamber, a workpiece to be coated is disposed above the second electrode, and the workpiece to be coated is disposed opposite to the metal target;
[0009] A shielding ring is disposed in the vacuum chamber and between the first electrode and the second electrode, and divides the vacuum chamber into a first area above the shielding ring and a second area below the shielding ring, and includes an opening, and the opening connects the first area and the second area;
[0010] A first gas component is used to input a first gas into the first region, the first gas forms plasma under the action of the first electrode and the second electrode, and the plasma is used to bombard the metal target material to form metal vapor;
[0011] The second gas component is used to deliver a second gas to the second area, and the second gas reacts with the metal vapor to form a corrosion-resistant coating on the surface of the workpiece to be coated.
[0012] Optionally, the coating device further comprises: a vacuum pump, configured to allow the airflow to flow from the first area to the second area and then be drawn out of the vacuum cavity.
[0013] Optionally, the vacuum pump is disposed below a base of the second electrode and is connected to the second region.
[0014] Optionally, the second gas component is disposed below the shielding ring, and the second gas component and the shielding ring are disposed separately.
[0015] Optionally, the second gas assembly is disposed within the shielding ring.
[0016] Optionally, a projection area of the opening of the shielding ring on the surface of the workpiece to be coated is greater than or equal to the area of the workpiece to be coated.
[0017] Optionally, the shielding ring is connected to the inner wall of the vacuum chamber.
[0018] Optionally, the material of the shielding ring includes at least one of oxide ceramics, nitride ceramics, silicon, SiC, quartz, etc.
[0019] Another object of the present invention is to provide a method for forming a component of a plasma reaction device, comprising: providing the above-mentioned coating device for forming a corrosion-resistant coating;
[0020] Providing a metal target and placing it below the first electrode;
[0021] Providing a component body as a workpiece to be coated, and placing it on the second electrode;
[0022] A first gas is introduced into the first region, the first gas forms plasma under the action of the first electrode and the second electrode, and the plasma excites the metal target to form metal vapor;
[0023] introducing a second gas into the second region;
[0024] The metal vapor enters the second region through the opening, and chemically reacts with the second gas to form a corrosion-resistant coating on the surface of the workpiece to be coated.
[0025] Optionally, the atomic radius of the metal element in the metal target is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium.
[0026] Optionally, the metal element includes at least one of Ho, Er, Tm, Yb, and Lu.
[0027] Optionally, the first gas includes at least one of inert gases such as He, Ne, Ar, and Xe.
[0028] Optionally, the second gas includes oxygen-containing gas and / or fluorine-containing gas.
[0029] Optionally, the oxygen-containing gas includes at least one of oxygen, ozone, and oxygen-enriched air.
[0030] Optionally, the fluorine-containing gas includes HF or fluorine-substituted alkanes.
[0031] Optionally, the general formula of the fluorine-substituted alkane is C x H y F z , where x is 1-5, y≥0, and z>0.
[0032] Another object of the present invention is to provide a component of a plasma reaction device, comprising:
[0033] Component body;
[0034] A corrosion-resistant coating is formed on the component body by the above-mentioned formation method; the atomic radius of the metal element in the corrosion-resistant coating is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium; the diffraction peaks of the corrosion-resistant coating obtained by X-ray diffraction are composed of a main peak and other peaks whose intensities are at least 1 / 5 of the main peak intensity; the half-peak width of the main peak is less than 1°.
[0035] Optionally, the corrosion-resistant coating is a rare earth metal compound, the rare earth metal compound includes at least one of oxides, fluorides, and fluoride oxides of rare earth metal elements, and the rare earth metal elements include at least one of Ho, Er, Tm, Yb, and Lu.
[0036] Optionally, the intensity ratio of the secondary peak to the main peak is less than 1 / 10, and the half-peak width of the main peak is less than 0.5°.
[0037] Optionally, the thickness of the corrosion-resistant coating ranges from 0.1 um to 1000 um.
[0038] Another object of the present invention is to provide a plasma reaction device, comprising:
[0039] A reaction chamber, wherein the reaction chamber is a plasma environment;
[0040] The component is exposed to the plasma environment.
[0041] Optionally, the plasma reaction device is an inductively coupled plasma reaction device;
[0042] The components include: at least one of a ceramic cover plate, a bushing, a gas nozzle, a gas connection flange, a focusing ring, an insulating ring, an electrostatic chuck, a cover ring or a plasma confinement device.
[0043] Optionally, the plasma reaction device is a capacitively coupled plasma reaction device;
[0044] The components include: at least one of a gas shower head, a gasket, a nozzle, a gas distribution plate, an electrostatic chuck, a plasma confinement device, a focusing ring, an insulating ring, and a covering ring.
[0045] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0046] The present invention selects rare earth metal compounds as the corrosion-resistant coating of the parts of the plasma reaction device, wherein the rare earth metal elements have similar chemical properties to yttrium, and have a smaller atomic radius and a larger relative atomic mass, so that the corrosion-resistant coating has better resistance to plasma physical bombardment and chemical corrosion. In order to further meet the higher corrosion resistance requirements of advanced processes, the present invention also sets a shielding ring in the coating device, which divides the vacuum cavity into two independent areas, so that the metallization step of forming metal vapor and the chemical reaction step of forming the coating compound are respectively carried out in two independent areas and do not interfere with each other, thereby realizing that the corrosion-resistant coating continuously formed on the surface of the workpiece to be coated has a single-crystal-like structure, that is: the powder diffraction spectrum of the corrosion-resistant coating is composed of a main peak and a secondary peak whose intensity is at least 1 / 5 less than the main peak intensity, which makes the crystal orientation of the grains in the coating highly consistent, and its corrosion resistance is further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The figure is a schematic structural diagram of parts of a plasma reaction device of the present invention.
[0048] Figure 2 It is a structural schematic diagram of an inductively coupled plasma reaction device of the present invention.
[0049] Figure 3 It is a structural schematic diagram of a capacitively coupled plasma reaction device of the present invention.
[0050] Figure 4 It is a schematic structural diagram of a coating device for forming a corrosion-resistant coating according to the present invention.
[0051] Figure 5 It is a schematic structural diagram of another coating device for forming a corrosion-resistant coating according to the present invention.
[0052] Figure 6 The present invention is a flowchart of a method for forming components of a plasma reaction device.
[0053] Figure 7 XRD spectrum of the corrosion-resistant coating Yb2O3 formed in an embodiment of the present invention.
[0054] Figure ID
[0055] Component body 1, corrosion-resistant coating 2; ceramic cover plate 201, bushing 202, gas nozzle 203, focusing ring 204, 307, insulating ring 205, 308, electrostatic chuck 206, 305, covering ring 207, 309, plasma confinement device 208, 306; cover plate 301, nozzle 302, gas distribution plate 303, gas shower head 304; vacuum chamber 10, first region 11, second region 12, first electrode 20, second electrode 30, shielding ring 40, opening 41, first gas component 50, second gas component 60, vacuum pump 70, metal target 01, workpiece to be coated 02, plasma 03. DETAILED DESCRIPTION
[0056] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] In the description of the present invention, it should be noted that the terms "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0058] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0059] The plasma reaction device comprises: a reaction chamber and components constituting the device. In the working state, the reaction chamber is a plasma environment, and the components are exposed to the plasma environment. Since plasma is highly corrosive, it is necessary to apply a corrosion-resistant coating on the surface of the component body to prevent the plasma from corroding the component body.
[0060] Research has found that yttrium-containing (such as Y2O3, YF3, YOF, etc.) coatings as corrosion-resistant coatings can resist plasma physical bombardment and have good chemical corrosion resistance. However, with the development of semiconductor devices, higher requirements are placed on the integration of semiconductor devices. The line width of semiconductor devices is getting smaller and smaller. To obtain a groove with a smaller line width, the power and steps used in the plasma etching process are greatly increased. As a result, the corrosion-resistant coating on the surface of the component needs to be subjected to plasma physical bombardment and / or chemical corrosion intensity, which is greatly enhanced and the action time is greatly extended, causing the yttrium-containing coating to begin to corrode and be easily bombarded to produce tiny particles. These particles are scattered on the wafer or cavity wall, forming pollution, and cannot meet the corrosion resistance requirements of the ever-changing semiconductor process, especially the advanced process below 5nm.
[0061] To solve this technical problem, the present invention uses an element with similar chemical stability to Y but stronger resistance to plasma physical bombardment (smaller ion radius, larger molar mass) as the main coating material to form a surface coating with a single crystal structure on the surface of the component. The coating can resist physical bombardment and chemical corrosion for a long time, maintain the stability of the environment in the reaction chamber, and meet the corrosion resistance requirements of components in advanced processes.
[0062] like Figure 1 As shown, the present invention provides a component of a plasma reaction device, which includes:
[0063] Component body 1;
[0064] A corrosion-resistant coating 2 is formed on the component body 1.
[0065] The atomic radius of the metal element in the corrosion-resistant coating is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium; the diffraction peak of the corrosion-resistant coating obtained by X-ray diffraction consists of a main peak and a secondary peak with an intensity at least 1 / 5 less than the main peak intensity; the half-peak width of the main peak is less than 1°.
[0066] In some embodiments, the intensity ratio of the secondary peak to the main peak is less than 1 / 10, and the half-peak width of the main peak is less than 0.5°.
[0067] In some embodiments, the thickness of the corrosion-resistant coating ranges from 0.1 um to 1000 um.
[0068] The plasma reaction device may be an inductively coupled plasma (ICP) reaction device, such as Figure 2 As shown, the components include: a ceramic cover plate 201, a bushing 202, a gas nozzle 203, a gas connecting flange (not shown), a focusing ring 204, an insulating ring 205, an electrostatic chuck 206, a covering ring 207 or at least one of a plasma confinement device 208.
[0069] It can be understood that the plasma reaction device can also be a capacitively coupled plasma (CCP) reaction device; Figure 3 As shown, the components include: a cover plate 301 , a nozzle 302 , a gas distribution plate 303 , a gas shower head 304 , an electrostatic chuck 305 , a plasma confinement device 306 , a focusing ring 307 , an insulating ring 308 , and at least one of a cover ring 309 .
[0070] The corrosion-resistant coating is a rare earth metal compound, including at least one of oxides, fluorides and oxyfluorides of rare earth metal elements.
[0071] Rare earth metal elements have similar outer electron structures, including yttrium (Z = 39) and lanthanide metal elements (La-Lu, atomic numbers from 57 to 71). Among them, lanthanide metal elements belong to the third subgroup with yttrium, and lanthanide metal elements are located in the sixth period of the periodic table. Compared with yttrium in the fifth period, the atomic structure is similar, the atomic radius is similar or smaller, but the relative atomic mass is greater than yttrium. Therefore, when subjected to plasma physical bombardment, the corrosion-resistant coating containing lanthanide metal elements has less energy loss due to inelastic collision and stronger resistance to plasma physical bombardment. At the same time, the electrons on the 4f orbit of lanthanide metal elements can shield the chemical action of external electrons, maintain the stable state of the atomic structure, and improve the resistance to plasma chemical corrosion. Since lanthanide metal elements are more resistant to plasma physical bombardment and chemical corrosion, when the coating containing lanthanide metal elements is applied to the surface of the component body, the stability of the plasma environment in the reaction chamber can be maintained, the generation of tiny particles during plasma etching can be reduced, and the requirements for tiny particles in advanced plasma etching processes (5nm and below) can be met.
[0072] The present invention adopts a compound of a rare earth metal element having similar chemical properties to yttrium as a corrosion-resistant coating material, which is more corrosion-resistant than yttrium-containing coatings. The XRD diffraction pattern of the corrosion-resistant coating of the present invention is composed of a main peak and a secondary peak whose intensity is at least 1 / 5 of the main peak intensity. The corrosion-resistant coating is a quasi-single crystal, which further enables the corrosion-resistant coating to have better resistance to physical bombardment and chemical corrosion than existing yttrium-containing coatings.
[0073] In the existing coating process, metal evaporation and oxidation are carried out in steps. The target metal is easily oxidized during the oxidation stage, which causes the target material to fail in the metal evaporation stage of the next cycle and fails to effectively evaporate metal molecules. At the same time, the evaporated metal vapor is mixed with oxidized molecules, which affects the effectiveness of the oxidation stage and makes it difficult to obtain the expected corrosion-resistant coating.
[0074] In order to form a corrosion-resistant coating with a single-crystal-like structure on a component body, the present invention also provides a coating device for forming the corrosion-resistant coating.
[0075] like Figure 4 As shown, a coating device for forming a corrosion-resistant coating of the present invention comprises:
[0076] A vacuum chamber 10;
[0077] A first electrode 20 is disposed on the top of the vacuum chamber 10 , and a metal target 01 is disposed below the first electrode 20 ;
[0078] The second electrode 30 is disposed in the vacuum chamber 10, and a workpiece 02 to be coated is disposed above the second electrode 30, and the workpiece 02 to be coated is disposed opposite to the metal target 01;
[0079] A shielding ring 40 is disposed in the vacuum chamber 10 and located between the first electrode 20 and the second electrode 30, and divides the vacuum chamber 10 into a first area 11 located above the shielding ring and a second area 12 located below the shielding ring. The shielding ring 40 includes an opening 41, and the opening 41 connects the first area 11 and the second area 12;
[0080] A first gas component 50 is used to input a first gas into the first region 11. The first gas forms a plasma 03 under the action of the first electrode 20 and the second electrode 30. The plasma 03 is used to bombard the metal target 01 to form metal vapor.
[0081] The second gas assembly 60 is used to deliver a second gas to the second area 12 , and the second gas reacts with metal vapor to form a corrosion-resistant coating on the surface of the workpiece 02 to be coated.
[0082] The shielding ring 40 separates the vacuum chamber 10, which can prevent the second gas from escaping to the first area and causing the second gas to contaminate the metal target 01, prevent the metal target 01 from being bombarded with metal vapor by the plasma 03 due to contamination, and improve the stability of the process. For example, the second gas is an oxygen-containing gas, which is easy to oxidize the metal target after escaping to the first area, which may reduce the excitation efficiency of the metal target. The metal vapor formed after excitation contains oxygen atoms, which leads to a decrease in the proportion of metal atoms, the accumulation of charges is destroyed, and the film cannot be formed on the surface of the workpiece 02 to be coated, and a single-crystal structure coating with good corrosion resistance cannot be formed. Furthermore, due to the introduction of the shielding ring 40, two relatively independent areas of metalization and chemical reaction are formed in the vacuum chamber 10, which can enable the deposition process to proceed continuously without interfering with each other, thereby improving the production efficiency of coating.
[0083] In some embodiments, a vacuum pump 70 may be provided to communicate with the second region 12. Turning on the vacuum pump 70 may make it easier for the metal vapor in the first region 11 to flow to the second region 12, and the second gas in the second region 12 may not easily escape to the first region 11 to contaminate the metal target 01. To achieve the above purpose, the vacuum pump 70 may be provided below the base of the second electrode 30 to extract as much as possible the second gas and / or metal vapor that cannot react on the surface of the workpiece 02 to form a coating, and to make the pressure of the second region 12 lower than that of the first region 11, thereby ensuring that the direction of the gas flow in the vacuum chamber 10 is always from the first region 11 to the second region 12 through the opening 41 of the shielding ring 40, and there will be no reverse flow of the second gas, thereby avoiding contamination of the metal target 01 by the second gas.
[0084] In this example, the second gas assembly 60 is disposed below the shielding ring 40 , and the second gas assembly 60 and the shielding ring 40 are disposed separately.
[0085] In some embodiments, the second gas assembly 60 is disposed in the shielding ring 40, such as Figure 5 shown.
[0086] In some embodiments, the projection area of the opening 41 of the shielding ring on the surface of the workpiece to be coated is greater than or equal to the area of the workpiece to be coated 02, so that the metal vapor flowing into the second area 12 through the opening 41 can completely and effectively cover the surface of the workpiece to be coated 02, and then fully react with the second gas to form a corrosion-resistant coating.
[0087] In some embodiments, the shielding ring 40 is connected to the inner wall of the vacuum chamber 10 so that there is no gap between the shielding ring 40 and the inner wall of the vacuum chamber 10. In this way, on the one hand, the shielding ring 40 is fixed, and on the other hand, the second gas in the second area 12 can be effectively prevented from escaping to the first area 11 through the gap between the shielding ring 40 and the inner wall of the vacuum chamber 10.
[0088] In some embodiments, the material of the shielding ring includes at least one of oxide ceramics, nitride ceramics, silicon, SiC, quartz, etc.
[0089] like Figure 6 As shown, the method for preparing parts of a plasma reaction device using the coating device for forming a corrosion-resistant coating of the present invention comprises:
[0090] Step S1, providing a coating device for forming a corrosion-resistant coating;
[0091] Step S2, providing a metal target and placing it below the first electrode;
[0092] Step S3, providing a component body as a workpiece to be coated, and placing it on the second electrode;
[0093] Step S4, introducing a first gas into the first region, the first gas forms plasma under the action of the first electrode and the second electrode, and the plasma excites the metal target to form metal vapor;
[0094] Step S5, introducing a second gas into the second area;
[0095] The metal vapor enters the second area through the opening of the shielding ring, and chemically reacts with the second gas to form a corrosion-resistant coating on the surface of the workpiece to be coated.
[0096] The atomic radius of the metal element in the metal target is smaller than the atomic radius of yttrium (Y), and the relative atomic mass is greater than the relative atomic mass of yttrium. The metal element has similar chemical stability properties to the Y element, but is more resistant to plasma physical bombardment. The metal element can be selected from rare earth metal elements, including at least one of holmium (Ho), erbium (Er,), thulium (Tm), ytterbium (Yb), and lutetium (Lu). The corrosion-resistant coating formed by the above-mentioned metal target is a rare earth metal compound, and the rare earth metal compound includes at least one of an oxide, a fluoride, and a fluoride oxide of a rare earth metal element.
[0097] The first gas can be selected from at least one of inert gases such as He, Ne, Ar, and Xe.
[0098] The second gas includes an oxygen-containing gas and / or a fluorine-containing gas.
[0099] In some embodiments, the oxygen-containing gas includes at least one of oxygen, ozone, and oxygen-enriched air.
[0100] In some embodiments, the fluorine-containing gas includes HF or fluorine-substituted alkanes. The general formula of the fluorine-substituted alkanes is C x H y F z , wherein x is 1-5, y≥0, z>0, for example, it can be at least one of CH2F2, CF4, C4F6, C4F8, CHF3, CH3F, etc.
[0101] The corrosion-resistant coating can be prepared by using a coating device, and the atomic radius of the metal element in the corrosion-resistant coating is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium; the diffraction peak of the corrosion-resistant coating obtained by X-ray diffraction consists of a main peak and a secondary peak whose intensity is at least 1 / 5 less than the main peak intensity; the half-peak width of the main peak is less than 1°, that is, a single-crystal-like coating can be formed by using a coating device, and the principle includes: because the material of the target material is metal, and the metal atoms excited by the plasma of the metal target material 01 are the same size, there is no obvious orientation difference between the metal atoms, and the binding positions (minimum binding energy active sites) of the metal atoms and the second gas molecules are relatively consistent, so that the orientations of the molecular flows formed by the reaction are relatively consistent. In addition, the distance between the metal target and the workpiece 02 to be coated is relatively close, so that the molecular flow is not easily deflected and collided when reaching the surface of the workpiece 02 to be coated, resulting in orientation differences. At the same time, due to the high energy of the excited molecular flow, it directly bonds with the molecules on the surface of the parts to reduce the probability of surface migration and maintain consistent crystallographic orientation. Therefore, the corrosion-resistant coating formed on the surface of the workpiece 02 to be coated presents a single-crystal structure, and the corrosion-resistant coating has better resistance to physical bombardment and chemical corrosion.
[0102] Example
[0103] use Figure 4 The coating device is used to prepare a focusing ring of a plasma reaction device. In the coating device, the RF source power output is 1000W, and the RF bias power output is 500W. The Yb metal target is placed below the first electrode 20; the focusing ring is placed on the second electrode 30 of the coating device, and the vacuum chamber 10 is evacuated to 5×10 -2Pa or less. A first gas Ar is introduced into the first region 11, and the flow rate of the first gas is 10 sccm. Turn on the RF source power source to form a plasma with the first gas; turn on the RF bias power source to bombard the metal target with the plasma to form Yb metal vapor. Ozone is introduced into the second region 12 as the second gas. The flow rate of the second gas is 30 sccm. Turn on the vacuum pump 70 to extract the gas under the base of the second electrode 30, so that the gas pressure in the second region 12 remains lower than the gas pressure in the first region 11, so as to ensure that the flow direction of the gas in the vacuum chamber 10 is always from the first region 11 to the second region 12 through the opening 41 of the shielding ring. In the vacuum chamber 10, Yb metal vapor enters the second region 12 through the opening 41 of the shielding ring, reacts chemically with ozone, and forms a corrosion-resistant coating Yb2O3 on the surface of the focusing ring. After 1800 seconds, the RF power source, RF bias power source, second gas assembly 60, first gas assembly 50 and vacuum pump 70 are successively turned off, and the focusing ring with the Yb2O3 corrosion-resistant coating is taken out. The spectrum of the corrosion-resistant coating on the surface of the focusing ring measured by X-ray powder diffraction is as follows: Figure 7 As shown, it has the main diffraction peak of the (440) plane of Yb2O3, the secondary strongest diffraction peak of the (433) plane, and the third strongest diffraction peak of the (222) plane. The intensity of the main diffraction peak (440) is 15 times that of the secondary strongest diffraction peak (433), and the intensity of the main diffraction peak (440) is 35 times that of the third diffraction peak (222). The half-peak width of the main diffraction peak of the (440) plane is 0.2°, showing a crystallization performance similar to that of a single crystal (within 1° of the half-peak width). Since the corrosion resistance of the coating is the average result of the corrosion resistance of each crystal plane, compared with the polycrystalline coating, the coating with a single-crystal structure has a highly consistent crystal orientation of the grains, and its corrosion resistance is improved with the corrosion resistance of the main crystal plane.
[0104] In summary, the present invention selects compounds of rare earth metal elements with smaller atomic radius and larger relative atomic mass than yttrium as corrosion-resistant coatings for parts of plasma reaction devices, which are more resistant to plasma physical bombardment and chemical corrosion than yttrium-containing coatings. In addition, by arranging a shielding ring in the coating device, the metallization step and the chemical reaction step (oxidation or fluorination) are carried out in independent spaces, which is not easy to contaminate the metal target material. The formed corrosion-resistant coating has a single-crystal structure, and the resistance to plasma bombardment and chemical corrosion is further enhanced, which is suitable for the development needs of semiconductor processes.
[0105] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A coating device for forming a corrosion-resistant coating, characterized in that: include: Vacuum chamber; A first electrode is disposed on the top of the vacuum chamber, and a metal target is disposed below the first electrode; A second electrode is disposed in the vacuum chamber, a workpiece to be coated is disposed above the second electrode, and the workpiece to be coated is disposed opposite to the metal target; A shielding ring is disposed in the vacuum chamber and between the first electrode and the second electrode, and divides the vacuum chamber into a first area above the shielding ring and a second area below the shielding ring, and includes an opening, and the opening connects the first area and the second area; A first gas component is used to input a first gas into the first region, the first gas forms plasma under the action of the first electrode and the second electrode, and the plasma is used to bombard the metal target material to form metal vapor; The second gas component is used to deliver a second gas to the second area, and the second gas reacts with the metal vapor to form a corrosion-resistant coating on the surface of the workpiece to be coated.
2. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: Also includes: A vacuum pump is used to allow the airflow to flow from the first area to the second area and then be drawn out of the vacuum cavity.
3. The coating device for forming a corrosion-resistant coating according to claim 2, characterized in that: The vacuum pump is disposed below the base of the second electrode and is communicated with the second region.
4. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: The second gas component is arranged below the shielding ring, and the second gas component is arranged separately from the shielding ring.
5. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: The second gas assembly is disposed in the shielding ring.
6. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: The projection area of the opening of the shielding ring on the surface of the workpiece to be coated is greater than or equal to the area of the workpiece to be coated.
7. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: The shielding ring is connected to the inner wall of the vacuum chamber.
8. The coating device for forming a corrosion-resistant coating according to claim 1, characterized in that: The material of the shielding ring includes at least one of oxide ceramics, nitride ceramics, silicon, SiC, and quartz.
9. A method for forming a corrosion-resistant coating on the surface of a component body, characterized in that: include: Providing a coating device for forming a corrosion-resistant coating as described in any one of claims 1 to 8; Providing a metal target and placing it below the first electrode; Providing a component body as a workpiece to be coated, and placing it on the second electrode; A first gas is introduced into the first region, the first gas forms plasma under the action of the first electrode and the second electrode, and the plasma excites the metal target to form metal vapor; introducing a second gas into the second region; The metal vapor enters the second region through the opening of the shielding ring, and chemically reacts with the second gas to form a corrosion-resistant coating on the surface of the workpiece to be coated.
10. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 9, characterized in that: The atomic radius of the metal element in the metal target material is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium.
11. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 10, characterized in that: The metal element includes at least one of Ho, Er, Tm, Yb, and Lu.
12. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 9, characterized in that: The first gas is an inert gas, including at least one of He, Ne, Ar, and Xe.
13. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 9, characterized in that: The second gas includes an oxygen-containing gas and / or a fluorine-containing gas.
14. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 13, characterized in that: The oxygen-containing gas includes at least one of oxygen, ozone and oxygen-enriched air.
15. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 13, characterized in that: The fluorine-containing gas includes HF or fluorine-substituted alkane.
16. The method for forming a corrosion-resistant coating on the surface of a component body according to claim 15, characterized in that: The general formula of the fluorine-substituted alkane is C x H y F z , where x is 1-5, y≥0, and z>0.
17. A component of a plasma reaction device, characterized in that: This component contains: Component body; A corrosion-resistant coating formed on the component body by the method for forming a corrosion-resistant coating on the surface of a component body according to any one of claims 9 to 16; The atomic radius of the metal element in the corrosion-resistant coating is smaller than the atomic radius of yttrium, and the relative atomic mass is greater than the relative atomic mass of yttrium; the diffraction peak of the corrosion-resistant coating obtained by X-ray diffraction consists of a main peak and a secondary peak with an intensity at least 1 / 5 less than the main peak intensity; the half-peak width of the main peak is less than 1°.
18. The component of the plasma reaction device according to claim 17, characterized in that: The corrosion-resistant coating is a rare earth metal compound, which includes at least one of oxides, fluorides, and fluoride oxides of rare earth metal elements, and the rare earth metal elements include at least one of Ho, Er, Tm, Yb, and Lu.
19. The component of the plasma reaction device according to claim 17, characterized in that: The intensity ratio of the secondary peak to the main peak is less than 1 / 10, and the half-peak width of the main peak is less than 0.5°.
20. The component of the plasma reaction device according to claim 17, characterized in that: The thickness of the corrosion-resistant coating ranges from 0.1um to 1000um.
21. A plasma reaction device, characterized in that: include: A reaction chamber, wherein the reaction chamber is a plasma environment; A component of a plasma reaction device according to any one of claims 17 to 20, wherein the component is exposed to the plasma environment.
22. The plasma reaction device according to claim 21, characterized in that: The plasma reaction device is an inductively coupled plasma reaction device; The components include: at least one of a ceramic cover plate, a bushing, a gas nozzle, a gas connection flange, a focusing ring, an insulating ring, an electrostatic chuck, a cover ring or a plasma confinement device.
23. The plasma reaction device according to claim 21, characterized in that: The plasma reaction device is a capacitively coupled plasma reaction device; The components include: at least one of a gas shower head, a gasket, a nozzle, a gas distribution plate, an electrostatic chuck, a plasma confinement device, a focusing ring, an insulating ring, and a covering ring.