Sustainable Resilient Sheets
By using polyurethane cores made of recycled materials, the problem of vinyl core curling under temperature changes is solved, achieving higher dimensional stability and bending strength, and promoting environmental sustainability.
Patent Information
- Application Number
- CN202180023724.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-24
- Filing Date
- 2021-01-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-01-22
AI Technical Summary
The floors or wall panels of existing vinyl cores are prone to curl when temperature changes, resulting in dimensional instability and installation problems, and traditional sheets are not environmentally friendly.
Using polyurethane cores made at least partly from recycled materials, including polyols and isocyanates, can achieve better dimensional stability and sustainability by adjusting formulations and additives to increase the density and bending strength of the core.
It provides better dimensional stability and bending strength, reduces temperature expansion deformation of the sheet, and improves the environmental friendliness of the product through the use of recycled materials.
Smart Images

Figure BDA0003860338500000101 
Figure BDA0003860338500000111 
Figure BDA0003860338500000181
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Application Serial No. 62 / 965,389, filed on January 24, 2020, the entire contents of which are incorporated herein by reference as described below. Technical Field
[0003] Various embodiments of the present invention relate generally to polymer-based building panels and more particularly to polyurethane formulations having high density characteristics for use in composite flooring, ceiling and / or wall panels. Background Art
[0004] Composite building panels and tiles are commonly used in businesses, homes, and institutions, offering many benefits including improved floor protection, comfort, design versatility, low maintenance, and in some cases, ease of installation. In addition, composite building panels can replace wood and plywood, providing environmental benefits, namely reducing deforestation.
[0005] Composite panels and tiles are constructed of several layers. An outer or image layer with a high-resolution decorative image of wood, tile or stone is usually sealed under a protective resin coating. The core layer, where most of the density of the entire panel is located, provides structure. The backing layer holds the composite panel together. Some composite panels and tiles also include an additional substrate layer to facilitate installation. The panels and tiles can be laid on a surface and mechanically bonded together to form floor coverings and wall or ceiling sheathing without the use of adhesives, thereby reducing labor and time during the installation phase. This type of floor covering is called a floating floor covering.
[0006] In recent years, manufacturers have developed boards and tiles with polymer rigid cores that are made of vinyl polymers mixed with additives such as wood plastic composites (WPC) or stone polymer composites (SPC). The composition of the core affects the overall board's properties such as stiffness or hardness, thickness, water resistance, thermal insulation, sound insulation, density, and durability. One of the disadvantages of vinyl flooring or wallboard is its tendency to curl. Curling is caused by the expansion and contraction of the layers within the floor or wallboard when the temperature changes. The different degrees of contraction and / or expansion of vinyl flooring or wallboards result in positive or negative curl, as well as uneven floors or wallboards. Curling of adjacent floor or wallboards can lead to damage, such as separation of boards, stress on seams, and / or surface delamination.
[0007] Surprisingly, the disclosed polymer-based floor or wall panels having one or more layers containing polyurethane provide better dimensional stability, better sound insulation, and better flex and locking strength compared to existing panels having traditional vinyl cores. In particular, the polymer-based floor or wall panels can achieve an ideal balance between high density and better flexural strength. In addition, the formulations of the present invention can be optionally, at least partially, made from recycled or reusable materials. Starting with recycled or reusable materials, such as recycled carpet fibers or plastic bottles, is beneficial to the environment, helping to reduce plastic waste entering landfills or the world's water bodies, while creating a sustainable and resilient alternative to traditional vinyl sheet materials. Summary of the invention
[0008] The present invention relates to a polyurethane core for flooring or wall panels. An exemplary embodiment of the present invention provides a polyurethane core comprising: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0009] In any embodiment of the present invention, the polyol may comprise from about 1% to about 40% by weight of one or more recycled materials.
[0010] In some embodiments, the polyol may include a polyester polyol and / or a polyether polyol.
[0011] In some embodiments, the one or more recycled materials may include polyester terephthalate carpet fibers.
[0012] In some embodiments, the one or more recycled materials may include polyethylene terephthalate bottles.
[0013] In some embodiments, the isocyanate may include at least one polyisocyanate.
[0014] In some embodiments, the polyisocyanate may have an NCO content of about 25 wt. % to about 35 wt. %.
[0015] In some embodiments, the polyisocyanate may include methylene diphenyl diisocyanate (MDI).
[0016] In some embodiments, the methylene diphenyl diisocyanate may be selected from 2,2'-MDI, 2,4'-MDI, and 4,4'-MDI.
[0017] In some embodiments, the methylene diphenyl diisocyanate may have an NCO content of 27.5 wt.%, a viscosity of 140 cps at 25° C., and a density of 1.20 g / cm 3, an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of about 2.2.
[0018] In some embodiments, methylene diphenyl diisocyanate may have an NCO content of 31.5 wt.%, a viscosity of 200 cps at 25° C., and a density of 1.23 g / cm2 at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of about 2.7.
[0019] In some embodiments, methylene diphenyl diisocyanate may have an NCO content of 32.4 wt.%, a viscosity of 17 cps at 25° C., and a density of 1.22 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.00001 mmHg at 25°C, and a functionality of about 2.01.
[0020] In some embodiments, the core may include from about 5% to about 50% by weight of the polyisocyanate.
[0021] In some embodiments, the polyurethane core may further include a chain extender.
[0022] In some embodiments, the chain extender may be selected from butanediol (BDO), diethylene glycol (DEG), ethylene glycol, propylene glycol, diethanolamine, trimethylolpropane, and combinations thereof.
[0023] In some embodiments, the core may include about 0% to 5% by weight of a chain extender.
[0024] In some embodiments disclosed herein, the polyurethane core may further include a catalyst.
[0025] In some embodiments, the catalyst may include a metal-based catalyst.
[0026] In some embodiments, the catalyst may include a gel catalyst.
[0027] In some embodiments, the catalyst may include a thermally activated catalyst.
[0028] In some embodiments, the polyurethane core may further include a dispersant and / or a surfactant.
[0029] In some embodiments, the polyurethane core may further include at least one filler.
[0030] In some embodiments, the at least one filler may include calcium carbonate.
[0031] In some embodiments, the core may include from about 0% to about 60% by weight of at least one filler.
[0032] In some embodiments, the core has a dimensional stability change at 70°C of 0.30% or less.
[0033] In some embodiments, the core has a dimensional stability change at 80°C of 0.40% or less.
[0034] In some embodiments, the core has a dimensional stability change of 0.30% or less at 70°C and a dimensional stability change of 0.40% or less at 80°C.
[0035] In some embodiments, the core can exhibit a first dimensional stability expressed as a percentage at 70°C and a second dimensional stability expressed as a percentage at 80°C, wherein the second dimensional stability is less than 0.30 greater than the first dimensional stability.
[0036] In some embodiments, the core can have a thickness of about 4 mm, wherein the core can exhibit a flexural strength of at least 30 MPa.
[0037] In some embodiments, the core can have a thickness of about 4 mm, wherein the core can exhibit a flexural strength of about 30 MPa to about 80 MPa.
[0038] In some embodiments, the core can have a thickness of about 4 mm, wherein the core can exhibit a flexural strength of about 35 MPa to about 65 MPa.
[0039] In some embodiments, the core can have a thickness of about 6.4 mm, wherein the core can exhibit a flexural strength of at least 100 MPa.
[0040] In some embodiments, the core may have a thickness of about 1.4 g / cm 3 -About 2.0g / cm 3 density.
[0041] In some embodiments, the core may have a thickness of about 1.4 g / cm 3 - to about 1.8 g / cm 3 density.
[0042] An exemplary embodiment of the present invention provides a polymer-based floor or wall covering panel comprising a polyurethane core and at least one substrate and an optional top layer. The polyurethane core may include: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0043] In some embodiments, the sheet has a dimensional stability of 0.2% or less at 70°C and a dimensional stability of 0.30% or less at 80°C.
[0044] In some embodiments, the sheet can exhibit a first dimensional stability expressed as a percentage at 70° C. and a second dimensional stability expressed as a percentage at 80° C., wherein the second dimensional stability is less than 0.20 greater than the first dimensional stability.
[0045] In some embodiments, the sheet has a tensile strength greater than 10 kN / m on at least one side of the sheet.
[0046] In some embodiments, the sheet may have a residual indentation of less than 2%.
[0047] In some embodiments, the sheet material may have a long-term indentation of less than 0.2 mm.
[0048] In some embodiments, the sheet material may have a long-term indentation of less than 0.1 mm.
[0049] In some embodiments, the substrate may include components derived from recycled materials.
[0050] An exemplary embodiment of the present invention provides a method for producing a polyurethane core for flooring or wallboard, the method comprising forming a mixture and extruding the mixture to form a core. The mixture may include a polyol and an isocyanate. The polyol may be made at least in part from one or more recycled materials. The method optionally includes annealing a substrate onto the core. The method optionally includes laminating a top layer onto the core and the substrate.
[0051] An exemplary embodiment of the present invention provides a floor or wall covering panel comprising a polyurethane-based core, a decorative print layer located near a top surface of the core, and a protective layer located near a top surface of the decorative print layer. The polyurethane-based core may include: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0052] In some embodiments, the sheet may further include a pad located adjacent a bottom surface of the core.
[0053] In some embodiments, the liner can be a polyurethane-based liner.The polyurethane-based liner can include: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0054] In some embodiments, the polyurethane-based core may be a polyurethane foam.
[0055] In some embodiments, the polyurethane-based cushion may be a polyurethane foam.
[0056] In some embodiments, the core has a density of about 60-90 lbs / ft 3 .
[0057] In some embodiments, the core may further include a reinforcement layer of glass fiber.
[0058] In some embodiments, the core may further include one or more chain extenders present in the core in an amount up to 30 parts per 100 parts of polyol.
[0059] In some embodiments, the core may further include one or more chain extenders present in the core in an amount of up to 2 parts per 100 parts of polyol.
[0060] In some embodiments, the core may further include one or more dispersants present in the core in an amount of up to 10 parts per 100 parts of polyol.
[0061] In some embodiments, the core may further include one or more fillers present in the core in an amount up to 500 parts per 100 parts of polyol.
[0062] In some embodiments, the core may further include one or more surfactants present in the core in an amount of up to 2 parts per 100 parts of polyol.
[0063] In some embodiments, the core may further include one or more desiccant agents present in the core in an amount of up to 10 parts per 100 parts of polyol.
[0064] In some embodiments, the polyol of the core may include about 1% to 40% by weight of one or more recycled materials.
[0065] In some embodiments, the isocyanate may be present in the core in an amount of 100-250 parts per 100 parts of polyol.
[0066] In some embodiments, the protective layer may include polyurethane.
[0067] In some embodiments, the polyurethane of the protective layer may include an isocyanate and a polyol made at least in part from one or more recycled materials.
[0068] In some embodiments, the one or more recycled materials of the core polyol may include polyester terephthalate (PET) carpet fibers.
[0069] In some embodiments, the one or more recycled materials of the polyol of the cushion may include polyester terephthalate (PET) carpet fibers.
[0070] In some embodiments, the one or more recycled materials of the core polyol may include polyester terephthalate (PET) plastic bottles.
[0071] In some embodiments, the one or more recycled materials of the polyol of the liner may include polyester terephthalate (PET) plastic bottles.
[0072] In some embodiments, the core may further include one or more glycols and / or diols.
[0073] In some embodiments, the one or more diols and / or glycols may include polytetrahydrofuran (polyTHF).
[0074] In some embodiments, the isocyanate of the core may include a polyisocyanate.
[0075] In some embodiments, the one or more chain extenders may be selected from butanediol (BDO), diethylene glycol (DEG), ethylene glycol, propylene glycol, diethanolamine, trimethylolpropane, and combinations thereof.
[0076] In some embodiments, the one or more catalysts may be selected from the group consisting of metal-based catalysts, gel catalysts, and thermally activated catalysts.
[0077] In some embodiments, the core may further comprise polyvinyl butyral.
[0078] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of 0.05-0.25% at 80°C.
[0079] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of 0.08-0.25% at 80°C.
[0080] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of 0.05-0.20% at 80°C.
[0081] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of 0.05-0.15% at 80°C.
[0082] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of 0.08-0.20% at 80°C.
[0083] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of about 0.08-0.15% at 80°C.
[0084] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of about 0.10-0.25% at 80°C.
[0085] In some embodiments, the sheet may exhibit a perpendicular dimensional stability of about 0.10-0.15% at 80°C.
[0086] In some embodiments, the core may exhibit a flexural strength between 30-65 MPa.
[0087] An exemplary embodiment of the present invention provides a floor or wall covering panel comprising a polyurethane-based core, a decorative print layer located near the top surface of the core, and a protective layer located near the top surface of the decorative print layer. The polyurethane-based core may include: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0088] In some embodiments, the sheet may further include a pad located adjacent a bottom surface of the core.
[0089] In some embodiments, the liner may be a polyurethane-based liner comprising: a polyol made at least in part from one or more recycled materials; and an isocyanate.
[0090] These and other aspects of the present invention are described in detail below and in the accompanying drawings. After reading the description of specific exemplary embodiments below in conjunction with the accompanying drawings, other aspects and features of the embodiments will become apparent to those of ordinary skill in the art. Although features of the present invention may be discussed with reference to certain embodiments and the accompanying drawings, all embodiments of the present invention may include one or more features discussed herein. In addition, although one or more embodiments may be discussed as having certain advantageous features, one or more such features may also be used in the various embodiments discussed herein. Similarly, although exemplary embodiments may be discussed below as device, system or method embodiments, it should be understood that these exemplary embodiments may be implemented in various devices, systems and methods of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] The following detailed description of the specific embodiments of the present invention will be better understood by reading in conjunction with the accompanying drawings. In order to illustrate the present invention, specific embodiments are shown in the accompanying drawings. However, it should be understood that the present invention is not limited to the precise arrangement and means of the embodiments shown in the accompanying drawings.
[0092] Figure 1 According to an exemplary embodiment of the present invention, a partially expanded view of a sustainable resilient panel ("SRP") is shown;
[0093] Figure 2A According to some exemplary embodiments of the present invention, a graph of travel (inches)-load (lbF) for a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 1 is shown;
[0094] Figure 2B According to some exemplary embodiments of the present invention, a travel (inch)-load (lbF) curve for a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 2 is shown;
[0095] Figure 2C According to some exemplary embodiments of the present invention, a travel (inch)-load (lbF) curve for a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 3 is shown;
[0096] Figure 2D According to some exemplary embodiments of the present invention, a stroke (inch)-load (lbF) curve of a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 4 is shown;
[0097] Figure 2E According to some exemplary embodiments of the present invention, a stroke (inch)-load (lbF) curve of a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 5 is shown;
[0098] Figure 2F According to some exemplary embodiments of the present invention, a travel (inch)-load (lbF) curve for a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 6 is shown;
[0099] Figure 2G According to some exemplary embodiments of the present invention, a travel (inch)-load (lbF) curve for a 4 mm SRP core and a 4 mm polyvinyl chloride (PVC) core of the formulation of Table 7 is shown;
[0100] Figure 3A According to some exemplary embodiments of the present invention, a graph of travel (inches) versus load (lbF) for a 6.2 mm SRP core is shown;
[0101] Figure 3B According to some exemplary embodiments of the present invention, a graph of travel (inches) versus load (lbF) for a 4 mm PVC core is shown;
[0102] Figure 3C According to some exemplary embodiments of the invention, a graph of travel (inches) versus load (lbF) for a 5 mm PVC core is shown. DETAILED DESCRIPTION
[0103] In order to facilitate understanding of the principles and features of the present invention, each exemplary embodiment will be explained below. The components, steps and materials of each element constituting the disclosed embodiments of the present invention described below are intended to be illustrative and not restrictive. Many suitable components, steps and materials that can perform the same or similar functions as the components, steps and materials described herein are intended to be included within the scope of the present invention. Such other components, steps and materials not described herein include but are not limited to similar components or steps developed after the embodiments disclosed by the present invention.
[0104] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0105] As used herein, the term "aliphatic" or "aliphatic group" refers to a straight chain (i.e., unbranched) or branched, substituted or unsubstituted hydrocarbon chain that is completely saturated or contains one or more unsaturated units, or a monocyclic hydrocarbon, bicyclic hydrocarbon, or tricyclic hydrocarbon that is completely saturated or contains one or more unsaturated units, but is not aromatic (also referred to herein as "carbocycle", "alicyclic" or "cycloalkyl"), but has a single point connection to the rest of the molecule. Unless otherwise indicated, an aliphatic group contains 1-30 aliphatic carbon atoms. In some embodiments, an aliphatic group contains 1-20 aliphatic carbon atoms. In other embodiments, an aliphatic group contains 1-10 aliphatic carbon atoms. In still other embodiments, an aliphatic group contains 1-8 aliphatic carbon atoms, and in yet other embodiments, an aliphatic group contains 1, 2, 3, or 4 aliphatic carbon atoms. Suitable aliphatic groups include, but are not limited to, straight or branched, substituted or unsubstituted alkyl, alkenyl, alkynyl, and hybrids thereof, such as (cycloalkyl) alkyl, (cycloalkenyl) alkyl, or (cycloalkyl) alkenyl.
[0106] like Figure 1 As shown, an exemplary embodiment of the present invention provides a polyurethane core, which includes: a polyol made at least in part from one or more recycled materials; and an isocyanate. A polymer-based floor or wall covering board can have a core layer 100 substantially composed of a polyurethane, which includes a polyurethane reaction product of a polyol and an isocyanate. In some embodiments, the core 100 can be composed of foamed polyurethane.
[0107] The core 100 may include other components that various additives are added to the core or cured product, which can change the appearance, properties, handling characteristics or performance of the core. For example, the core formula of the present invention may also include UV stabilizers, anti-adhesion pigments, antibacterial agents, colorants, dyes, wetting agents, surfactants, defoamers, plasticizers and / or foaming agents. Other materials include but are not limited to impact strength enhancers, reinforcing agents, reaction rate enhancers or catalysts, crosslinking agents, fluorescent whitening agents, propylene carbonate, colorants, fluorescent agents, brighteners, hindered amine light stabilizers, processing aids, mica, talcum powder, nanofillers, silane coupling agents, antislip agents, hydrophilic or hydrophobic components, water activators, tackifiers, flow aids, anticaking agents, wetting agents and / or toughening agents, for example, one or more block copolymers. The core 100 may include the weight parts per hundred parts of polyol (phr) resin and / or the components and ranges according to the weight parts of formula (I), but may include more components, and some components may also be excluded. For illustrative purposes, as shown in formulation (I), there are 5 parts of chain extender for every 100 parts of polyol in the formulation. Additionally, various embodiments of formulation (I) may have 0-30 parts of chain extender for every 100 parts of polyol in the formulation.
[0108] Recipe (I)
[0109]
[0110]
[0111] A variety of polymer resins can be used to form a core suitable for the present application, including polyols, such as polyether polyols, polyester polyols, Mannich polyols, glycerol / sucrose polyols and combinations thereof. The polyol resin can be at least partially formed from recycled and / or renewable components, for example, polyester terephthalate (PET) from carpet fibers or polyurethane foams from carpet pads and other cushioning materials. Other polyols from products before and / or after use are also considered, for example, plastic bottles (i.e., soda bottles, water bottles, food cans, etc.), including plastic fragments and / or waste generated in the bottle manufacturing process. In some embodiments, the polyol resin can be formed from recycled polyurethane foam. In certain embodiments, the polymer resin can be formed from bio-derived materials, for example, polyols derived from vegetable oils, castor, soybeans, cottonseed, neem seeds, etc.
[0112] In some embodiments, the polymer resin may be produced by mechanical recycling methods, including but not limited to rebonding flexible foam, regrinding or powdering, adhesive pressing or particle bonding, and compression molding. In some embodiments, the polymer resin may be produced by chemical recycling methods, including but not limited to glycolysis, hydrolysis, pyrolysis, and hydrogenation.
[0113] The polyol used in the present invention may include a hydroxyl value of about 230-500 mg KOH / g. The polyol used in the present invention may have a water content lower than 0.2 wt%, for example, about 0.02 wt% to about 0.18 wt%. The polyol used in the present invention may have an acid value equal to or lower than 2 mg KOH / g, particularly 0.9-1.9 mg KOH / g. The polyol used in the present invention may have a functionality of about 2 to about 4, for example, about 2.0 to about 2.2, about 2.2 to about 2.4, about 2.4 to about 2.6, about 2.6 to about 2.8, about 2.8 to about 3.0, about 3.2 to about 3.6, or about 3.6 to about 4.0. The polyols used in the present invention may have an OH content of about 10% to about 21% by weight, such as about 10% to about 13%, about 12% to about 15%, about 14% to about 17%, about 16% to about 19%, or about 18% to about 21%. The viscosity of the polyols used in the present invention ranges from about 2,500 to about 6,000 centipoise (cps) at 25°C. The polyols used in the present invention may have a density of about 10.2 to about 10.4 pounds per gallon. The specific gravity of the polyols used in the present invention at 25°C ranges from about 1.2 to about 1.3.
[0114] Arropol is a polyol used in some embodiments of the present invention. Arropol 36 is an aromatic polyester polyol produced by Arropol Chemicals, Inc., Dalton, Georgia or ArrowStar, LLC, Dalton Georgia, which is derived from post-consumer polyester terephthalate (PET) carpet fibers. Arropol 36 contains 50% recycled materials, including pre-consumer and / or post-consumer materials, and is formed by melting PET carpet fibers and hydrating the molten PET to form a polyol. Arropol 36 has a hydroxyl number range of 350-450, typically about 397.69 mg KOH / g, a water content of 0.07% (<0.2%) by weight, an acid number of 0.97 (<2) mg KOH / g, a weighted average equivalent weight of 141.06, an average molecular weight of 297.65, a functionality of 2.11, an OH content of 12.05%, a viscosity of 2,100 at 20 rpm on spindle #5, a density of 10.27 lbs / gallon, and a specific gravity of 1.231. is another aromatic polyester polyol used in some embodiments of the present invention and is manufactured by Huntsman Corporation. Terol 11 contains about 6.1% pre-consumer recycled material and about 15.8% post-consumer recycled material. Terol 11 has a hydroxyl number range of 410-460, typically about 435 mg KOH / g, a water content of 0.05% (<0.10%) by weight, an acid number of 1.0 (<2.0) mgKOH / g, a functionality of 2.0, a viscosity of 1,000 cps at 25°C, and a specific gravity of 1.23. Terol 250 contains about 8.2% pre-consumer recycled material and about 21.1% post-consumer recycled material. Terol 250 has a hydroxyl number range of 235-255, is typically about 250 mg KOH / g, has a water content of 0.05% (<0.15%) by weight, an acid number of 1.0 (<2.0) mg KOH / g, a functionality of 2.0, a viscosity of 5,000 cps at 25°C, and a specific gravity of 1.234.
[0115] In some embodiments, the polyol may include about 1%-40% by weight of one or more recycled materials (e.g., about 1%-5%, about 5%-10%, about 10%-15%, about 15%-20%, about 20%-25%, about 25%-30%, about 30%-35%, or about 35%-40%).
[0116] In some embodiments, diols and / or glycols can be used in combination with or in place of a portion of a polyol resin. The glycols can include polycarbonate glycols, such as polyester glycols, polyether glycols, ethylene glycol, polytetrahydrofuran (polyTHF), which can be selectively added to the core to react with the polyols and isocyanates. In some embodiments, the glycols can include about 0% to about 20% by weight (e.g., about 1% to 5%, about 5% to 10%, about 10% to 15%, or about 15% to 20%) of one or more recycled materials.
[0117] In some embodiments, polyvinyl butyral (PVB) resin can be used in combination with or in place of a portion of the polyol resin. In some embodiments, PVB can be used as a blowing agent. In this case, PVB can reduce the density of the polyurethane core without reducing the rigidity or strength of the core. PVB resin is an acetal formed by the reaction of an aldehyde and polyvinyl alcohol. Butvar resin is a polyvinyl butyral resin from Eastman Chemical Company, Kingsport, Tennessee. Butvar 90 has an average molecular weight of about 70 to about 100,000, a solution viscosity of 600-1,200 cps at 25°C in a 15% by weight 60:40 toluene / ethanol solution, a specific gravity of 1.100, a water absorption of 0.5% within 24 hours, a hydroxyl content of 18.5%-20.5%, an acetate content of between 0%-2.5%, and a butyral content of 80%. Butvar 72 has an average molecular weight of about 170 to about 250,000, a solution viscosity of 7,000 to 14,000 cps in a 15% by weight 60:40 toluene / ethanol solution at 25°C, a specific gravity of 1.100, a water absorption of 0.5% in 24 hours, a hydroxyl content of between 17.5% and 20.0%, an acetate content of between 0% and 2.5%, and a butyraldehyde content of 80%. Butvar 74 has an average molecular weight of about 120 to about 150,000, a solution viscosity of 3,000 to 7,000 cps in a 15% by weight 60:40 toluene / ethanol solution at 25°C, a specific gravity of 1.100, a water absorption of 0.5% in 24 hours, a hydroxyl content of between 17.5% and 20.0%, an acetate content of between 0% and 2.5%, and a butyral content of 80%. Butvar 76 has an average molecular weight of about 90 to about 120,000, a solution viscosity of 500 to 1,000 cps in a 15% by weight 60:40 toluene / ethanol solution at 25°C, a specific gravity of 1.083, a water absorption of 0.3% in 24 hours, a hydroxyl content of 11.5% to 13.5%, an acetate content of 0% to 2.5%, and a butyral content of 80%. Butvar 79 has an average molecular weight of about 50 to about 80,000, a solution viscosity of 100 to 400 cps in a 15% by weight 60:40 toluene / ethanol solution at 25°C, a specific gravity of 1.083, a water absorption of 0.3% in 24 hours, a hydroxyl content of 11.5% to 13.5%, an acetate content of 0% to 2.5%, and a butyral content of 80%.Butvar 98 has an average molecular weight of about 40 to about 70,000, a solution viscosity of 200-400 cps at 25°C in a 15 weight percent 60:40 toluene / ethanol solution, a specific gravity of 1.100, a water absorption of 0.5% in 24 hours, a hydroxyl content of 18.0%-20.0%, an acetate content of 0%-2.5%, and a butyral content of 80%.
[0118] The isocyanates used in the present invention may be alicyclic, aliphatic and / or aromatic. Examples of isocyanates include: toluene-2,4-diisocyanate; toluene-2,6-diisocyanate (TDI); 1,5-naphthalene diisocyanate; isopropylbenzene-2,4-diisocyanate; 4-methoxy-1,3-phenyl diisocyanate; 4-chloro-1,3-phenyl diisocyanate; diphenylmethane-4,4-diisocyanate; diphenylmethane-2,4-diisocyanate; diphenylmethane-2,2-diisocyanate; 4-bromo-1,3-phenyl diisocyanate; 4-ethoxy-1,3- Phenyl diisocyanate; 2,4'-diisocyanate diphenyl ether; 5,6-dimethyl-1,3-phenyl diisocyanate; methylene diphenyl diisocyanate (including 2,2'-MDI, 2,4'-MDI and 4,4"-MDI); 4,4-diisocyanate diphenyl ether; 4,6-dimethyl-1,3-phenyl diisocyanate; 9,10-anthracene diisocyanate; 2,4,6-toluene triisocyanate; 2,4,4'-triisocyanate diphenyl ether; 1,4-tetramethylene diisocyanate; 1,6-hexamethylene diisocyanate; 1,10-decamethylene diisocyanate; 1,3-cyclohexane diisocyanate; 4,4'-methylene-bis-(cyclohexyl isocyanate); xylene diisocyanate; 1-isocyanate-3-methyl-isocyanate-3,5,5-trimethylcyclohexane (isophorone diisocyanate); 1-3-bis(isocyanato-1-methylethyl)benzene (m-TMXDI); 1,4-bis(isocyanato-1-methylethyl)benzene (p-TMXDI); the above isocyanates or a mixture of two or more of the above isocyanate compounds or their oligomers or polymers. A variety of polymeric isocyanates can be used in various embodiments of the present invention. Suitable examples include polymers and oligomers of diphenylmethane diisocyanate (MDI and pMDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI) and combinations thereof. Isocyanates are available from The Dow Chemical Company under the trade name TERAFORCE TM 、ISONATE TM 、VORASTAR TM HYPOL TM and PAPI TM , obtained from BASF under the registered name or from Huntsman under the registered name get.
[0119] The polyisocyanate used in the present invention may include a functionality of about 2.0 to about 2.7, an NCO content of about 25 wt% to about 35 wt%, a viscosity of about 15 to about 200 cps at 25°C, a flash point above 200°C (COC), a density range of about 1.2 g / cm3 to about 1.4 g / cm3 at 25°C, an initial boiling point of about 190°C at 5 mm Hg, and a vapor pressure range of about 0.00001 mm Hg to about 0.0010 mm Hg at 25°C. In some embodiments, prepolymer isocyanates may be used in addition to or in place of polyisocyanates. The prepolymer isocyanate can include functionality and properties substantially similar to the polyisocyanate, including, for example, a functionality of about 2.0-2.7, an NCO content of about 25 wt % to about 35 wt %, although prepolymer isocyanates having an NCO content of less than 25 wt % (e.g., less than about 24 wt %, less than about 20 wt %, less than about 15 wt %, less than about 10 wt %, less than about 8 wt %, less than about 5 wt %, or less than about 3 wt %) can also be used. In some embodiments, the core may include one or more polyisocyanates in an amount ranging from about 100 to 250 parts (e.g., about 100-105, about 105-110, about 110-115, about 115-120, about 120-125, about 125-130, about 130-135, about 135-140, about 140-145, about 145-150, about 150-155, about 155-160, about 160-165, about About 165-170, about 170-175, about 175-180, about 180-185, about 185-190, about 190-195, about 195-200, about 200-205, about 205-210, about 210-215, about 215-220, about 220-225, about 225-230, about 230-235, about 235-240, about 240-245, or about 245-250) per hundred parts (polyol) resin. In some embodiments, the core may contain about 5% to about 50%, including, for example, about 5%-10%, about 10%-15%, about 15%-20%, about 20%-25%, about 25%-30%, about 30%-35%, about 35%-40%, about 40%-45%, or about 45%-50% polyisocyanate by weight.
[0120] Chain extenders, curing agents and cross-linking agents may be optionally added to the core to increase hardness and strength. Chain extenders may include low molecular weight diols and / or diamines and may be aliphatic or aromatic. Suitable chain extenders include, but are not limited to, 1,4-butanediol (BDO), diethylene glycol (DEG), ethylene glycol, propylene glycol, 2-methyl-1,3-propanediol, trimethylolpropane, N,N'-bis(2-hydroxypropylaniline), diethanolamine, 1,6-hexamethylenediamine, ethylenediamine (EDA), dimethylolbutyric acid (DMBA), isophoronediamine, 4,4'-bis(sec-butylamino)dicyclohexylmethane, 4,4'-bis(sec-butylamino)diphenylmethane, diethyltoluenediamine, 4,4'-methylenebis(2-chloroaniline), isobutyl 4-chloro-3,5-diaminobenzoate, 2,5-dimethylthiotoluenediamine, trimethylene glycol bis-di-p-aminobenzoate, 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and combinations thereof. In some embodiments, the core may include one or more chain extenders in the range of 0 to about 30 parts, such as about 0-5, about 5-10, about 10-15, about 15-20, about 20- to 25, or about 25-30 parts per hundred parts of (polyol) resin. In some embodiments, the core may include about 0% to about 5% (e.g., about 0%-0.5%, about 0.5%-1.0%, about 1.0%-1.5%, about 1.5%-2.0%, about 2.0%-2.5%, about 2.5%-3.0%, about 3.0%-3.5%, about 3.5%-4.0%, about 4.0%-4.5%, or 4.5%-5.0%) of chain extenders by weight.
[0121] Catalysts in polyurethane systems can be selected to promote and accelerate the gelation and polymerization of polyurethane cores. In some embodiments, metal-based gel catalysts, such as nickel, copper or bismuth, can be used to generate high-density rigid cores. N-200 is a heat-activated gel catalyst for polyurethane formation, available from Evonik Industries, Essen, Germany. In certain embodiments, amine-based gel catalysts can be used to generate high-density rigid foam cores. Suitable amine-based catalysts include, but are not limited to, 1,4-diazabicyclo-[2,2,2]-octane (DABCO), 2,2'-bis-(dimethylaminoethyl ether) (BDMAEE), N-methylmorpholine, 2-morpholinoethanol, N,N-bis-(3-dimethylaminopropyl)-N-isopropanolamine, N,N-bis-(3-dimethylaminopropyl)amine, N,N,N'-trimethyl-N'-(2-hydroxyethyl)bis(2-aminoethyl)ether. A1 is an amine catalyst for polyurethane formation, available from Evonik Industries, Essen. In some embodiments, potassium-based catalysts, such as potassium octoate or potassium 2-ethylhexanoate, can be used as catalysts for producing high-density rigid foam cores. Potassium octoate is an isocyanurate catalyst available from Momentive Performance Materials, Inc., Watford, New York. In some embodiments, the core can include one or more catalysts in a range of 0.1 to about 2 parts (e.g., about 0.01-0.10, about 0.11-0.20, about 0.21-0.30, about 0.31-0.40, about 0.41-0.50, about 0.51-0.60, about 0.61-0.70, about 0.71-0.80, about 0.81-0. 90, about 0.91-1.00, about 1.01-1.10, about 1.11-1.20, about 1.21-1.30, about 1.31-1.40, about 1.41-1.50, about 1.51-1.60, about 1.61-1.70, about 1.71-1.80, about 1.81-1.90 or 1.91-2.00 parts) per hundred parts (polyol) resin.
[0122] Fillers can be selectively added to the core to increase its density and hardness, among other properties. In some embodiments, the filler can include a flame retardant, for example, FR-125 and FR-782 are flame retardants available from Cellular Technologies, Inc., Birmingham, England. Fillers can include barium sulfate, calcium carbonate, expanded silica, colloidal silica, vermiculite, silicates, wood flour, rice husks, straw, clay, sand, glass fibers, glass balls, and combinations thereof. In some embodiments, the core may include one or more fillers ranging from 0 to about 500 parts (e.g., about 0-10, about 10-20, about 20-30, about 30-40, about 40-50, about 50-60, about 60-70, about 70-80, about 80-90, about 90-100, about 100-110, about 110-120, about 120-130, about 130-140, about 140-150, about 150-160, about 160-170, about 170-180, about 180-190, about 190-200, about 200-210, about 210-220, about 220-230, about 230-240, about 240-250, about 250 -260, about 260-270, about 270-280, about 280-290, about 290-300, about 300-310, about 310-320, about 320-330, about 330-340, about 340-350, about 350-360, about 360-370, about 370-380, about 380-390, about 390-400, about 400-410, about 410-420, about 420-430, about 430-440, about 440-450, about 450-460, about 460-470, about 470-480, about 480-490, about 490-500 parts) per hundred parts of (polyol) resin, but higher ranges are also contemplated. In some embodiments, the core may contain one or more fillers ranging from about 0% to about 60% by weight (e.g., about 0%-5%, about 5%-10%, about 10%-15%, about 15%-20%, about 20%-25%, about 25%-30%, about 30%-35%, about 35%-40%, about 40%-45%, about 45%-50%, about 50%-55%, or about 55%-60%).
[0123] Dispersants and wetting agents may be optionally added to the core to improve the dispersion of the filler and reduce viscosity. In some embodiments, dispersants can be used to overcome the higher viscosity associated with high filler loadings. CA-71 is a wetting agent available from Univar. In some embodiments, the core may include one or more dispersants and / or wetting agents in a range of 0-about 10 parts (e.g., 0-1, about 1-2, about 2-3, about 3-4, about 4-5, about 5-6, about 6-7, about 7-8, about 8-9, or about 9-10) per hundred parts (polyol) resin.
[0124] Surfactants can be selectively added to the core to improve the dispersibility of the components, i.e., by reducing surface tension, promoting emulsification and nucleation during mixing. In some embodiments, the surfactant may include an organosiloxane or a silicon-based surfactant. DC193 is an organosilicon surfactant purchased from Evonik Industries. In some embodiments, the core may include one or more surfactants in a range of 0 to about 2 parts (e.g., about 0.01-0.10, about 0.11-0.20, about 0.21-0.30, about 0.31-0.40, about 0.41-0.50, about 0.51-0.60, about 0.61-0.70, about 0.71-0.80, about 0.81-0. .90, 0.91-1.00, about 1.01-1.10, about 1.11-1.20, about 1.21-1.30, about 1.31-1.40, about 1.41-1.50, about 1.51-1.60, about 1.61-1.70, about 1.71-1.80, about 1.81-1.90 or 1.91-2.00 parts) per hundred parts (polyol) resin.
[0125] Molecular sieves and / or desiccant may be optionally added to the core to remove moisture, improve storage stability and / or improve dispersibility. For high density materials, it is important to remove any trace moisture commonly found in the raw materials. In some embodiments, the molecular sieve and / or desiccant may include renewable and recyclable materials. The molecular sieve may include a zeolite-based paste or powder. The molecular sieve may be microporous or mesoporous, with the micropores ranging in size from The pore size of mesopores ranges from 2nm to 50nm. is ideal. Molecular sieves may include, but are not limited to, aluminosilicate zeolites, porous glass, activated carbon, clay, silica, and combinations thereof. JACAAB P3 is a castor oil and zeolite aluminosilicate molecular sieve available from Univar Solutions, Dublin, Ohio. In some embodiments, the core may contain one or more molecular sieves and / or dehumidifiers in a range of 0-about 10 parts (e.g., 0-1, about 1-2, about 2-3, about 3-4, about 4-5, about 5-6, about 6-7, about 7-8, about 8-9, or about 9-10 parts) per hundred parts (polyol) resin.
[0126] In some embodiments, the core has several desirable physical properties, including, for example, lower density, better dimensional stability, and better flexural strength. The density of the core can range from about 0.6 g / cm 3 (37.5lbs / ft 3 )-about 2.2g / cm 3 (137.3lbs / ft 3 )(e.g., about 0.6 g / cm 3 , about 0.7g / cm 3 , about 0.8g / cm 3 , about 0.9g / cm 3 , about 1.0g / cm 3 , about 1.1g / cm 3 , about 1.2g / cm 3 , about 1.3g / cm 3 , about 1.4g / cm 3 , about 1.5g / cm 3 , about 1.6g / cm 3 , about 1.8g / cm 3 , about 2.0g / cm 3 or about 2.2g / cm 3 , or any range within these values, such as 0.7-1.2 g / cm 3 In some embodiments, when the core is used to form a wallboard, the density can be much lower, such as as low as about 0.4 g / cm 3 (25.0lbs / ft 3 ).
[0127] Dimensional stability, as described in ISO 23999:2018, measures the ability of a resilient floor covering to retain its original dimensions after exposure to heat under specified conditions. Vertical deformation or curl deformation is measured before and after exposure to the heat treatment. The vertical distance between the support plate and the wear surface of the test sample is measured at four places around the edge, usually the corner where the distance is greatest. The test sample is placed horizontally on a support plate previously placed in an oven. The test sample is allowed to reach a test temperature of 80±2°C and maintained at that temperature for 6 hours±15 minutes. The test sample is removed from the oven and allowed to recover for 24 hours. In some embodiments, other temperatures and / or times may be used to test dimensional stability. Measurements of dimensional changes due to heat exposure may be collected within two minutes after the test sample is removed from the oven and before recovery. This test can indicate the enhanced dimensional stability of the polymer-based core before recovery.
[0128] Dimensional stability can be determined by calculating the change in the dimensions of the sample in the vertical and horizontal directions. For each measurement, the change refers to the initial length (horizontal and vertical). Linear change dL expressed as a percentage 完整 It is given by the following formula:
[0129] Among them, L 0 is the initial length, L 1 is the length after recovery.
[0130] Thermal linear change dL 热 The same can be determined by calculating the change in size for each measurement relative to the initial length in the vertical and horizontal directions, and L 1,热 is the length after heat test.
[0131]
[0132] For multilayer flooring to comply with the EN16511:2014+A1:2019 European standard, the dimensional stability due to temperature change must be equal to or less than 0.25% at 80° C. Evaluating the polyurethane core alone can be a useful predictor of the performance of multilayer flooring containing a polyurethane core. In some embodiments, the polyurethane core may exhibit a dimensional stability at 70° C. equal to or less than 0.25% (e.g., 0.25% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, 0.01% or less, or any range within these values, such as 0.08-0.20%) when the polyurethane core is measured according to standard ISO 23999:2018 and exposed to a uniform temperature of 70° C. ± 2° C. for 6 hours ± 15 minutes and then recovered for 24 hours.
[0133] In some embodiments, the polyurethane core may exhibit a dimensional stability at 80° C. equal to or less than 0.40% variation (e.g., 0.40% or less, 0.35% or less, 0.30% or less, 0.25% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, 0.01% or less, or any range within these values, e.g., 0.08-0.20%) when measured according to standard ISO 23999:2018 and exposed to a uniform temperature of 80° C. ± 2° C. for 6 hours ± 15 minutes and then recovered for 24 hours.
[0134] In some embodiments, the core may exhibit a vertical dimensional stability that is different from the horizontal dimensional stability at 70° C. For example, the core (or the entire floor / wall panel) may have a vertical dimensional stability of about 0.25% at 70° C., a horizontal dimensional stability of about 0.11% at 70° C., and a warpage range of about -0.5 mm to about +0.5 mm at 70° C.
[0135] In some embodiments, the core may exhibit a vertical dimensional stability different from the horizontal dimensional stability at 80° C. For example, the vertical dimensional stability of the core at 80° C. is about 0.20%, the horizontal dimensional stability at 80° C. is about 0.22%, and the warpage at 80° C. ranges from about -1.8 mm to about +0.5 mm. In certain embodiments, the dimensional stability of the core at 70° C. may vary by only about 0.01% to about 0.30% (e.g., about 0.01%-0.05%, about 0.05%-0.10%, about 0.10%-0.15%, about 0.15%-0.20%, about 0.20%-0.25%, or about 0.25%-0.30%) compared to 80° C.
[0136] The flexural strength of the core can be determined using a three-point bend test as described in ISO 178:2019. For rectangular specimens, the flexural strength σ is measured by the following formula:
[0137] Where F is the load (force) at the breaking point, L is the length of the support span, b is the width, and d is the thickness.
[0138] In some embodiments, the core can have a diameter of about 1 mm to about 11 mm (e.g., about 1 mm, about 1.2 mm, about 1.5 mm, about 1.8 mm, about 2 mm, about 2.2 mm, about 2.5 mm, about 2.8 mm, about 3 mm, about 3.2 mm, about 3.5 mm, about 3.8 mm, about 4 mm, about 4.2 mm, about 4.5 mm, about 4.8 mm, about 5 mm, about 5.2 mm, about 5.5 mm, about 5.8 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, about 15 mm, about 16 mm, about 17 mm, about 18 mm, about 19 mm, about 20 mm, about 21 mm, about 22 mm, about 23 mm, about 24 mm, about 25 mm, about 26 mm, about 27 mm, about 28 mm, about 29 mm, about 30 mm, about 31 mm, about 32 mm, about 33 mm, about 34 mm, about 35 mm, about 36 mm, about 37 mm, about 38 mm, about 39 mm, A thickness of about 6.2 mm, about 6.5 mm, about 6.8 mm, about 7 mm, about 7.2 mm, about 7.5 mm, about 7.8 mm, about 8 mm, about 8.2 mm, about 8.5 mm, about 8.8 mm, about 9 mm, about 9.2 mm, about 9.5 mm, about 9.8 mm, about 10 mm, about 10.2 mm, about 10.5 mm, about 10.8 mm, or about 11 mm, or any range within these values, e.g., 3.5-4.5 mm).
[0139] In some embodiments, a core having a thickness of about 4 mm may exhibit a flexural strength of at least 30 MPa (e.g., 30 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 100 MPa or more, 150 MPa or more, or any range within these values, such as 40-80 MPa). In another embodiment, the core may have a thickness of about 6.4 mm, wherein the core may exhibit a flexural strength of at least 100 MPa (e.g., 100 MPa or more, 110 MPa or more, 120 MPa or more, 130 MPa or more, 140 MPa or more, 150 MPa or more, 160 MPa or more, 170 MPa or more, 180 MPa or more, 200 MPa or more, 250 MPa or more, or any range within these values, such as 110-140 MPa).
[0140] In certain embodiments, a core having a thickness of 4 mm may exhibit a pressure of 39.6 MPa (5740 lbF / in 2 )-63.4MPa(9200lbF / in 2 ) of the flexural strength, but the flexural strength of the core may vary above or below the range provided and may depend on the density of the core.
[0141] In some embodiments, other layers can be added to the core 100 for reinforcement and / or forming a composite sheet material, such as a floor or wall panel 200. The floor or wall panel 200 may include substrates 102, 104, such as an external image / decorative print layer, a laminate layer, a protective layer, an inner layer and / or a backing layer. In certain embodiments, the floor may include one or more other layers having a polyurethane composition, which may be substantially similar to the polyurethane composition of the core. For example, in some embodiments, the protective layer, the decorative print layer, the core layer, and the substrate layer may contain a polyurethane formulation. The polyurethane formulation used in each layer may be made from a reaction of a polyol and an isocyanate, wherein the polyol is at least partially made from one or more recyclable materials, as discussed herein. In any embodiment disclosed in the present invention, the floor may include one or more other layers having a non-polymer or polymer-based composition different from the polyurethane composition of the core, such as fiberglass, polyester, propylene, polyethylene, or other.
[0142] As previously mentioned, in order for a multilayer floor to comply with the European standard EN 16511:2014+A1:2019, the dimensional stability due to temperature variation must be equal to or less than 0.25% at 80° C. In some embodiments, a multilayer floor or wall panel having a substrate such as a decorative print layer, a protective layer, an inner layer and / or a backing layer and a core comprising a sustainable elastic polyurethane core can exhibit better dimensional stability. For example, when exposed to a uniform temperature of 70°C ± 2°C for 6 hours ± 15 minutes and then recovered for 24 hours, the multi-layer floor or wall panel can exhibit a dimensional stability (vertical and / or horizontal) at 70°C of equal to or less than 0.25% variation (e.g., 0.25% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, 0.01% or less, or any range within these values, e.g., 0.08-0.20%). In some embodiments, the vertical dimensional stability of the floor or wall panel can be in the range of about 0.08% to about 0.13% variation, and the horizontal dimensional stability of the floor or wall panel can be in the range of about 0.09% to about 0.12%.
[0143] When exposed to an elevated uniform temperature of 80°C ±2°C for 6 hours ±15 minutes, followed by a 24-hour recovery, the multi-layer floor or wall panel has a dimensional stability (horizontal and / or vertical) at 80°C of equal to or less than 0.25% change (e.g., 0.25% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.03% or less, 0.02% or less, 0.01% or less, or any range within these values, such as 0.08-0.20%). In some embodiments, the vertical dimensional stability of the floor or wall panel may be in the range of about 0.12% to about 0.14%, and the horizontal dimensional stability may be in the range of about 0.13% to about 0.14%. In certain embodiments, the dimensional stability of the floor or wall panels may surprisingly vary by only about 0.01% to about 0.06% at tested oven temperatures of 70°C to 80°C.
[0144] In some embodiments, a floor or wall panel may include a core having a mechanical locking system (e.g., a tongue and groove) so that a first edge of a panel can be connected to a second edge of an adjacent panel and locked together. In some embodiments, the core formulation disclosed herein increases locking strength and facilitates entry of a locking element into a locking groove.
[0145] The locking strength or force strength of mechanically assembled floor or wall panels with a mechanical locking system can be determined by pulling adjacent panels apart to an opening of 0.22 mm or until the lock breaks, whichever occurs first. A tensile testing machine with two clamping devices on which clamps for clamping the sample are mounted. The tensile testing machine is calibrated in accordance with ISO7500-1:2018 and ISO 24334:2019 and complies with the force range for Class 3 locking strength measurements. The length, width, and thickness of the sample are measured to be approximately 2 mm, approximately 3 mm, approximately 4 mm, approximately 5 mm, approximately 6 mm, approximately 7 mm, approximately 8 mm, approximately 9 mm, approximately 10 mm, or approximately 11 mm with an accuracy of 0.1 mm. The sample can be sawn to specific size and balanced with an accuracy of 0.1 g. An external extensometer or other optical measurement system is set up to measure the elongation of the sample with an accuracy of 0.01 mm.
[0146] In some embodiments, assembled floor or wall panels comprising a sustainable resilient polyurethane core can have a locking strength of at least 8 kN / m (e.g., 8.0 kN / m, about 8.5 kN / m, about 9.0 kN / m, about 9.5 kN / m, about 10.0 kN / m, about 10.5 kN / m, about 11.0 kN / m, about 11.5 kN / m, about 12.0 kN / m, about 12.5 kN / m, about 13.0 kN / m, about 14.0 kN / m, or any range within these values, such as 9.0-11.5 kN / m) for the long side of the panel. In some embodiments, assembled floor or wall panels comprising a sustainable resilient polyurethane core can have a locking strength of at least 7 kN / m (e.g., 7.0 kN / m, about 7.2 kN / m, about 7.4 kN / m, about 7.6 kN / m, about 7.8 kN / m, about 8.0 kN / m, about 8.5 kN / m, about 9.0 kN / m, about 9.5 kN / m, about 10.0 kN / m, about 10.5 kN / m, about 11.0 kN / m, about 11.5 kN / m, about 12.0 kN / m, about 13.0 kN / m, about 14.0 kN / m, or any range within these values, such as 7.6-9.0 kN / m) for the short edge of the panel. The locking strength of assembled floors or wall panels including a sustainable elastic polyurethane core can be significantly improved compared to assembled floors or wall panels including a polyethylene-based core with an average locking strength of approximately 4.4 kN / m on the long side and an average locking strength of approximately 8.7 kN / m on the short side.
[0147] Short-term and residual indentation of panels is performed as specified in ASTM F1700-20 and / or ASTM F1914-18. This test method measures the short-term indentation of resilient floor or wall panels and can be used as a predictor of performance over time in actual installations. The indentation of resilient floor coverings is measured using a specific type of indenter, either flat or spherical, at a specified load and time and can be measured after the initial load and after a specified recovery time. The indentation tester is a spherical base device consisting essentially of a rigidly mounted indenter that functions at an initial load of 2.00 ± 0.02 lbf (8.90 ± 0.09 N), a total deadweight load of 30.00 lbf ± 0.25 lbf (133.45 ± 1.11 N), and a suitable micrometer calibrated in increments of 0.0005 inches (0.01 mm). The diameter of the spherical base shall be 0.250 ± 0.0005 inches (6.35 ± 0.01 mm). Another type of indentation tester consists of a deadweight loaded indenter and interchangeable bases of variable geometry. The device is equipped with a dial indicator to measure the depth of the indentation and a rigid metal plate to support the sample.
[0148] Prior to testing, condition the test specimens by exposing them to air at 73.4±3.6°F (23±2°C) and 50±5% relative humidity, or by immersing them in water for 15 to 30 minutes, wherein the water temperature is maintained at 77±0.9°F (25±0.5°C) or 115±1°F (46±0.5°C).
[0149] To measure the initial thickness of a conditioned continuous elastic sheet, a 0.178" (4.52mm) diameter flat presser foot applies a total load of 140 pounds for 10 minutes ± 2 seconds, 30 minutes ± 2 seconds, or 60 ± 1 minutes. After the desired time, read the indentation from the dial indicator and record the thickness value to the nearest 0.001" (0.025mm). After a specified recovery time, usually 60 minutes, record the thickness at the same point where the initial measurement was made to the nearest 0.001" (0.025mm).
[0150] In some embodiments, a floor or wall panel comprising a sustainable elastic polyurethane core may have a short term indentation and a residual indentation of less than about 2% (e.g., less than 2.0%, less than 1.9%, less than 1.8%, less than 1.7%, less than 1.6%, less than 1.5%, less than 1.4%, less than 1.3%, less than 1.2%, less than 1.1%, less than 1.0%, less than 0.9%, less than 0.8%, less than 0.7%, less than 0.6%, less than 0.5%, less than 0.4%, less than 0.3%, less than 0.2%, less than 0.1%, or any range within these values, such as 0.9-1.7%). The floor or wall panel comprising a sustainable elastic polyurethane core exhibits better stiffness than a floor or wall panel comprising a polyethylene-based core having an average short term indentation and a residual indentation of about 2.9%.
[0151] Similar to short-term indentation, the static load limit test of a floor or wall panel per ASTM F970-17 measures the indentation recovery properties of a resilient floor or wall panel and can be used as a predictor of performance over time in an actual installation. Measure and record the initial thickness of the sample to the nearest 0.001 inch (0.025 mm). Apply a load of 75 pounds, 125 pounds, 175 pounds, 250 pounds, or 1,000 pounds for 24 hours ± 15 minutes. After the load is removed, allow the sample to recover for 24 hours ± 15 minutes. Measure the final thickness to the nearest 0.001 inch (0.025 mm) to determine the long-term static load limit of the sample.
[0152] In some embodiments, a floor or wall panel comprising a sustainable resilient polyurethane core can have a long-term indentation or thickness change of less than about 0.1 mm (e.g., less than about 0.10 mm, less than about 0.09 mm, less than about 0.08 mm, less than about 0.07 mm, less than about 0.06 mm, less than about 0.05 mm, less than about 0.04 mm, less than about 0.03 mm, less than about 0.02 mm, less than 0.01 mm, or any range within these values, e.g., 0.07-0.09 mm) after being subjected to a static load of 250 pounds for 24 hours. In some embodiments, a floor or wall panel comprising a sustainable resilient polyurethane core can have a long-term indentation or thickness change of less than about 0.2 mm (e.g., less than about 0.20 mm, less than about 0.18 mm, less than about 0.16 mm, less than about 0.14 mm, less than about 0.12 mm, less than about 0.10 mm, less than about 0.09 mm, less than about 0.08 mm, less than about 0.07 mm, less than about 0.06 mm, less than about 0.05 mm, less than about 0.04 mm, less than about 0.03 mm, less than about 0.02 mm, less than about 0.01 mm, or any range within these values, e.g., 0.08-0.14 mm) after being subjected to a static load of 1,000 pounds for 24 hours. The floor or wall panels comprising the sustainable elastic polyurethane exhibited improved stiffness compared to the floor or wall panels comprising a polyethylene based core having an average long term indentation of 0.26 mm at a static load limit of 250 pounds and an average long term indentation of 0.66 mm at a static load limit of 1,000 pounds.
[0153] The caster chair test evaluates the durability of floor assemblies by simulating the conditions to which floor covering panels will be subjected in actual use. The test specimens consist of floor coverings with one or more joints, assembled as required (e.g., welded, snapped together using locking elements, or glued). The appearance and stability and / or flatness of the floor are measured by delamination, seam opening, or curling of elastic or laminate floor coverings under the movement of the caster chair. The caster chair, weighing approximately 198 lb ± 2 lb (90 kg ± 1 kg), moves in a cyclic path with multiple changes in direction, stopping and starting, and the frequency of passage varies by area. Three different evaluations include: (1) appearance changes of the test specimens after 5,000 cycles and 25,000 cycles according to ISO 9405; (2) color changes after 750 cycles, evaluated by grayscale; and (3) evaluation of the degree of degradation of the specimens after 10,000 cycles or 25,000 cycles.
[0154] In some embodiments, a floor or wall panel comprising a sustainable resilient polyurethane core can withstand 10,000 cycles of the castor chair test with a flatness change of less than about 0.10% (e.g., less than about 0.10%, less than about 0.09%, less than about 0.08%, less than about 0.07%, less than about 0.06%, less than about 0.05%, less than about 0.04%, less than about 0.03%, less than about 0.02%, less than about 0.01%, or any range of these values, such as 0.05-0.09%). The floor or wall panel comprising a sustainable resilient polyurethane core exhibits greater durability than a floor or wall panel comprising a polyethylene-based core having a flatness change of about 0.11% after being subjected to 10,000 cycles of the castor chair test.
[0155] In some embodiments, a floor or wall panel comprising a sustainable resilient polyurethane core can withstand 25,000 cycles of the castor chair test with a flatness change of less than about 0.14% (e.g., less than about 0.14%, less than about 0.13%, less than about 0.12%, less than about 0.11%, less than about 0.10%, less than about 0.09%, less than about 0.08%, less than about 0.07%, less than about 0.06%, less than about 0.05%, less than about 0.04%, less than about 0.03%, less than about 0.02%, less than about 0.01%, or any range within these values, such as 0.05-0.10%). The floor or wall panel comprising a sustainable resilient polyurethane core exhibits better durability than a floor or wall panel comprising a polyethylene-based core having a flatness change of about 0.14% after being subjected to 25,000 cycles of the castor chair test.
[0156] In some embodiments, a floor or wall panel comprising a sustainable resilient polyurethane core can withstand 75,000 cycles of the castor chair test with a flatness change of less than about 0.17% (e.g., less than about 0.17%, less than about 0.16%, less than about 0.15%, less than about 0.14%, less than about 0.13%, less than about 0.12%, less than about 0.11%, less than about 0.10%, less than about 0.09%, less than about 0.08%, less than about 0.07%, less than about 0.06%, less than about 0.05%, less than about 0.04%, less than about 0.03%, less than about 0.02%, less than about 0.01%, or any range within these values, such as 0.08-0.15%). Whereas most floors or wall panels comprising a polyethylene-based core would fail if subjected to the 75,000 castor chair test, floors or wall panels comprising a sustainable resilient polyurethane core exhibit better durability.
[0157] In some embodiments, floors or wall panels comprising a sustainable elastic polyurethane core can provide better insulation performance, for example, an improved R-value ranging from about R0.4 to about R8 (e.g., about R0.4, about R0.8, about R1.2, about R1.6, about R2.0, about R2.4, about R2.8, about R3.2, about R3.6, about R4.0, about R4.4, about R4.8, about R5.2, about R5.6, about R6.0, about R6.4, about R6.8, about R7.2, about R7.6, about R8.0, or any range within these values, for example, R1.6-R2.4).
[0158] The high density core can be prepared by combining the components in formula (I) above. In some embodiments, the components other than the isocyanate can be premixed. The mixture can be mixed with the isocyanate by a high pressure impact mixing head. In some embodiments, the components can be mixed with a low pressure, high shear mixing head. After mixing, the exothermic reaction causes the foam to expand rapidly. In some embodiments, the mixture can be deposited into a mold having the desired shape and size of the core, for example, a board, sheet, block, slat, etc. having a size of 4 feet by 8 feet, 4 feet by 9 feet, or 4 feet by 10 feet. Alternatively, the mixture can be deposited on a first moving conveyor. As the foam expands, a second moving conveyor can limit the expansion to the desired core thickness by contacting the foam on the opposite surface of the first moving conveyor. During the extrusion process, other layers can be added above and below the core to form a board and / or tile. When the board and / or tile leaves the conveying system, the board and / or tile can be cut into different lengths and stacked. The width and length may include various sizes, such as 4' x 8', 4' x 9' or 4' x 10' plywood sheet sizes specified by the product quality grade marking (on the lumber, etc.). In addition, the plywood thickness specified by the product quality grade marking (on the lumber, etc.) ranges from about 1 / 4 inch to about 1-1 / 4 inches. Other sizes may include 4.3mm thick x 4.25 inches / 5.59 inches / 9.84 inches wide x 47.64 inches long. Some special sizes are also contemplated, such as smaller sheets for the Japanese market.
[0159] In some embodiments, the formulation for the core can be prepared as a thermoplastic or thermoset material.
[0160] The following examples further illustrate various aspects of the present invention. However, they are in no way intended to limit the teachings or disclosures of the present invention as described herein.
[0161] Example
[0162] Example 1: Formulation
[0163] The density, dimensional stability, and flexural strength of the sustainable elastic core were evaluated for a variety of formulations, including, for example, the formulations in Tables 1-8.
[0164] Table 1
[0165]
[0166] The density of the core having the formulation in Table 1 is about 1.38 g / cm 3 (about 86lb / ft 3 ).like Figure 2A As shown, the bending strength of the test sample with a thickness of about 4 mm is about 63.5 MPa (about 9200 lbF / in 2 ).
[0167] Table 2
[0168]
[0169] The density of the core having the formulation in Table 2 is about 1.37 g / cm 3 (about 85.8lb / ft 3 ).like Figure 2B As shown, the bending strength of the test sample with a thickness of about 4 mm is about 49.9 MPa (about 7234 lbF / in 2 ).
[0170] Table 3
[0171]
[0172] The density of the core having the formulation in Table 3 is about 1.15 g / cm 3 (about 71.9lb / ft 3 ).like Figure 2C As shown, the bending strength of the test sample with a thickness of about 4 mm is about 44.5 MPa (about 6448 lbF / in 2 ).
[0173] Table 4
[0174]
[0175] The density of the core having the formulation in Table 4 is about 1.22 g / cm 3 (approx. 76.2 lb / ft 3 ).like Figure 2D As shown, the bending strength of the test sample with a thickness of about 4 mm is about 41.8 MPa (about 6065 lbF / in 2 ).
[0176] Table 5
[0177]
[0178] The density of the core having the formulation in Table 5 is about 1.09 g / cm 3 (about 67.9lb / ft 3 ).like Figure 2E As shown, the bending strength of the test sample with a thickness of about 4 mm is about 40.1 MPa (about 5819 lbF / in 2 ).
[0179] Table 6
[0180]
[0181] The density of the core having the formulation in Table 6 is about 1.13 g / cm 3 (about 70.3lb / ft 3 ).like Figure 2F As shown, the bending strength of the sample with a thickness of about 4 mm is about 43.9 MPa (about 6369 lbF / in 2 ).
[0182] Table 7
[0183]
[0184] The density of the core having the formulation in Table 7 is about 1.30 g / cm 3 (about 81.3lb / ft 3 ).like Figure 2G As shown, the bending strength of the test sample with a thickness of about 4 mm is about 39.6 MPa (about 5740 lbF / in 2 ).
[0185] Table 8
[0186]
[0187] The density of the core having the formulation in Table 8 is about 1.37 g / cm 3 (about 85.8lb / ft 3 ).
[0188] The density of the test sample with a polyethylene core and a thickness of about 4 mm was about 0.99 g / cm 3 (about 62lb / ft 3 ), the bending strength is about 15.2MPa (about 2202lbF / in 2 ).
[0189] Example 2: Dimensional stability of sustainable elastic core
[0190] Cores comprising the polyurethane formulations provided in Tables 1-8 and having a thickness of 4.0 mm were made into test specimens. As specified in ISO 23999:2018, the dimensional stability of the specimens is measured by the change or expansion upon exposure to elevated temperatures, such as 70°C and 80°C for 6 hours each. The core test specimens experienced minimal change or expansion when exposed to 70°C or 80°C for 6 hours and allowed to recover for 24 hours. The vertical dimensional stability of the floor or wall panel test specimens increased by about 0.19% to about 0.25% at 70°C, while the polyethylene-based core increased by about 0.21% at 70°C. The vertical stability of the core test specimens increased by 0.20% to about 0.22% at 80°C, while the polyethylene-based core increased by about 0.57% to about 0.83% at 80°C. Importantly, the core test samples had a dimensional stability change of about 0.01% to about 0.06% between 70°C and 80°C, while the polyethylene-based core had a dimensional stability change of about 0.36% to about 0.62% between 70°C and 80°C.
[0191] Example 3: Flexural Strength of Sustainable Elastic Core
[0192] Cores containing the polyurethane formulations provided in Tables 1-8 and having a thickness of 4.0 mm were made into test specimens. Flexural strength was measured on a three-point bend fixture with a spacing of 6.5 inches between the supports and a travel head of 2 feet per minute. All test specimens were 1 inch x 9 inches and 4 mm (0.158 inches) thick, as specified in ISO 178:2019.
[0193] The flexural strength of the polyurethane core test specimen shall be at least 38.5 MPa (5582 lbF / in 2 ).like Figure 3A As shown, the polyurethane core test sample with a thickness of 6.2 mm exhibited a 60.9 MPa (8830 lbF / in 2 )'s bending strength. Figure 2A-2G As shown, with a thickness of 4.0 mm ( Figure 2A-2G , 3B), 5.0mm thickness ( Figure 3C )'s polyethylene-based core, the sustainable elastic board core composed of the polyurethane formulations provided in Tables 1-8 has significantly stronger flexural strength.
[0194] Example 4: Dimensional stability of sustainable elastic panels
[0195] Multilayer boards measuring 190 mm x 1210 mm x 6.7 mm, having a 1.2 mm top layer, a 4.0 mm core composed of the polyurethane formulations provided in Tables 1-8, and a 1.5 mm substrate layer were made into test specimens. As specified in ISO 23999:2018, the dimensional stability of the test specimens is measured by the change or expansion after exposure to elevated temperatures, such as 70°C and 80°C for 6 hours each. When exposed to 70°C or 80°C for 6 hours and allowed to recover for 24 hours, the floor or wall board test specimens experienced minimal change or expansion. The vertical dimensional stability of the floor or wall board test specimens increased by about 0.08% to about 0.13% at 70°C, while the boards containing the polyethylene-based core increased by about 0.15% at 70°C. The vertical stability of the floor or wall board test specimens increased by about 0.12% to about 0.14% at 80°C, while the test specimens containing the polyethylene-based core increased by about 0.33% to about 0.39% at 80°C. Importantly, the dimensional stability of the floor or wallboard test samples changed from about 0.01% to about 0.06% between 70°C and 80°C, while the dimensional stability of the floor or wallboard test samples containing the polyethylene core changed from about 0.18% to about 0.24% between 70°C and 80°C.
[0196] Example 5: Stress strength of sustainable elastic plate
[0197] Multilayer boards with dimensions of 190 mm x 1210 mm x 6.7 mm, having a 1.2 mm top layer, a 4.0 mm core consisting of the polyurethane formulations provided in Tables 1-8, and a 1.5 mm substrate layer were made into test samples. The tensile test machine was calibrated according to ISO7500-1:2018, and the force range for the locking strength measurement met the Class 3 requirements. The long side of the floor or wall panel test sample was superior to the short side and exhibited a locking and / or force strength of 10.94 kN / m. The short side exhibited a locking and / or force strength of 7.78 kN / m.
[0198] Example 6: Short-term indentation and residual indentation of a sustainable elastic sheet
[0199] A multilayer board with dimensions of 190 mm x 1210 mm x 6.7 mm, a 1.2 mm top layer, a 4.0 mm core composed of the polyurethane formulation provided in Tables 1-8, and a 1.5 mm substrate layer was made into a test sample. The test sample was subjected to a static load limit test according to ASTM F1700-20 and / or ASTM F1914-18. Specifically, a load of 140 pounds was loaded onto the test sample for 60 minutes and allowed to recover for 60 minutes. The test sample had a residual indentation of 1.73%.
[0200] Example 7: Static Load Limit of Sustainable Elastic Panel
[0201] A multilayer board with a size of 190 mm x 1210 mm x 6.7 mm, a top layer of 1.2 mm, a core of 4.0 mm composed of the polyurethane formula provided in Tables 1-8, and a substrate layer of 1.5 mm was made into a test sample. The test sample was subjected to a static load limit test according to ASTM F970-17. Specifically, a load of 250 pounds was loaded onto the test sample for 24 hours and allowed to recover for 24 hours. The thickness of the test sample changed by 0.05 mm. After a load of 1,000 pounds was applied to the test sample for 24 hours, the thickness of the test sample changed by 0.07 mm.
[0202] Example 8: Caster Testing of Sustainable Elastic Panels
[0203] Multilayer boards measuring 190 mm x 1210 mm x 6.7 mm, with a 1.2 mm top layer, a 4.0 mm core composed of the polyurethane formulations provided in Tables 1-8, and a 1.5 mm substrate layer were assembled with multiple joints and made into test samples suitable for ISO 4918:2016 and ISO 9405 castor chair tests. After 10,000 cycles, the test sample maintained good appearance with a flatness change of 0.08%. After 25,000 cycles, the test sample maintained good appearance with a flatness change of 0.11%. After 75,000 cycles, which is well above the test castor chair test cycle requirement, the test sample maintained good appearance with a flatness change of 0.13%.
[0204] It should be understood that the application of the embodiments and claims disclosed herein is not limited to the details of the construction and arrangement of the parts shown in the specification and drawings. On the contrary, the specification and drawings provide examples of the contemplated embodiments. The embodiments and claims disclosed herein can also be practiced and executed in other embodiments and in various ways. In addition, it should be understood that the words and terms used herein are for illustrative purposes and should not be regarded as limitations on the claims.
[0205] Therefore, those skilled in the art will appreciate that the concepts upon which the present application and claims are based can be readily used as a basis for designing other structures, methods and systems to achieve the multiple purposes of the embodiments and claims set forth in the present application. Therefore, it is important that the claims be deemed to include such equivalent structures.
[0206] In addition, the purpose of the above abstract is to enable the USPTO and the public, especially practitioners in the field who are not familiar with patent and legal terms or expressions, to quickly determine the nature and substance of the technical disclosure of the present application through a cursory search. The abstract is neither intended to define the claims of the present application nor to limit the scope of the claims in any way.
Claims
1. A polymer-based floor or wall covering panel comprising: A polyurethane core comprising: a polyol made at least in part from one or more recycled materials; and an isocyanate; and at least one substrate and optionally a top layer; Wherein, the polyurethane core is a thermoplastic polyurethane core.
2. The polymer-based floor or wall covering panel according to claim 1, characterized in that: The polyol comprises 1% to 40% by weight of one or more recycled materials.
3. The polymer-based floor or wall covering panel according to claim 1, characterized in that: The polyols include polyester polyols and / or polyether polyols.
4. The polymer-based floor or wall covering sheet according to claim 3, characterized in that: The one or more recycled materials include polyester terephthalate carpet fibers.
5. The polymer-based floor or wall covering panel according to claim 3, characterized in that: The one or more recycled materials include polyethylene terephthalate bottles.
6. The polymer-based floor or wall covering panel of claim 1, characterized in that: The isocyanate includes at least one polyisocyanate.
7. The polymer-based floor or wall covering panel according to claim 6, characterized in that: The polyisocyanate has an NCO content of 25 wt.% to 35 wt.%.
8. The polymer-based floor or wall covering sheet according to claim 6, characterized in that: The polyisocyanate includes methylene diphenyl diisocyanate.
9. The polymer-based floor or wall covering panel according to claim 8, characterized in that: The methylene diphenyl diisocyanate is selected from 2,2'-MDI, 2,4'-MDI and 4,4'-MDI.
10. The polymer-based floor or wall covering panel of claim 8, characterized in that: The methylene diphenyl diisocyanate has an NCO content of 27.5 wt.%, a viscosity of 0.14 Pa·s at 25° C., and a density of 1.20 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of 2.
2.
11. The polymer-based floor or wall covering panel of claim 8, characterized in that: The methylene diphenyl diisocyanate has an NCO content of 31.5 wt.%, a viscosity of 0.2 Pa·s at 25° C., and a density of 1.23 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of 2.
7.
12. The polymer-based floor or wall covering panel of claim 8, wherein: The methylene diphenyl diisocyanate has an NCO content of 32.4 wt.%, a viscosity of 0.017 Pa·s at 25° C., and a density of 1.220 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.00001 mmHg at 25°C, and a functionality of 2.
01.
13. The polymer-based floor or wall covering panel of claim 6, characterized in that: The polyurethane core includes 5% to 50% by weight of polyisocyanate.
14. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core also includes a chain extender.
15. The polymer-based floor or wall covering panel according to claim 14, characterized in that: The chain extender is selected from butanediol, diethylene glycol, ethylene glycol, propylene glycol, diethanolamine, trimethylolpropane and combinations thereof.
16. The polymer-based floor or wall covering panel of claim 14, wherein: The polyurethane core includes 0% to 5% by weight of a chain extender.
17. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core also includes a catalyst.
18. The polymer-based floor or wall covering panel of claim 17, wherein: The catalyst includes a metal-based catalyst.
19. The polymer-based floor or wall covering panel of claim 17, wherein: The catalyst includes a gel catalyst.
20. The polymer-based floor or wall covering panel of claim 17, wherein: The catalyst comprises a thermally activated catalyst.
21. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core also includes a dispersant and / or a surfactant.
22. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core also includes at least one filler.
23. The polymer based floor or wall covering panel of claim 22, wherein: The at least one filler comprises calcium carbonate.
24. The polymer-based floor or wall covering panel of claim 22, wherein: The polyurethane core includes 0% to 60% by weight of at least one filler.
25. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a dimensional stability change at 70° C. of 0.30% or less.
26. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a dimensional stability change at 80° C. of 0.40% or less.
27. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a dimensional stability change at 70°C of 0.30% or less and a dimensional stability change at 80°C of 0.40% or less.
28. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core exhibits a first dimensional stability expressed as a percentage at 70° C. and a second dimensional stability expressed as a percentage at 80° C., wherein the second dimensional stability is less than 0.30 greater than the first dimensional stability.
29. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a thickness of 4 mm, wherein the polyurethane core exhibits a flexural strength of at least 30 MPa.
30. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a thickness of 4 mm, wherein the polyurethane core exhibits a flexural strength of 30 MPa-80 MPa.
31. The polymer based floor or wall covering panel of claim 1, wherein: The polyurethane core has a thickness of 4 mm, wherein the polyurethane core exhibits a flexural strength of 35 MPa-65 MPa.
32. The polymer-based floor or wall covering panel of claim 1, wherein: The polyurethane core has a thickness of 6.4 mm, wherein the polyurethane core exhibits a flexural strength of at least 100 MPa.
33. The polymer based floor or wall covering panel of claim 1, wherein: The polyurethane core has a 1.4 g / cm 3 -2.0g / cm 3 density.
34. The polymer based floor or wall covering panel of claim 1, wherein: The polyurethane core has a 1.4 g / cm 3 -1.8g / cm 3 density.
35. The polymer-based floor or wall covering panel of claim 1, wherein: The dimensional stability of the sheet at 70° C. is equal to or less than 0.2%, and the dimensional stability at 80° C. is equal to or less than 0.30%.
36. The polymer-based floor or wall covering panel of claim 1, wherein: The sheet exhibits a first dimensional stability expressed as a percentage at 70° C. and a second dimensional stability expressed as a percentage at 80° C., wherein the second dimensional stability is less than 0.20 greater than the first dimensional stability.
37. The polymer-based floor or wall covering panel of claim 1, wherein: The sheet material has a tensile strength greater than 10 kN / m on at least one side of the sheet material.
38. The polymer-based floor or wall covering panel of claim 1, wherein: The sheet material has a residual indentation of less than 2%.
39. The polymer-based floor or wall covering panel of claim 1, wherein: The sheet material has a long term indentation of less than 0.2 mm.
40. The polymer-based floor or wall covering panel of claim 1, wherein: The sheet material has a long-term indentation of less than 0.1 mm.
41. The polymer-based floor or wall covering panel of claim 1, wherein: The substrate includes components derived from recycled materials.
42. A floor or wall covering panel comprising: Polyurethane-based core; a decorative printed layer located adjacent a top surface of the core; as well as a protective layer disposed adjacent a top surface of the decorative print layer; The polyurethane-based core comprises polyol and isocyanate at least partially made from one or more recycled materials; and the polyurethane-based core is a thermoplastic polyurethane core.
43. A floor or wall covering sheet according to claim 42, characterised in that: Also included is a pad located adjacent the bottom surface of the core.
44. A floor or wall covering sheet according to claim 43, characterised in that: The liner is a polyurethane-based liner, wherein the polyurethane-based liner includes: a polyol made at least in part from one or more recycled materials; and an isocyanate.
45. A floor or wall covering sheet according to claim 42, characterized in that: The polyurethane-based core is a polyurethane foam.
46. The floor or wall covering sheet of claim 43, wherein: The polyurethane based cushion is a polyurethane foam.
47. The floor or wall covering sheet of claim 42, wherein: The core density is 60-90 lbs / ft 3 .
48. The floor or wall covering sheet of claim 42, wherein: The core also includes a reinforcement layer of glass fibers.
49. The floor or wall covering sheet of claim 42, wherein: The core also includes one or more chain extenders present in the core in an amount of up to 30 parts per 100 parts of polyol.
50. The floor or wall covering sheet of claim 42, wherein: The core also includes one or more catalysts present in the core in an amount of up to 2 parts per 100 parts of polyol.
51. The floor or wall covering sheet of claim 42, wherein: The core includes one or more dispersants present in the core in an amount of up to 10 parts per 100 parts of polyol.
52. The floor or wall covering sheet of claim 42, wherein: The core also includes one or more fillers present in the core in an amount of up to 500 parts per 100 parts of polyol.
53. The floor or wall covering sheet of claim 42, wherein: The core includes one or more surfactants present in the core in an amount of up to 2 parts per 100 parts of polyol.
54. The floor or wall covering sheet of claim 42, wherein: The core also includes one or more moisture scavengers present in the core in an amount of up to 10 parts per 100 parts of polyol.
55. The floor or wall covering sheet of claim 42, wherein: The core polyol comprises 1% to 40% by weight of one or more recycled materials.
56. The floor or wall covering sheet of claim 42, wherein: The isocyanate is present in the core in an amount of 100 to 250 parts per 100 parts of polyol.
57. The floor or wall covering sheet of claim 42, wherein: The protective layer includes polyurethane.
58. A floor or wall covering sheet according to claim 57, characterised in that: The polyurethane of the protective layer includes an isocyanate and a polyol made at least in part from one or more recycled materials.
59. The floor or wall covering sheet of claim 42, wherein: The one or more recycled materials of the core polyol include polyester terephthalate carpet fibers.
60. The floor or wall covering sheet of claim 43, wherein: The one or more recycled materials of the polyol of the cushion include polyester terephthalate carpet fibers.
61. The floor or wall covering sheet of claim 42, wherein: The one or more recycled materials of the core polyol include polyester terephthalate plastic bottles.
62. The floor or wall covering sheet of claim 43, wherein: The one or more recycled materials of the polyol of the liner include polyester terephthalate plastic bottles.
63. The floor or wall covering sheet of claim 42, wherein: The core also includes one or more glycols.
64. The floor or wall covering sheet of claim 42, wherein: The one or more diols include polytetrahydrofuran.
65. The floor or wall covering sheet of claim 42, wherein: The isocyanate of the core comprises a polyisocyanate.
66. A floor or wall covering panel according to claim 65, characterised in that: The polyisocyanate has an NCO content of 25 wt.% to 35 wt.%.
67. The floor or wall covering sheet of claim 65, characterized in that: The polyisocyanate includes methylene diphenyl diisocyanate.
68. A floor or wall covering sheet according to claim 67, characterised in that: The methylene diphenyl diisocyanate is selected from 2,2'-MDI, 2,4'-MDI and 4,4'-MDI.
69. A floor or wall covering sheet according to claim 67, characterized in that: The methylene diphenyl diisocyanate has an NCO content of 27.5 wt.%, a viscosity of 0.14 Pa·s at 25° C., and a density of 1.20 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of 2.
2.
70. The floor or wall covering sheet of claim 67, wherein: The methylene diphenyl diisocyanate has an NCO content of 31.5 wt.%, a viscosity of 0.2 Pa·s at 25° C., and a density of 1.23 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.0002 mmHg at 25°C, and a functionality of 2.
7.
71. The floor or wall covering sheet of claim 67, wherein: The methylene diphenyl diisocyanate has an NCO content of 32.4 wt.%, a viscosity of 0.017 Pa·s at 25° C., and a density of 1.22 g / cm at 25° C. 3 , an initial boiling point of 190°C at 5 mmHg, a vapor pressure of 0.00001 mmHg at 25°C, and a functionality of 2.
01.
72. The floor or wall covering sheet of claim 49, wherein: The one or more chain extenders are selected from the group consisting of butanediol, diethylene glycol, ethylene glycol, propylene glycol, diethanolamine, trimethylolpropane, and combinations thereof.
73. A floor or wall covering panel according to claim 50, characterized in that: The one or more catalysts are selected from the group consisting of metal-based catalysts, gel catalysts, and thermally activated catalysts.
74. A floor or wall covering panel according to claim 42, characterized in that: The core also comprises polyvinyl butyral.
75. A floor or wall covering panel according to claim 42, characterized in that: The sheet exhibits a perpendicular dimensional stability of 0.05-0.25% at 80°C.
76. A floor or wall covering panel according to claim 42, characterized in that: The panels exhibited a vertical dimensional stability of 0.08-0.25% at 80°C.
77. A floor or wall covering panel according to claim 42, characterized in that: The sheet exhibits a vertical dimensional stability of 0.05-0.20% at 80°C.
78. A floor or wall covering panel according to claim 42, characterized in that: The sheet exhibits a vertical dimensional stability of 0.05-0.15% at 80°C.
79. A floor or wall covering panel according to claim 42, characterized in that: The panels exhibited a vertical dimensional stability of 0.08-0.20% at 80°C.
80. A floor or wall covering panel according to claim 42, characterized in that: The panels exhibited a vertical dimensional stability of 0.08-0.15% at 80°C.
81. A floor or wall covering panel according to claim 42, characterized in that: The sheet exhibits a vertical dimensional stability of 0.10-0.25% at 80°C.
82. A floor or wall covering panel according to claim 42, characterized in that: The sheet exhibited a vertical dimensional stability of 0.10-0.15% at 80°C.
83. A floor or wall covering panel according to claim 42, characterized in that: The core exhibits a flexural strength between 30-65 MPa.
Citation Information
Patent Citations
Water-blown, flame retardant rigid polyurethane foam
CN101316875A
Panel with fire barrier
CN105008122A
Method for producing sandwich components
CN109415481A
Pyrrolidine based catalysts for use in polyurethane materials
IN201617028255A
Polyol for polyurethane
JP2000017068A