Method for preparing catalyst
By treating the silica support at high temperature and reacting with the metal-C-bonded compound complex, a yttrium, neodymium or scandium compound catalyst supported on the surface of the silica is solved, and high-efficiency ethylene and Propylene polymerization avoids the use of activators.
Patent Information
- Application Number
- CN202180043105.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-10
- Filing Date
- 2021-06-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-06-14
AI Technical Summary
The existing catalysts are insufficiently active in the polymerization of ethylene and propylene, especially in the absence of aluminum or boron compound activators, and the pretreatment temperature of the silica is too low to cause the catalyst activity to be low.
By heating the silica support above 550°C and contacting the metal-C bond compound complex containing yttrium, neodymium or scandium, the metal is bonded to the surface of the silica through the M-O-Si bond, forming a highly active catalyst, avoiding the use of aluminum Oxide or other activator.
The activity of the catalyst is improved, the efficiency of polymerization of ethylene and propylene is enhanced, and the efficiency and product quality of the polymerization reaction are not required without the addition of activators such as aluminum or boron compounds.
Smart Images

Figure CN115667326B_ABST
Abstract
Description
[0001] The present invention relates to a process for preparing a catalyst, in particular a catalyst suitable for the polymerization of ethylene and / or propylene, and wherein the catalyst comprises a compound of yttrium, neodymium or scandium supported on a silica support.
[0002] The polymerization of olefins, particularly ethylene and / or propylene, is widely practiced commercially and uses many different methods and catalysts. For example, the polymerization can be operated in a reactor in a gas phase, a solution phase or a slurry phase. This method is well known and is the subject of many patent applications and literature studies.
[0003] Generally, most catalysts can be characterized as one of three main types that are widely used in different processes, these being the so-called "Phillips catalysts" based on supported chromium, the "Ziegler-Natta catalysts" most commonly based on titanium and magnesium (although some other metals may be used in place of titanium), and the "metallocene catalysts", also commonly referred to as "single site catalysts", which may be based on a variety of metals, including titanium, chromium, zirconium and hafnium. Likewise, the different types of catalysts and their many variations are the subject of numerous patent applications and literature studies.
[0004] It is also known that some rare earth metal compounds are active in the polymerization of olefins.
[0005] For example, Woodman et al. Macromolecules 2005, 38, 3060-3067 describes the preparation of silica-supported rare earth metal catalysts based on Sc, Y, La, Nd, Sm, Gd and Dy. These catalysts were used by Woodman et al. for ethylene polymerization.
[0006] We have now found that improved polymerization catalysts based on compounds of yttrium, neodymium or scandium supported on silica are obtained if the silica is pretreated by heating above a minimum temperature and compounds of yttrium, neodymium or scandium containing at least one metal-C bond are used.
[0007] Thus, in a first aspect, there is provided a process for preparing a catalyst suitable for the polymerisation of ethylene and / or propylene, the catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein the process comprises:
[0008] a) treating the silica support by heating at a temperature of at least 550° C. to at least partially dehydroxylate the silica support but leave isolated silanol groups on the surface,
[0009] b) contacting the treated silica support with a complex of the formula:
[0010] D m MX1 X 2 R
[0011] in
[0012] M is selected from Y, Sc and Nd,
[0013] R is a hydrocarbon group or a substituted hydrocarbon group,
[0014] X 1 and X 2 is an anionic group,
[0015] D is a neutral donor group, and
[0016] m is 0 or greater,
[0017] The complex is allowed to react with silanol and the metal (M) of the complex becomes bound to the surface through the formation of MO-Si bonds.
[0018] Similarly, in a second aspect, there is provided a process for preparing a catalyst suitable for the polymerization of ethylene and / or propylene, the catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein the process comprises:
[0019] a) treating a silica support by heating at a temperature of at least 550° C.,
[0020] b) contacting the treated silica support with a complex of the formula:
[0021] D m MX 1 X 2 R
[0022] in
[0023] M is selected from Y, Sc and Nd,
[0024] R is a hydrocarbon group or a substituted hydrocarbon group,
[0025] X 1 and X 2 is an anionic group,
[0026] D is a neutral donor group, and
[0027] m is 0 or greater,
[0028] And it is characterized in that the silica support is not contacted with aluminoxane before the treatment in step (a) or the contact with the complex in step (b).
[0029] In particular, in the present invention it has been found that the catalysts so prepared are not only active for polymerisation but that they are more active than catalysts prepared from the same complex but in which the silica has not been heated or has been heated at a lower temperature.
[0030] Further, it has been found that the treatment of silica and use of complexes as claimed can provide polymerization activity without the need for the addition of activators, such as the commonly used aluminum or boron compounds included in Woodman et al. mentioned above.
[0031] Without wishing to be bound by theory, this is believed to be due to the formation of a specific supported complex on the silica surface by reaction of the metal complex and the heat-treated silica support.
[0032] In a second aspect, the silica support is not in contact with aluminoxane prior to the treatment of step (a) or the contact with the complex of step (b). It is also preferred in the first aspect that the silica support is not in contact with aluminoxane prior to the treatment of step (a) or the contact with the complex of step (b). Preferably, in the first or second aspect of the invention, the silica support is not in contact with aluminoxane or any other catalyst activator prior to the treatment of step (a) or the contact with the complex of step (b). As used herein, "catalyst activator" is a compound that is added to the catalyst during catalyst preparation or during polymerization, and which activates the catalyst so that the catalyst has catalytic activity. Typical activators for specific types of catalysts are known in the art, and non-limiting examples include aluminoxane compounds, modified aluminoxane compounds, and alkyl aluminum.
[0033] It is also preferred in either aspect that the silica support is not contacted with any compound that might react with the treated silica between the treatment in step (a) and the contacting with the complex in step (b), and more preferably is not contacted with any such compound prior to the treatment in step (a).
[0034] Most preferably, no further treatment steps of the silica support are carried out between the treatment in step (a) and the contacting with the complex in step (b).
[0035] More generally, with regard to the treatment of silica, the silica must be heated to a temperature of at least 550° C. Preferably, the silica is heated to a temperature of at least 600° C., and more preferably at least 650° C. The silica is also preferably heated to a temperature below 1000° C., and preferably below 900° C. A particularly preferred temperature range is 600-850° C., such as 650-800° C.
[0036] The heating may be carried out in any suitable atmosphere, including air, an inert gas such as nitrogen, or under vacuum. The heating may be carried out at any suitable pressure, although atmospheric pressure or pressure below atmospheric pressure is preferred. More preferably, the heating is carried out under reduced pressure, such as 5 x 10 4 Pa or less, such as 5 x 10 3 Most preferably the pressure is 100 Pa or less, such as 10 Pa or less.
[0037] During treatment, the silica is preferably heated to the desired treatment temperature (above 550° C., and preferably within the preferred range defined above), and then maintained at that temperature for at least 1 hour, such as 1-12 hours.
[0038] Typically, during treatment of the silica support by heating at a temperature of at least 550° C., the support is partially dehydroxylated to leave isolated silanol groups on the surface. Then, upon contact with the treated silica surface, the metal-containing complex (the metal being yttrium, neodymium or scandium) reacts with the silanols and the metal of the complex becomes bound to the silica surface by formation of MO—Si bonds.
[0039] The silanol groups on the surface formed by the temperature treatment of step (a) as claimed can be considered to be "isolated". As used herein, this means that they are separated far enough from each other so that the complex reacts with the silanol and becomes bound to the surface through a single MO-Si bond. Generally, the concentration of silanol groups on the surface after the temperature treatment of step (a) (and / or when subsequently contacted with the complex) is less than or equal to 2 silanol groups per square nanometer of silica surface. The concentration of silanol groups can be measured by any suitable technique, but according to the present invention, it is preferably measured by titrating the OH groups of silanols using n-butyl lithium. (In a typical measurement, a known amount (such as 0.5 g) of silica is contacted with a solution containing an excess of n-butyl lithium in hexane for 1 hour. The amount of butane formed by the reaction of butyl lithium with silanol is proportional to the number of silanols present. Butane is preferably collected and quantified by GC. The surface area is measured by BET before calcination according to D3663-03 (2015), as discussed further below).
[0040] Therefore, less than or equal to 2 silanol groups per square nanometer corresponds to ≤ 2.0 OH / nm 2 Preferably, the concentration of silanol groups is less than or equal to 1.5 OH / nm 2 , for example, less than or equal to 1.0 OH / nm 2 Preferably, the concentration is at least 0.5 OH / nm 2 .
[0041] The supported metal compound should contain at least one metal-carbon bond (again the metal is yttrium, neodymium or scandium). Again, without wishing to be bound by theory, it is believed that the presence of at least one metal-carbon bond in the supported metal compound can provide activity without the need for adding an activator during polymerization. 1 and X 2 When neither of them is a hydrocarbon group, X 1 and X 2 At least one of the should preferentially react with the surface (Si-O-)3Si-OH groups to produce a metal compound supported on a silica support containing a metal-carbon bond. 1 or X 2 When the X group is a hydride, it is believed that the hydride bond in the metal-containing complex preferentially reacts with the surface silanol under the elimination of H2, so that the supported metal compound retains at least one metal-carbon from the hydrocarbon group R. Obviously, if one or two X groups in the metal-containing complex are also hydrocarbon groups, the supported metal compound will inevitably retain at least one metal-carbon bond. Preferably, the metal-containing complex retains the initial complex D m MX 1 X 2 R's R group.
[0042] Therefore, the present invention also provides a method for preparing a catalyst suitable for the polymerization of ethylene and / or propylene, comprising a yttrium, neodymium or scandium compound supported on a silica support according to the first and / or second aspect, wherein the yttrium, neodymium or scandium compound supported on the silica support comprises the R group of the complex.
[0043] With regard to silica itself, many silica materials are known for use as catalyst supports, and in particular for supported polymerization catalysts. The starting silica material in the present invention can be broadly selected from such materials.
[0044] Typically, however, the silica prior to calcination may have a particle size of 50-1000 m / s as measured by BET according to ASTM D3663-03 (2015). 2 / g, for example, in the range of 100-500 m 2 / g range. Silica may generally have a porosity of up to 5 ml / g, such as 0.2-3.5 ml / g. The average particle size (D50) may generally be 2-250 μm, especially 3-200 μm, and preferably 5-100 μm. The average pore size in silica may generally be 20-1000 angstroms, such as 50-800 angstroms. Examples of suitable silica materials include Sylopol and other silicas available from Grace Davison, including Sylopol 2104, Sylopol 2109, SyloPol 2408, SyloPol 5550, SyloPol 55SJ; and silicas available from PQ Corporation, such as ES70 and ES70X, MD 747JR.
[0045] The silica support is preferably a silica support consisting essentially of silica, which means that it comprises at least 99% by weight of silica. However, in some embodiments, it may also contain other materials mixed therewith, such as alumina or aluminosilicates.
[0046] About Complex D m MX 1 X 2 R, X 1 and X 2 Suitable groups for are those anionic groups which satisfy the valence of the metal M, such as hydride, hydrocarbyl, halide, alcoholate, ester, thiolate, amide, silyl and the like.
[0047] However, in a preferred embodiment, X 1 and X 2 At least one of X is selected from hydride, hydrocarbon group and substituted hydrocarbon group, more preferably X 1 and X 2 Both are selected from hydrides, hydrocarbyl and substituted hydrocarbyl.
[0048] In one embodiment, X 1 and X 2 At least one of them is a hydride, such as X 1 and X 2 Both are hydrides.
[0049] In a more preferred embodiment, X 1 and X 2 At least one of X is a hydrocarbon group or a substituted hydrocarbon group, and most preferably X 1 and X 2 Both are hydrocarbon groups or substituted hydrocarbon groups.
[0050] In all embodiments, the hydrocarbyl or substituted hydrocarbyl is a group that is bonded to M through a metal-carbon bond.
[0051] Examples of hydrocarbon groups are linear, branched and cyclic alkyl groups (e.g. methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, benzyl, etc.), aryl groups (e.g. phenyl, toluoyl, mesityl, etc.) and allyl groups.
[0052] Examples of substituted hydrocarbyl groups are the groups listed above, but wherein the group contains one or more heteroatoms, i.e. atoms other than carbon or hydrogen. However, even if substituted, the group still remains connected to the metal M via a metal-carbon bond. (For the avoidance of doubt, the metal-carbon / MC bond follows the definition of the group as a hydrocarbyl group. In contrast, if connected via a heteroatom or other substituent, the ligand will be defined according to that group, e.g. an alcoholate or an amide group, to give two examples). Therefore, all D in the present invention are m MX 1 X 2 The R complex contains at least one metal-carbon bond (wherein the metal is yttrium, neodymium or scandium).
[0053] In a preferred embodiment, any hydrocarbyl groups present (including R) are selected from alkyl and allyl groups, and any substituted hydrocarbyl groups present (also including R) are selected from substituted alkyl and substituted allyl groups.
[0054] More preferably, X 1 , X 2 Each of R and R is selected from an alkyl group, a substituted alkyl group, an allyl group, and a substituted allyl group.
[0055] In a preferred embodiment, X 1 , X 2 Each of R and R is the same hydrocarbyl or substituted hydrocarbyl, and most preferably each is allyl or substituted allyl.
[0056] Particularly preferred groups are silicon-substituted allyl groups, especially trialkylsilanes, and the most preferred groups are 1,3-C3H3(SiR'3)2 groups, where R' is a linear, branched or cyclic alkyl group, such as methyl, ethyl, n-propyl, tert-butyl, cyclohexyl, and the like.
[0057] More generally, in complex D m MX 1 X 2 R, X 1 , X 2 and R can be chosen widely and independently within the defined requirements. However, for practical reasons, X 1 , X 2and R are usually the same group. (And accordingly, there are 3 MC bonds in the initial complex, all of which are hydrocarbon groups).
[0058] In all embodiments, suitable examples of D are neutral donor groups, such as linear and cyclic ethers and thioethers, amines, phosphines, aromatic heterocycles, such as pyridine, etc. Typically m is 0-3, such as 0, 1 or 2. However, preferably, the complex has no donor group D and therefore m is 0.
[0059] Most preferably, complex D m MX 1 X 2 R is a monomer complex.
[0060] Typically, the complex is added to the support in an amount corresponding to 0.5-10 wt% of metal (eg yttrium) compared to the mass of silica, with a range of 1-5 wt% being preferred.
[0061] Generally, the metal content of the supported catalyst is in the same range, ie, 0.5-10 wt% metal compared to the mass of the catalyst, with a range of 1-5 wt% being preferred.
[0062] The metal M is selected from yttrium, neodymium and scandium. M is preferably selected from yttrium and neodymium, yttrium being particularly preferred, ie M is preferably Y.
[0063] In this case the complex is D m YX 1 X 2 R. For the avoidance of doubt, when M is Y, all other features of the complex, ligands, methods preferably remain as previously defined.
[0064] The catalysts produced in the first and second aspects of the invention are suitable for the polymerisation of ethylene and / or propylene.
[0065] Thus, in a third aspect, the present invention provides a catalyst suitable for the polymerisation of ethylene and / or propylene, said catalyst being prepared by the process of the first and / or second aspect.
[0066] Preferred embodiments of the catalyst are as described above, for example typically comprising 0.5-10 wt% of metal compared to the mass of the catalyst.
[0067] In a fourth aspect, the present invention provides a method for the polymerization of ethylene or propylene, the method comprising:
[0068] (i) preparing a catalyst for the polymerization of ethylene and / or propylene, the catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein the process for preparing the catalyst comprises:
[0069] a) treating a silica support by heating at a temperature of at least 550° C.,
[0070] b) contacting the treated silica support with a complex of the formula:
[0071] D m MX 1 X 2 R
[0072] in
[0073] M is selected from Y, Sc and Nd,
[0074] R is a hydrocarbon group or a substituted hydrocarbon group,
[0075] X 1 and X 2 is an anionic group,
[0076] D is a neutral donor group, and
[0077] m is 0 or greater,
[0078] and
[0079] (ii) contacting the catalyst with ethylene or propylene and optionally a comonomer in a polymerization reactor,
[0080] wherein during step (ii) an aluminium alkyl or other alkylating agent is either not used or is used in an amount of less than 5 moles of alkylating agent per mole of metal (M) in the catalyst.
[0081] In a fifth aspect, which is also a preferred embodiment of the fourth aspect, the catalyst is prepared as described for the first and / or second aspect.
[0082] Therefore, in a fifth aspect, the present invention also provides a method for the polymerization of ethylene or propylene, the method comprising:
[0083] a) preparing a catalyst according to the first aspect of the invention and / or according to the second aspect of the invention, and
[0084] b) polymerizing ethylene or propylene by contacting the catalyst with ethylene or propylene and optionally a comonomer in a polymerization reactor.
[0085] In a preferred embodiment of the fifth aspect, during step (b) an aluminum alkyl or other alkylating agent is either not used or is used in an amount of less than 5 moles of alkylating agent per mole of metal (yttrium, neodymium or scandium) in the catalyst.
[0086] The polymerization methods of the fourth and fifth aspects may be carried out in any suitable polymerization reactor / under any suitable polymerization conditions, including in a gas phase polymerization reactor / under gas phase polymerization conditions, a slurry phase polymerization reactor / under slurry phase polymerization conditions or a solution phase polymerization reactor / under solution phase polymerization conditions.
[0087] The preferred polymerization process is a slurry polymerization process. In this process, the polymerization of a monomer (such as ethylene) is carried out in an inert diluent (generally an alkane, such as isobutane) to produce a slurry of polymer particles suspended in the diluent. Typical reactors include autoclaves and slurry loop polymerization reactors.
[0088] Typical reactors and conditions useful for carrying out polymerizations are well known in the art and need not be described here.
[0089] The polymerisation in the fourth or fifth aspect is polymerisation of ethylene or propylene. Preferably, the polymerisation is a process for polymerisation of ethylene.
[0090] Typically, a polymerization process may be a homopolymerization in which a single monomer is polymerized or a copolymerization in which two or more monomers are polymerized. Also typically, and as used herein, a process for the polymerization of a particular monomer, such as ethylene, refers to a process in which the monomer is the sole monomer (homopolymerization) or is the monomer present in the reactor in the largest amount together with a smaller amount of other monomers (copolymerization). For example, "ethylene polymerization" refers to a process in which ethylene monomer is present as the sole monomer (ethylene homopolymerization) or is present with other monomers, but ethylene is present in the largest amount (ethylene copolymerization). In this method, the monomer present in the largest amount (e.g., ethylene) may be referred to as the "primary" monomer. The other monomers in this reaction are referred to as comonomers.
[0091] In the present invention, the process is used for the polymerization of ethylene or propylene. Therefore, this comprises:
[0092] - homopolymerization of ethylene,
[0093] - Copolymerization of ethylene with comonomers,
[0094] - homopolymerization of propylene, and
[0095] - Copolymerization of propylene with comonomers.
[0096] Preferred comonomers in the present invention, if present, are olefins other than the principal monomers, especially other C2-C 10 α-olefins. For the avoidance of doubt, when ethylene is the principal monomer, the comonomer may be propylene and vice versa. Furthermore, more than one comonomer may be used.
[0097] In many polymerization processes, activators such as aluminum alkyls may be required to obtain activity, or may be used to increase activity.
[0098] A particular feature of the catalysts of the present invention is that they are active even without the use of an activator, such as an aluminum alkyl. In fact, the use of activators at levels too high appears to be detrimental to activity.
[0099] Preferably, in the fourth or fifth aspects, an aluminum alkyl or other alkylating agent is either not used or is used in an amount of less than 1 mole of alkylating agent per mole of metal in the catalyst.
[0100] The method of the fourth or fifth aspect may also include other components typically present in a polymerization process. For example, hydrogen is typically present as a chain transfer agent. Other components may be present depending on the method of operation - for example, a slurry process is typically carried out in an inert diluent (such as isobutane), while a gas phase process may include an inert gas such as nitrogen in the gas phase. Such options are well known to those skilled in the art. Example
[0101] Catalyst preparation
[0102] Catalyst 1: Catalyst containing Y, treated silica at 700°C
[0103] Sylopol 2408 silica (WR Grace) was heated at 700°C under dynamic vacuum for 12 hours.
[0104] Y{1,3-C3H3(SiMe3)2}3 was prepared according to the method described by White and Hanusa in Organometallics 2006, 25, p.5621-5630.
[0105] The treated support is then contacted with Y{1,3-C3H3(SiMe3)2}3 in hexane at room temperature. On contact, the support rapidly turns yellow. After two hours, the reaction is interrupted and the product is dried. A bright yellow support is obtained.
[0106] The catalyst was analyzed by DRIFT, which showed that all silanols on the silica surface reacted. Based on the mass balance, the composition of the catalyst was calculated as shown in Table 1.
[0107] Table 1 - Elemental analysis results and olefin quantification.
[0108]
[0109] The 8.54 wt% carbon found on the surface corresponds to a 17.1 C / Y ratio, which is very close to the theoretical value of 18 C / Y for (≡SiO)Y{1,3-C3H3(SiMe3)2}2. The amount of olefin C3H4(SiMe3)2 released during grafting matches the expected “loss” of one of the initial allylic groups.
[0110] Catalyst 2: Catalyst containing Nd, treated silica at 700°C
[0111] Sylopol 2408 silica (WR Grace) was heated at 700°C under dynamic vacuum for 12 hours.
[0112] Nd{1,3-C3H3(SiMe3)2}3 was prepared in an identical manner to that of Y{1,3-C3H3(SiMe3)2}3 but using NdCl3.
[0113] The treated support was then contacted with Nd{1,3-C3H3(SiMe3)2} in hexane at room temperature. After 24 hours of reaction, the product was filtered and washed 3 times with 6 mL of toluene and 3 times with hexane (6 mL). The powder was then dried under high vacuum.
[0114] Comparative Catalyst A: Catalyst containing Y, silica treated at 200°C
[0115] Sylopol 2408 silica (WR Grace) was heated at 200°C under dynamic vacuum for 12 hours.
[0116] The treated support is then contacted with Y{1,3-C3H3(SiMe3)2}3 in hexane at room temperature. On contact, the support rapidly turns yellow. After two hours, the reaction is interrupted and the product is dried. A bright yellow support is obtained.
[0117]
[0118] Ethylene polymerization
[0119] 1) Small autoclave
[0120] The polymerization tests were carried out in an 80 ml autoclave with 50 ml of heptane as solvent. The reactor was pressurized with ethylene to a pressure of 10 bar. In the selected experiments, 1-hexene was added as comonomer. The reaction temperature was 80°C. No hydrogen was used during the polymerization.
[0121] The catalyst was injected into the reactor to initiate the reaction, and the reaction was carried out for 30 minutes before the reaction was stopped.
[0122] Table 1 shows the results obtained for Catalyst 1.
[0123] Table 1
[0124]
[0125] The results of Run 1 show that the catalyst is active without the addition of TIBAL or other activators. The results of Run 2 show increased activity in the presence of 21 mol% 1-hexene, while a comparison of Run 3 with Run 2 shows that the addition of 1 mM TIBAL, a well-known activator, is actually detrimental to activity.
[0126] Table 2 shows the results obtained for Comparative Catalyst A in the presence of TIBAL and 1-hexene:
[0127] Table 2
[0128]
[0129] Comparison of Run 4 with Run 3 shows that the activity of Comparative Catalyst A, in which the silica was activated at 200°C, is much lower than the activity seen under equivalent conditions for Catalyst 1, in which the silica was activated at 700°C.
[0130] Table 3 shows the results obtained from Catalyst 2:
[0131] Table 3
[0132]
[0133] These results indicate that the Nd-containing catalysts are also active for polymerization.
[0134] 2) 5L Autoclave
[0135] The polymerization test was carried out in a 5 L autoclave with 1.5 L of isobutane as solvent. The reactor was pressurized with ethylene to a pressure of 10 bar. 2.6 mol % of hydrogen and 30 g of 1-hexene were added as comonomer relative to ethylene. The reactor was then heated to a reaction temperature of 80°C. The total equilibrium pressure of the system was 24.4 bar.
[0136] 100 mg of catalyst (Catalyst 1) was injected into the reactor as a 10 wt% suspension in oil to initiate the reaction, and the reaction was allowed to proceed for 1 hour before the reaction was stopped.
[0137] Figure 1 The results obtained as a function of TIBAL addition are shown for Catalyst 1. It can be seen that the highest activity is obtained at the lowest TIBAL level, consistent with the results shown in the small autoclave.
Claims
1. A process for preparing a catalyst suitable for the polymerization of ethylene and / or propylene, the catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein the process include: a) treating a silica support by heating at a temperature of at least 550° C. to at least partially dehydroxylate the silica support but leaving silanol groups on the surface, b) contacting the treated silica support with a complex of the formula: D m MX 1 X 2 R in M is selected from Y, Sc and Nd, R is a hydrocarbon group or a substituted hydrocarbon group, X 1 and X 2 is an anionic group, D is a neutral donor group, and m is 0 to 3, The complex is allowed to react with silanols and the metal (M) of the complex becomes bound to the surface through the formation of MO-Si bonds.
2. A process for preparing a catalyst suitable for the polymerization of ethylene and / or propylene, said catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein said process include: a) treating a silica support by heating at a temperature of at least 550° C., b) contacting the treated silica support with a complex of the formula: D m MX 1 X 2 R in M is selected from Y, Sc and Nd, R is a hydrocarbon group or a substituted hydrocarbon group, X 1 and X 2 is an anionic group, D is a neutral donor group, and m is 0 to 3, The method is characterized in that the silica support is not contacted with aluminoxane before the treatment in step (a) or the contact with the complex in step (b).
3. A process according to claim 1 or claim 2, wherein the silica support is not contacted with any compound that may react with the treated silica between the treatment in step (a) and the contacting with the complex in step (b).
4. A method according to claim 1 or claim 2, wherein X 1 and X 2 At least one of the following is selected from the group consisting of hydride, hydrocarbon group and substituted hydrocarbon group.
5. A method according to claim 1 or claim 2, wherein X 1 and X 2 Both are selected from hydrides, hydrocarbyl and substituted hydrocarbyl.
6. A method according to claim 1 or claim 2, wherein X 1 , X 2 Each of R and R is a hydrocarbon group or a substituted hydrocarbon group.
7. A process according to claim 1 or claim 2 wherein at least R is allyl or substituted allyl.
8. The method according to claim 7, wherein X 1 , X 2 Each of R and R is an allyl group or a substituted allyl group.
9. The method according to claim 7, wherein the group is a silicon-substituted allyl group.
10. The method according to claim 9, wherein the group is a trialkylsilane.
11. The method according to claim 9, wherein each of the allyl groups is 1,3-C 3 H 3 (SiR' 3 ) 2 A group wherein R' is a linear, branched or cyclic alkyl group.
12. A method according to claim 1 or claim 2, wherein m is equal to 0.
13. A process according to claim 1 or claim 2, wherein the metal (M) content of the supported catalyst is in the range of 0.5 to 10 wt% metal compared to the mass of the catalyst.
14. The process according to claim 13, wherein the metal (M) content of the supported catalyst is in the range of 1-5 wt%.
15. A method according to claim 1 or claim 2, wherein the metal is yttrium (Y).
16. A catalyst suitable for the polymerization of ethylene and / or propylene, said catalyst being prepared by the process of claim 1 or claim 2.
17. A method for the polymerization of ethylene or propylene, the method include: (i) preparing a catalyst for the polymerization of ethylene and / or propylene, said catalyst comprising a compound of yttrium, neodymium or scandium supported on a silica support, and wherein said process comprises: a) treating a silica support by heating at a temperature of at least 550° C., b) contacting the treated silica support with a complex of the formula: D m MX 1 X 2 R in M is selected from Y, Sc and Nd, R is a hydrocarbon group or a substituted hydrocarbon group, X 1 and X 2 is an anionic group, D is a neutral donor group, and m is 0 to 3, and (ii) contacting the catalyst with ethylene or propylene and optionally a comonomer in a polymerization reactor, wherein during step (ii) an aluminium alkyl or other alkylating agent is either not used or is used in an amount of less than 5 moles of alkylating agent per mole of metal (M) in the catalyst.
18. A process according to claim 17, wherein the catalyst is prepared by the process of claim 1 or claim 2.
19. A method for the polymerization of ethylene or propylene, the method include: (i) preparing a catalyst according to the process of claim 1 or claim 2, and (ii) contacting the catalyst with ethylene or propylene and optionally a comonomer in a polymerization reactor.
Citation Information
Patent Citations
Polyethylene polymerization catalyst and process
CA2192722A1
Activating supports with controlled distribution of oh groups
CN102421810A
Activating supports
CN103328516A
Polymerization catalyst composition, method for producing synthetic polyisoprene, and synthetic polyisoprene
CN104379613A
Method for producing supported metallocene catalyst and olefin polymerization process using the same
CN1263537A