Preparation device and process of heavy metal adsorption guar gum coated bacterial agent composite material
By using guar gum coated bacterial agent composite materials in heavy metal contaminated soil, the problem of poor stability of existing adsorbent materials is solved, and the significant repair effect of heavy metal contaminated soil is achieved. Through ultrasonic-ultraviolet light treatment and fluidized bed wrapping technology , forming efficient coating materials, solving the problem of heavy metal contaminated soil repair.
Patent Information
- Application Number
- CN202211298639.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-21
AI Technical Summary
The adsorption effect of existing adsorption materials on heavy metals is not significant and have poor stability, making it difficult to effectively repair heavy metal contaminated soil.
Using heavy metal adsorption guar gum coated bacteria composite material, the guar gum is homogenized and refined by ultrasonic-ultraviolet coupling treatment to enhance its surfactivity, and diatomaceous earth is mixed with citric acid, sodium bicarbonate, and linoleic acid. To form a coating material, use a fluidized bed to wrap the activated bacteria agent, and perform cold air drying and ultraviolet light irradiation to improve adsorption effect and stability.
It significantly improves the repair effect of heavy metal contaminated soil. The coating material is stable before use, is easy to promote and apply, and can effectively adsorb and release bacterial agents during use, significantly improving the soil repair effect.
Smart Images

Figure CN115651811B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental protection, and in particular to a preparation device and process for a heavy metal adsorbed guar gum coated bacterial agent composite material. Background Art
[0002] Heavy metal pollution is one of the biggest environmental problems in soil pollution today, with its serious hazards and wide pollution area. The discharge of three wastes from industries such as electronics, electroplating, chemical industry and leather making, the mining and smelting of minerals, the application of pesticides and fertilizers, the discharge of domestic waste generated in cities, sewage irrigation and the application of sludge in agriculture are the main sources of heavy metal pollution in soil. The heavy metals in heavy metal-contaminated soil mainly include Co, As, Cr, Hg, Mn, Ni, Pb, Cd, Cu, Zn, etc. Most of them are complex pollution of several heavy metals. Due to the rapid development of China's industry, the discharge of three wastes has also increased dramatically, and heavy metal pollution in China's soil has become more and more serious. The national sewage irrigation area survey organized by the Ministry of Agriculture shows that China now has a sewage irrigation area of approximately 1.4 million hm2. 2 , of which 64.8% of the total area of sewage irrigation is land polluted by heavy metals, 46.7% of the area is slightly polluted, 9.7% of the area is moderately polluted, and 8.4% of the area is seriously polluted. The area polluted by heavy metals cadmium and mercury accounts for the largest proportion. In some areas, heavy metal pollution has reached a very serious level.
[0003] Heavy metal contaminated soil causes harm to the environment through the following channels: (1) Under the leaching effect of rainwater, heavy metals in the soil penetrate downward and enter the groundwater, which is very likely to cause heavy metal pollution in the groundwater; (2) Soil contaminated by heavy metals is in direct contact with the environment, and humans and animals may absorb soil particles directly or indirectly; (3) When external environmental conditions change, the bioavailability of heavy metals in the soil is also improved. At this time, plants can more easily absorb and utilize heavy metals, which allows heavy metals to enter the food chain and cause heavy metal poisoning to various organisms in the food chain. The same heavy metal has many different forms in the soil. Depending on the form, its migration and transformation characteristics, pollution properties, and degree of harm are different. The difference between soil heavy metal pollution and organic pollutants is that the heavy metals in the soil are biodegradable and relatively stable, making it difficult to remediate heavy metal contaminated soil. In addition, the stability of current adsorption materials is poor, and the adsorption effect on heavy metals is not significant. Summary of the invention
[0004] The object of the present invention is to provide a preparation device and a preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A preparation device for a heavy metal adsorbed guar gum coated bacterial agent composite material, comprising a box body, a working chamber is provided in the box body, a placement plate and a processing component are provided in the working chamber, placement holes are symmetrically provided on the placement plate, two placement holes are provided with matching test tubes, the placement plate is connected to an execution end of the processing component, the processing component is composed of a shaking component, a cleaning component and a dumping component, and a collection component for collecting waste liquid is provided inside the box body below the processing component;
[0007] The shaking assembly includes an inverted L-shaped plate, the bottom end of the L-shaped plate is connected to the placement plate through a dumping assembly, a moving plate is provided between the top plate of the L-shaped plate and the placement plate, and the cleaning assembly is provided on the moving plate;
[0008] The cleaning component includes through holes symmetrically opened on the movable plate, two of the through holes are provided with water spray barrels, the top ends of the two water spray barrels are connected to the fixed plate through a rotating component, a second electric telescopic rod is installed on one side of the lower surface of the movable plate, and the telescopic end of the second electric telescopic rod passes through the movable plate and is fixedly connected to the fixed plate.
[0009] Preferably, a driving motor is provided on one side of the top of the box, the driving motor is installed in a protective shell, the output end of the driving motor passes through the top wall of the box and is fixedly connected to the top plate of the L-shaped plate, a first electric telescopic rod is provided on one side of the cleaning assembly above the movable plate, the first electric telescopic rod is fixedly connected to the lower surface of the top plate of the L-shaped plate, and the telescopic end of the first electric telescopic rod is connected to the upper surface of the movable plate, and a distance sensor is installed inside the lower surface of the movable plate. In this preferred embodiment, the driving motor, the first electric telescopic rod and the movable plate can prevent the test tube from being thrown out when the test tube is centrifugally shaken.
[0010] Preferably, the rotating assembly includes a rotating shaft fixedly connected to the top ends of the two water spray barrels, the two rotating shafts are rotatably connected to the lower surface of the fixing plate, a rotating motor is installed at the center of the lower surface of the fixing plate by bolts, a driving wheel is fixedly installed at the output end of the rotating motor, and driven wheels are fixedly sleeved on the two rotating shafts, and the driving wheel and the two driven wheels are connected by a transmission belt. In this preferred embodiment, the two water spray barrels can be rotated by the rotating assembly.
[0011] Preferably, the bottom ends of the two water spray barrels are flush with the lower surface of the movable plate, a disinfection water tank is welded on the other side of the top of the box, a water pump is installed inside the disinfection water tank, the output port of the water pump is connected to a water pipe through a pipeline, the lower surface of the water pipe is symmetrically connected to a telescopic hose, one end of the two telescopic hoses passes through the top wall of the box, the top plate of the L-shaped plate, the fixed plate and the rotating shaft in the rotating assembly in sequence and is inserted into the water spray barrel, the upper surface of the movable plate away from the second electric telescopic rod is fixedly connected with a vertical guide rod, and the guide rod passes through the fixed plate. In this preferred embodiment, the disinfection water in the disinfection water tank can be sprayed out from the water spray barrel to facilitate washing the inner wall of the test tube.
[0012] Preferably, the outer walls of the two water spray barrels are provided with brushes, and the diameters of the two water spray barrels are smaller than the diameter of the test tube. In this preferred embodiment, the water spray barrel is convenient for inserting into the test tube and cleaning the inner wall of the test tube by the brush.
[0013] Preferably, the dumping assembly includes a U-shaped groove opened at the bottom of the L-shaped plate, the two side ends of the placement plate are movably connected to the inner wall of the U-shaped groove through a welded rotating shaft, and the outer wall of the bottom end of the L-shaped plate is installed with a flip motor through bolts, and the output end of the flip motor is fixedly connected to the rotating shaft. In this preferred embodiment, the dumping assembly is used to facilitate pouring out and draining the remaining water in the test tube after cleaning.
[0014] Preferably, the collection assembly includes a collection chamber opened inside the box, a funnel is connected above the collection chamber, the funnel is embedded in the bottom plate of the working chamber, a drainage pipe is provided at the bottom of one side of the box, the drainage pipe is communicated with the collection chamber, and a valve is installed on the drainage pipe. In this preferred embodiment, the collection assembly is used to facilitate the collection of water poured out of the test tube.
[0015] According to the technical scheme of the above-mentioned device for preparing a heavy metal adsorbing guar gum coated bacterial agent composite material, a preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material is also provided, comprising the following steps:
[0016] According to the technical scheme of the above-mentioned device for preparing a heavy metal adsorbing guar gum coated bacterial agent composite material, a preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material is also provided, comprising the following steps:
[0017] Step 1: Bacterial agent activation treatment:
[0018] The bacterial agents are placed in a microbial culture medium box for shaking and activation, and then centrifuged and the precipitate is cryogenically crushed;
[0019] Step 2: Preparation of coating material guar gum:
[0020] The first step is to place the guar gum in an ultrasonic-ultraviolet light coupling environment for treatment, and take it out for use after completion; the second step is to place the diatomaceous earth in a cold plasma treatment device for cold plasma treatment, and take it out for use after completion; the third step is to weigh 55-65 parts of the guar gum treated in the first step, 12-18 parts of the diatomaceous earth treated in the second step, 5-7 parts of citric acid, 5-7 parts of sodium bicarbonate, and 3-6 parts of linoleic acid in corresponding weight parts, mix them evenly, and then perform deep cold crushing treatment;
[0021] Step 3: Package processing:
[0022] The microbial agent after deep cold crushing treatment in step 1 is suspended in the air by using a fluidized bed, and then the coating material obtained in step 2 is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying treatment is performed to obtain the coating material for use;
[0023] Step 4: UV irradiation treatment:
[0024] The coating material obtained in step 3 is placed in an ultraviolet environment for ultraviolet light irradiation treatment.
[0025] Preferably, the bacterial agent in step 1 is at least one of filamentous fungi, bacteria or yeast.
[0026] Preferably, the coating material in step 2 is guar gum, wherein the ultrasound-ultraviolet light coupling environment in the first step is an ultrasound frequency of 40-100kHz, an ultraviolet light wavelength of 200-400nm, and a treatment time of 20-24min, and the cold plasma treatment in the second step is controlled to have a treatment power of 200-400W, a vacuum degree of 40-50Pa during discharge, a gas flow rate of 1-2L / min, and a treatment time of 3-7min;
[0027] During the ultraviolet light irradiation treatment in step 4, the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 20-30 cm, and the treatment time is 1-2 hours.
[0028] The bacterial agent is subjected to a shaking activation treatment, mainly to purify the bacterial agent, remove dead strains, and increase the proportion of live bacteria. The coating material provided in the present application utilizes the principle of effervescence, matches an acid source and an alkali source and mixes them with guar gum, etc., to make a coating material with a coating and water-disintegrating effect. However, when it is used for the coating of the bacterial agent, the stability of the performance of the bacterial agent can be guaranteed. When the composite material is used, the acid source and the carbon source react, and the release of the bacterial agent can be promoted, thereby playing the effect of repairing the soil. Guar gum is a plant gum extracted from melon beans, a leguminous plant planted in the Indian subcontinent. It is polygalactose mannose in chemical composition.
[0029] Due to its unique molecular structure and physicochemical properties, guar gum is not water-resistant because it grows in a high temperature, drought and water-deficient environment, so it can be hydrated and dissolved in cold water. This is a great advantage compared to the starch series additives that need to be gelatinized before use. Another feature of guar gum is that its molecular structure is very similar to that of cellulose molecules. The mannose units in the guar gum molecules are connected to form the main chain through 1,4-B glycosidic bonds, and the galactose side chains are connected to the mannose main chain at intervals of 1,6a bonds. The similarity with cellulose molecules makes it easy to adsorb to the fiber to produce retention, filtration and enhancement effects. And the molecular weight is not high, so it will not produce excessive flocculation. This application utilizes the molecular structure and physicochemical properties of guar gum, mainly using it to form a film material, which is used for the curing agent matrix component, but directly using it to prepare the coating material will make the inclusions unable to be released and the effect of heavy metal adsorption cannot be achieved.
[0030] Therefore, the coating material of the present application is not prepared by a single component guar gum, but the guar gum is placed in an ultrasonic-ultraviolet light coupling environment for treatment, and the acoustic flow effect, cavitation effect, thermal effect, etc. of the ultrasonic wave and the light wave effect of the ultraviolet light cooperate with each other, on the one hand, the guar gum is homogenized and refined, and on the other hand, its surface activity is enhanced and its processing characteristics are improved;
[0031] Diatomaceous earth has the function of adsorbing heavy metals. The adsorption effect of using only diatomaceous earth is general. Therefore, the present application also uses diatomaceous earth as a raw material for coating materials. On the one hand, it can adsorb heavy metals. On the other hand, it improves the film characteristics of diatomaceous earth and improves the release effect of bacterial agents. The present application places diatomaceous earth in a cold plasma treatment device for treatment, mainly to enhance the surface activity of diatomaceous earth, increase the specific surface area, and enhance its adsorption effect on heavy metals. The treated guar gum and diatomaceous earth are mixed with citric acid, sodium bicarbonate, and linoleic acid, and then crushed to make a homogeneous and refined special coating material. This material is coated on the surface of the activated biological strain using a fluidized bed, which can not only adsorb heavy metals, but also protect the bacterial agent. Finally, ultraviolet curing treatment is performed, mainly using the effect of ultraviolet light to sterilize the coating body, thereby further improving the quality of the composite material.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] After the bacterial agent is activated, a special coating material is coated on the surface of the activated bacterial agent. When it is used for soil remediation contaminated by heavy metals, the composite material absorbs moisture in the soil, disintegrates, and the bacterial agent is released to repair the soil, and the repair effect is significant. In addition, the composite material prepared by the method of the present application has stable performance and is easy to promote and apply because the bacterial agent is coated before use. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a three-dimensional diagram of the overall structure of the present invention;
[0035] Figure 2 It is the overall front cross-sectional view of the present invention;
[0036] Figure 3 It is a front view of the processing component of the present invention;
[0037] Figure 4 A three-dimensional diagram of the processing component of the present invention;
[0038] Figure 5 It is a schematic diagram of the structure of the rotating assembly of the present invention;
[0039] Figure 6 This is a top sectional view of the disinfection water tank of the present invention.
[0040] In the figure: 1, box body; 101, working chamber; 102, processing component; 103, placement plate; 1031, placement hole; 1032, test tube; 2, shaking component; 201, driving motor; 2011, protective shell; 202, L-shaped plate; 203, first electric telescopic rod; 204, moving plate; 2041, distance sensor; 3, cleaning component; 301, through hole; 302, water sprayer; 3021, brush; 303, telescopic hose; 304, Disinfection water tank; 305, water pump; 306, water guide pipe; 307, second electric telescopic rod; 308, guide rod; 309, fixed plate; 4, rotating component; 401, rotating motor; 402, driving wheel; 403, rotating shaft; 404, driven wheel; 405, transmission belt; 5, dumping component; 501, U-shaped groove; 502, flipping motor; 6, collecting component; 601, collecting chamber; 602, funnel; 603, drain pipe; 6031, valve. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0042] In order to facilitate understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0043] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0045] A control panel is installed on the front of the box 1 in the device, and the control panel is electrically connected to the electrical components in the device through wires.
[0046] Please refer to Figures 1 to 6 , the present invention provides a technical solution:
[0047] A preparation device for a heavy metal adsorbing guar gum coated bacterial agent composite material comprises a box body 1, a working chamber 101 is provided in the box body 1, a placement plate 103 and a processing component 102 are provided in the working chamber 101. The placement plate 103 is symmetrically provided with placement holes 1031, two placement holes 1031 are provided with matching test tubes 1032, and the placement plate 103 is connected to the execution end of the processing component 102;
[0048] The processing component 102 is composed of a shaking component 2, a cleaning component 3 and a dumping component 5. A collection component 6 for collecting waste liquid is provided inside the box 1 below the processing component 102. The shaking component 2 includes an inverted L-shaped plate 202, and the bottom end of the L-shaped plate 202 is connected to the placement plate 103 through the dumping component 5. A moving plate 204 is provided between the top plate of the L-shaped plate 202 and the placement plate 103, and the cleaning component 3 is provided on the moving plate 204. A driving motor 201 is provided on one side of the top of the box 1;
[0049] The driving motor 201 is installed in the protective shell 2011, and the output end of the driving motor 201 passes through the top wall of the box body 1 and is fixedly connected to the top plate of the L-shaped plate 202. A first electric telescopic rod 203 is provided on one side of the cleaning component 3 above the movable plate 204. The first electric telescopic rod 203 is fixedly connected to the lower surface of the top plate of the L-shaped plate 202, and the telescopic end of the first electric telescopic rod 203 is connected to the upper surface of the movable plate 204. A distance sensor 2041 is installed inside the lower surface of the movable plate 204.
[0050] When activating the bacterial agent, the bacterial agent is placed in the test tube 1032 in the device and sealed by the sealing cover, and then the test tube 1032 is placed in the placement hole 1031 in the placement plate 103. The staff starts the shaking component 2 through the control panel to move the moving plate 204 downward to press the top of the test tube 1032, and then the placement plate 103 rotates under the operation of the shaking component 2, thereby realizing the shaking bacteria activation treatment and increasing the proportion of live bacteria. Then, the test tube 1032 is removed to take out the bacterial agent for subsequent operations;
[0051] Furthermore, the first electric telescopic rod 203 drives the movable plate 204 to move downward, and the distance sensor 2041 detects the distance to the upper surface of the placement plate 103 and transmits the data to the control panel for analysis and processing until the set value is reached, so as to avoid damage to the test tube caused by excessive pressure on the movable plate 204;
[0052] Furthermore, the driving motor 201 drives the L-shaped plate 202 to rotate, and the rotating L-shaped plate 202 drives the connected placement plate 103 to rotate, and the rotating placement plate 103 causes the bacterial agent in the test tube 1032 to undergo a vibration activation treatment.
[0053] Please refer to Figures 2 to 6 The bottom ends of the two water spray barrels 302 are flush with the lower surface of the movable plate 204, a disinfection water tank 304 is welded on the other side of the top of the box body 1, a water pump 305 is installed inside the disinfection water tank 304, the output port of the water pump 305 is connected to a water pipe 306 through a pipeline, and the lower surface of the water pipe 306 is symmetrically connected to a telescopic hose 303, one end of the two telescopic hoses 303 are successively inserted through the top wall of the box body 1, the top plate of the L-shaped plate 202, the fixed plate 309 and the rotating shaft 403 in the rotating component 4 into the water spray barrel 302;
[0054] A vertical guide rod 308 is fixedly connected to the upper surface of the movable plate 204 away from the second electric telescopic rod 307, and the guide rod 308 passes through the fixed plate 309. The outer walls of the two water spray barrels 302 are both provided with brushes 3021, and the diameters of the two water spray barrels 302 are smaller than the diameter of the test tube 1032;
[0055] The rotating assembly 4 includes a rotating shaft 403 fixedly connected to the top of the two water spray barrels 302, and the two rotating shafts 403 are both rotatably connected to the lower surface of the fixed plate 309. A rotating motor 401 is installed at the center of the lower surface of the fixed plate 309 by bolts. A driving wheel 402 is fixedly installed at the output end of the rotating motor 401. A driven wheel 404 is fixedly sleeved on the two rotating shafts 403. The driving wheel 402 and the two driven wheels 404 are connected by a transmission belt 405.
[0056] The tipping assembly 5 includes a U-shaped groove 501 opened at the bottom end of the L-shaped plate 202. The two side ends of the placement plate 103 are movably connected to the inner wall of the U-shaped groove 501 through a welded rotating shaft. The outer wall of the bottom end of the L-shaped plate 202 is installed with a flip motor 502 by bolts, and the output end of the flip motor 502 is fixedly connected to the rotating shaft.
[0057] After the bacterial agent in the test tube 1032 is taken out, the test tube 1032 is put in place, and the shaking component 2 and the cleaning component 3 are started in sequence through the control panel. The shaking component 2 continues to press the top of the test tube 1032, and the cleaning component 3 works to move the water spray barrel 302 downward, and the water spray barrel 302 moves into the test tube 1032 and sprays the disinfectant. Under the operation of the rotating component 4, the inside of the test tube 1032 can be sterilized and cleaned. After a period of time, the shaking component 2 and the cleaning component 3 are reset, and the pouring component 5 works to flip the placement plate 103 by 90 degrees, so that the test tube 1032 is horizontal and the remaining water is poured out, thereby realizing automatic cleaning of the test tube 1032 after use, which is simple and convenient to operate and does not require manual cleaning;
[0058] Furthermore, the first electric telescopic rod 203 in the shaking assembly 2 works to drive the moving plate 204 to move downward;
[0059] Furthermore, the second electric telescopic rod 307 in the cleaning assembly 3 drives the fixed plate 309 to move downward, and the downwardly moved fixed plate 309 causes the two water spray barrels 302 to move downward, and the downwardly moved water spray barrels 302 are inserted into the test tube 1032. At this time, the water pump 305 works to send the disinfectant in the disinfection water tank 304 into the water spray barrels 302 through the telescopic hose 303 and spray it out;
[0060] Furthermore, after the shaking component 2 and the cleaning component 2 are reset, the flip motor 502 in the dumping component 5 starts working, and the output end of the flip motor 502 rotates to drive the connected placement plate 103 to rotate along the U-shaped groove 501, and then dumps.
[0061] Please refer to Figure 1 and Figure 2 The collecting assembly 6 includes a collecting chamber 601 opened inside the box body 1, a funnel 602 is connected to the top of the collecting chamber 601, the funnel 602 is embedded in the bottom plate of the working chamber 101, a drain pipe 603 is provided at the bottom of one side of the box body 1, the drain pipe 603 is communicated with the collecting chamber 601, and a valve 6031 is installed on the drain pipe 603.
[0062] When pouring, the water poured out from the test tube 1032 enters the collection chamber 601 through the funnel 602 for storage, and the waste water in the collection chamber 601 can be discharged from the drain pipe 603 by opening the valve 6031.
[0063] According to the above embodiment of the device for preparing a heavy metal adsorbing guar gum coated bacterial agent composite material, a preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material is also provided, comprising the following steps:
[0064] Step 1: Activation of bacterial agents: Place the bacterial agents in the microbial culture medium box 1 for shaking and activation, centrifuge after completion, and perform deep-cold crushing on the precipitate;
[0065] Step 2, preparation of coating material guar gum: first, placing guar gum in an ultrasonic-ultraviolet light coupling environment for treatment, and taking it out for use after completion; second, placing diatomaceous earth in a cold plasma treatment device for cold plasma treatment, and taking it out for use after completion; third, weighing 55-65 parts of guar gum treated in the first step, 12-18 parts of diatomaceous earth treated in the second step, 5-7 parts of citric acid, 5-7 parts of sodium bicarbonate, and 3-6 parts of linoleic acid in corresponding weight parts, mixing them evenly, and then performing deep cold crushing treatment;
[0066] Step 3, coating treatment: using a fluidized bed to suspend the microbial agent after deep-cold crushing treatment in step 1 in the air, and then adding the coating material obtained in step 2 to the fluidized bed in the form of spray, coating the microbial agent in a suspended and rolling state, and then performing cold air drying treatment to obtain the coating material for use;
[0067] Step 4: UV irradiation treatment: placing the coating material obtained in step 3 in a UV environment for UV irradiation treatment.
[0068] In step 1, the bacterial agent is at least one of filamentous fungi, bacteria, and yeast.
[0069] In step 2, the coating material is guar gum, wherein the ultrasound-ultraviolet light coupling environment in the first step is an ultrasound frequency of 40-100kHz, an ultraviolet light wavelength of 200-400nm, and a treatment time of 20-24min, and in the second step, the cold plasma treatment is controlled to have a treatment power of 200-400W, a vacuum degree of 40-50Pa during discharge, a gas flow rate of 1-2L / min, and a treatment time of 3-7min;
[0070] In step 4, during the ultraviolet light irradiation treatment, the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 20-30 cm, and the treatment time is 1-2 hours.
[0071] In order to further explain the present invention, it is described below in conjunction with the following specific embodiments.
[0072] Process 1
[0073] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0074] (1) Bacterial agent activation treatment:
[0075] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0076] (2) Preparation of coating material guar gum:
[0077] A. Place guar gum in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 40kHz and an ultraviolet light wavelength of 200nm, and take it out after treatment for 20 minutes for later use;
[0078] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 200W, a vacuum degree of 40Pa during discharge, a gas flow rate of 1L / min, and taking it out for use after treatment for 3min;
[0079] C. Weigh corresponding weight portions of 55 parts of guar gum treated in operation A, 12 parts of diatomaceous earth treated in operation B, 5 parts of citric acid, 5 parts of sodium bicarbonate, and 3 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0080] (3) Packet processing:
[0081] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0082] (4) Ultraviolet light treatment:
[0083] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 20 cm, and the treatment time is 1 hour.
[0084] Process 2
[0085] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0086] (1) Bacterial agent activation treatment:
[0087] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0088] (2) Preparation of coating material guar gum:
[0089] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After the treatment for 22 minutes, the guar gum was taken out for use;
[0090] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0091] C. Weigh corresponding weight portions of 60 parts of guar gum treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0092] (3) Packet processing:
[0093] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0094] (4) Ultraviolet light treatment:
[0095] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0096] Process three
[0097] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0098] (1) Bacterial agent activation treatment:
[0099] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0100] (2) Preparation of coating material guar gum:
[0101] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 100 kHz and an ultraviolet light wavelength of 400 nm. After the treatment for 24 minutes, the guar gum was taken out for use;
[0102] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 400W, a vacuum degree of 50Pa during discharge, a gas flow rate of 2L / min, and taking it out for use after 7 minutes of treatment;
[0103] C. Weigh corresponding weight portions of 65 parts of guar gum treated in operation A, 18 parts of diatomaceous earth treated in operation B, 7 parts of citric acid, 7 parts of sodium bicarbonate, and 6 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0104] (3) Packet processing:
[0105] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0106] (4) Ultraviolet light treatment:
[0107] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 30 cm, and the treatment time is 2 hours.
[0108] Process Four
[0109] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0110] (1) Preparation of coating material guar gum:
[0111] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After the treatment for 22 minutes, the guar gum was taken out for use;
[0112] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0113] C. Weigh corresponding weight portions of 60 parts of guar gum treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0114] (2) Packet processing:
[0115] The bacterial agent is suspended in the air using a fluidized bed, and then the coating material obtained in step (1) is added to the fluidized bed in the form of a spray, and the bacterial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0116] (3) Ultraviolet light treatment:
[0117] The coating material obtained in step (2) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 hours.
[0118] Process Five
[0119] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0120] (1) Bacterial agent activation treatment:
[0121] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0122] (2) Preparation of coating material guar gum:
[0123] A. Place the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, and a gas flow rate of 1.5L / min. After 5 minutes of treatment, take it out for use;
[0124] B. Weigh 60 parts of guar gum, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid in corresponding weight parts, mix well, and then perform deep cold crushing treatment;
[0125] (3) Packet processing:
[0126] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0127] (4) Ultraviolet light treatment:
[0128] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0129] Process Six
[0130] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0131] (1) Bacterial agent activation treatment:
[0132] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0133] (2) Preparation of coating material guar gum:
[0134] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After the treatment for 22 minutes, the guar gum was taken out for use;
[0135] B. Weigh corresponding weight portions of 60 parts of guar gum treated in operation A, 15 parts of diatomaceous earth, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0136] (3) Packet processing:
[0137] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0138] (4) Ultraviolet light treatment:
[0139] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0140] Process seven
[0141] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0142] (1) Raw material pretreatment:
[0143] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After the treatment for 22 minutes, the guar gum was taken out for use;
[0144] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0145] C. Weigh corresponding weight portions of 60 parts of guar gum treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0146] (2) Ultraviolet light treatment:
[0147] The raw material pretreated in step (1) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coated material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 hours.
[0148] Process Eight
[0149] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0150] (1) Bacterial agent activation treatment:
[0151] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0152] (2) Preparation of coating material guar gum:
[0153] A. The guar gum was placed in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After the treatment for 22 minutes, the guar gum was taken out for use;
[0154] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0155] C. Weigh corresponding weight portions of 60 parts of guar gum treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid, mix well, and then perform deep cold crushing treatment;
[0156] (3) Packet processing:
[0157] The microbial agent that has been cryogenically crushed in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then subjected to a cold air drying treatment.
[0158] Process Nine
[0159] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0160] (1) Bacterial agent activation treatment:
[0161] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0162] (2) Preparation of coating materials:
[0163] A. Treat the starch in an ultrasonic-ultraviolet light coupling environment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. Treat for 22 minutes and then take it out for later use;
[0164] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0165] C. Weigh 60 parts of starch treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid in corresponding weight portions, mix well, and then perform deep cold crushing treatment;
[0166] (3) Packet processing:
[0167] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0168] (4) Ultraviolet light treatment:
[0169] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0170] Craft 10
[0171] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0172] (1) Bacterial agent activation treatment:
[0173] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0174] (2) Preparation of coating materials:
[0175] A. Place chitosan in an ultrasonic-ultraviolet light coupling environment for treatment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. After 22 minutes of treatment, take it out for use;
[0176] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0177] C. Weigh 60 parts of chitosan treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid in corresponding weight portions, mix well, and then perform deep cold crushing treatment;
[0178] (3) Packet processing:
[0179] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0180] (4) Ultraviolet light treatment:
[0181] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0182] Craft 11
[0183] A preparation process of a heavy metal adsorbing guar gum coated bacterial agent composite material comprises the following steps:
[0184] (1) Bacterial agent activation treatment:
[0185] The bacterial agents are placed in microbial culture medium for shaking and activation, and then centrifuged after completion, and the precipitate is cryogenically crushed;
[0186] (2) Preparation of coating materials:
[0187] A. Treat the cellulose in an ultrasonic-ultraviolet light coupling environment, with an ultrasonic frequency of 70kHz and an ultraviolet light wavelength of 300nm. Treat for 22 minutes and then take it out for later use;
[0188] B. placing the diatomite in a cold plasma treatment device for cold plasma treatment, with a treatment power of 300W, a vacuum degree of 45Pa during discharge, a gas flow rate of 1.5L / min, and taking it out for use after 5 minutes of treatment;
[0189] C. Weigh 60 parts of cellulose treated in operation A, 15 parts of diatomaceous earth treated in operation B, 6 parts of citric acid, 6 parts of sodium bicarbonate, and 4.5 parts of linoleic acid in corresponding weight portions, mix well, and then perform deep cold crushing treatment;
[0190] (3) Packet processing:
[0191] The microbial agent after cryogenic pulverization in step (1) is suspended in the air using a fluidized bed, and then the coating material obtained in step (2) is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying is performed to obtain the coating material for use;
[0192] (4) Ultraviolet light treatment:
[0193] The coating material obtained in step (3) is placed in an ultraviolet environment for ultraviolet light irradiation treatment, and the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 25 cm, and the treatment time is 1.5 h.
[0194] In view of the prior art, the present application tested the results and prepared composite materials using the above process 2, process 9 to process 11 respectively. Then, the prepared composite materials were tested for performance. The samples were placed in polyethylene plastic bottles at a temperature of 40°C ± 1°C and a relative suitability of 75% ± 5%. Samples were taken in October, January, February and March respectively, and the corresponding indicators were tested and compared with the results in October (the release situation in the composite material was evaluated by the cumulative release percentage at 5h and 18h during the release process).
[0195] The specific test comparison data are shown in Table 1 below:
[0196] Table 1
[0197]
[0198]
[0199] The data analysis in Table 1 shows that after being stored in a polyethylene plastic bottle at a temperature of 40°C ± 1°C and a relative humidity of 75% for 3 months, when starch, chitosan, and cellulose were used as the main ingredients of the coating material in Examples 9 to 11, the release of the composite material content became relatively fast, and the composite material content also decreased rapidly. The composite material prepared by the method of the present application has the expected appearance, the release of the content, and the content, and the coating material prepared by the method of the present application has good stability under the above conditions.
[0200] In order to further compare the technical effects of the present application, composite materials were prepared using the above-mentioned process 2, process 4 to process 8 respectively, and cadmium-contaminated soil (the content of extractable cadmium was 0.34 mg / kg) was used as the test object. The contaminated soil was randomly divided into 7 groups, and then each group of soil was repaired using process 2, process 4 to process 7, and the repair results were statistically analyzed after 30 days of repair.
[0201] The specific test comparison data are shown in Table 2 below:
[0202] Table 2
[0203] Removal rate of extractable cadmium (%) Passivation rate (%) Example 2 92.1 96.3 Example 4 78.6 82.0 Example 5 82.3 86.6 Example 6 86.6 82.3 Example 7 36.5 56.3 Example 8 89.6 91.3 Example 9 56.9 63.5 Example 10 62.5 68.5 Embodiment 11 59.6 62.3 Control group 68.6 56.1
[0204] By activating the bacterial agent and further coating it to form a composite material, when the heavy metal contaminated soil is repaired, the outer coating material absorbs soil moisture and disintegrates, and the coated bacterial agent is released, thereby repairing the soil. The data analysis in Table 2 shows that when starch, chitosan, and cellulose are used as coating materials in Example 9, Example 10, and Example 11, respectively, the removal rates of extractable cadmium are 56.9%, 62.5%, and 59.6%, respectively, and the passivation rates are 63.5%, 68.5%, and 62.5%, respectively. When guar gum is used as the coating material in Example 2, the removal rate of extractable cadmium reaches 92.1%, and the passivation rate is 96.3%.
[0205] It can be concluded from Table 1 and Table 2 that the composite material prepared by the method of the present application has stable performance compared to starch, chitosan and cellulose and has a good adsorption effect on heavy metals.
[0206] Workflow of the present invention:
[0207] When activating the bacterial agent, the bacterial agent is placed in the test tube 1032 in the device and sealed by the sealing cover, and then the test tube 1032 is placed in the placement hole 1031 in the placement plate 103. The staff starts the shaking component 2 through the control panel to move the moving plate 204 downward to press the top of the test tube 1032, and then the placement plate 103 rotates under the operation of the shaking component 2, thereby realizing the shaking bacteria activation treatment and increasing the proportion of live bacteria. Then, the test tube 1032 is removed to take out the bacterial agent for subsequent operations;
[0208] Furthermore, the first electric telescopic rod 203 drives the movable plate 204 to move downward, and the distance sensor 2041 detects the distance to the upper surface of the placement plate 103 and transmits the data to the control panel for analysis and processing until the set value is reached, so as to avoid damage to the test tube caused by excessive pressure on the movable plate 204;
[0209] Furthermore, the driving motor 201 drives the L-shaped plate 202 to rotate, and the rotating L-shaped plate 202 drives the connected placement plate 103 to rotate, and the rotating placement plate 103 causes the bacterial agent in the test tube 1032 to undergo a vibration activation treatment.
[0210] After the bacterial agent in the test tube 1032 is taken out, the test tube 1032 is put in place, and the shaking component 2 and the cleaning component 3 are started in sequence through the control panel. The shaking component 2 continues to press the top of the test tube 1032, and the cleaning component 3 works to move the water spray barrel 302 downward, and the water spray barrel 302 moves into the test tube 1032 and sprays the disinfectant. Under the operation of the rotating component 4, the inside of the test tube 1032 can be sterilized and cleaned. After a period of time, the shaking component 2 and the cleaning component 3 are reset, and the dumping component 5 works to flip the placement plate 103 by 90 degrees, so that the test tube 1032 is horizontal to facilitate pouring out the remaining water;
[0211] Furthermore, the first electric telescopic rod 203 in the shaking assembly 2 works to drive the moving plate 204 to move downward;
[0212] Furthermore, the second electric telescopic rod 307 in the cleaning assembly 3 drives the fixed plate 309 to move downward, and the downwardly moved fixed plate 309 causes the two water spray barrels 302 to move downward, and the downwardly moved water spray barrels 302 are inserted into the test tube 1032. At this time, the water pump 305 works to send the disinfectant in the disinfection water tank 304 into the water spray barrels 302 through the telescopic hose 303 and spray it out;
[0213] Furthermore, after the shaking component 2 and the cleaning component 2 are reset, the flipping motor 502 in the dumping component 5 starts working, and the output end of the flipping motor 502 rotates to drive the connected placement plate 103 to rotate along the U-shaped groove 501, and then dumping is completed. The water poured out from the test tube 1032 enters the collection chamber 601 through the funnel 602.
[0214] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A preparation device for a heavy metal adsorbing guar gum coated bacterial agent composite material, comprising a housing (1), It is characterized in that A working chamber (101) is provided in the box body (1), a placement plate (103) and a processing component (102) are provided in the working chamber (101), placement holes (1031) are symmetrically provided on the placement plate (103), matching test tubes (1032) are installed in two of the placement holes (1031), the placement plate (103) is connected to the execution end of the processing component (102), the processing component (102) is composed of a shaking component (2), a cleaning component (3) and a dumping component (5), and a collection component (6) for collecting waste liquid is provided below the processing component (102) inside the box body (1); The shaking assembly (2) comprises an inverted L-shaped plate (202), the bottom end of the L-shaped plate (202) being connected to the placement plate (103) via a dumping assembly (5), a moving plate (204) being provided between the top plate of the L-shaped plate (202) and the placement plate (103), and the cleaning assembly (3) being provided on the moving plate (204); The cleaning component (3) comprises through holes (301) symmetrically opened on the movable plate (204), two through holes (301) are each provided with a water spray barrel (302), the top ends of the two water spray barrels (302) are connected to a fixed plate (309) via a rotating component (4), a second electric telescopic rod (307) is installed on one side of the lower surface of the movable plate (204), and the telescopic end of the second electric telescopic rod (307) passes through the movable plate (204) and is fixedly connected to the fixed plate (309); A driving motor (201) is provided on one side of the top of the box (1), the driving motor (201) being installed in a protective shell (211), the output end of the driving motor (201) passing through the top wall of the box (1) and fixedly connected to the top plate of the L-shaped plate (202), a first electric telescopic rod (203) is provided on one side of the cleaning component (3) above the moving plate (204), the first electric telescopic rod (203) being fixedly connected to the lower surface of the top plate of the L-shaped plate (202), and the telescopic end of the first electric telescopic rod (203) being connected to the upper surface of the moving plate (204), and a distance sensor (2041) is installed inside the lower surface of the moving plate (204); The rotating assembly (4) comprises a rotating shaft (403) fixedly connected to the top ends of the two water spray barrels (302); the two rotating shafts (403) are both rotatably connected to the lower surface of the fixing plate (309); a rotating motor (401) is installed at the center of the lower surface of the fixing plate (309) via bolts; a driving wheel (402) is fixedly installed at the output end of the rotating motor (401); driven wheels (404) are fixedly sleeved on the two rotating shafts (403); the driving wheel (402) and the two driven wheels (404) are connected in transmission via a transmission belt (405); The bottom ends of the two water spray barrels (302) are flush with the lower surface of the movable plate (204); a disinfection water tank (304) is welded to the other side of the top of the box body (1); a water pump (305) is installed inside the disinfection water tank (304); the output port of the water pump (305) is connected to a water pipe (306) through a pipeline; the lower surface of the water pipe (306) is symmetrically connected to a telescopic hose (303); one end of the two telescopic hoses (303) passes through the top wall of the box body (1), the top plate of the L-shaped plate (202), the fixed plate (309) and the rotating shaft (403) in the rotating assembly (4) in sequence and is inserted into the water spray barrel (302); a vertical guide rod (308) is fixedly connected to the upper surface of the movable plate (204) on the side away from the second electric telescopic rod (307); the guide rod (308) passes through the fixed plate (309); The tipping assembly (5) comprises a U-shaped groove (501) formed at the bottom end of the L-shaped plate (202); the two side ends of the placement plate (103) are movably connected to the inner wall of the U-shaped groove (501) via a welded rotating shaft; a flip motor (502) is installed on the outer wall of the bottom end of the L-shaped plate (202) via bolts; and the output end of the flip motor (502) is fixedly connected to the rotating shaft; The collecting assembly (6) comprises a collecting chamber (601) opened inside the box (1); a funnel (602) is connected to the top of the collecting chamber (601); the funnel (602) is embedded in the bottom plate of the working chamber (101); a drainage pipe (603) is provided at the bottom of one side of the box (1); the drainage pipe (603) is in communication with the collecting chamber (601); and a valve (6031) is installed on the drainage pipe (603); The preparation process of the device for preparing the composite material of guar gum coated bacterial agent with heavy metal adsorption comprises the following steps: Step 1: Bacterial agent activation treatment: The bacterial agents are placed in a microbial culture medium box (1) for shaking and activation, and after completion, centrifuged and the precipitate is subjected to deep-cold crushing. The bacterial agent in step 1 is at least one of filamentous fungi, bacteria or yeast; Step 2: Preparation of coating material guar gum: The first step is to place the guar gum in an ultrasonic-ultraviolet light coupling environment for treatment, and take it out for use after completion; the second step is to place the diatomaceous earth in a cold plasma treatment device for cold plasma treatment, and take it out for use after completion; the third step is to weigh 55-65 parts of the guar gum treated in the first step, 12-18 parts of the diatomaceous earth treated in the second step, 5-7 parts of citric acid, 5-7 parts of sodium bicarbonate, and 3-6 parts of linoleic acid in corresponding weight parts, mix them evenly, and then perform deep cold crushing treatment; Step 3: Package processing: The microbial agent after deep cold crushing treatment in step 1 is suspended in the air by using a fluidized bed, and then the coating material obtained in step 2 is added to the fluidized bed in the form of a spray, and the microbial agent is coated in a suspended and rolling state, and then cold air drying treatment is performed to obtain the coating material for use; Step 4: UV irradiation treatment: The coating material obtained in step 3 is placed in an ultraviolet environment for ultraviolet light irradiation treatment; Wherein, the coating material in step 2 is guar gum, wherein the ultrasound-ultraviolet light coupling environment in the first step is an ultrasound frequency of 40-100kHz, an ultraviolet light wavelength of 200-400nm, and a treatment time of 20-24min, and during the second step, the cold plasma treatment is controlled to have a treatment power of 200-400W, a vacuum degree of 40-50Pa during discharge, a gas flow rate of 1-2L / min, and a treatment time of 3-7min; During the ultraviolet light irradiation treatment in step 4, the horizontal distance between the coating material and the ultraviolet lamp is controlled to be 20-30 cm, and the treatment time is 1-2 hours.
2. The preparation device of the heavy metal adsorbing guar gum coated bacterial agent composite material according to claim 1, It is characterized in that The outer walls of the two water spray barrels (302) are each provided with a brush (3021), and the diameter of the two water spray barrels (302) is smaller than the diameter of the test tube (1032).