Aluminum alloy magnetic field assisted CMT arc additive manufacturing device and method
By using magnetic field-assisted CMT arc technology in aluminum alloy additive manufacturing to refine grains and improve welding wire utilization, the problems of forming quality and height in aluminum alloy additive manufacturing are solved.
Patent Information
- Application Number
- CN202211465994.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-22
AI Technical Summary
In the aluminum alloy additive manufacturing process, there are defects such as poor surface quality, pores, segregation and cracks, and the thickness of the welding wire is small, making it difficult to meet high manufacturing requirements.
An aluminum alloy magnetic field-assisted CMT arc additive manufacturing device is used to generate a longitudinal magnetic field through the main coil to rotate the molten pool to refine the grains, and generate an opposite magnetic field through the secondary coil to shrink the arc into an elliptical shape, reducing the amount of transverse melting and increasing the number of layers. high.
It can effectively refine the organizational grains of metal components, improve mechanical properties, reduce pores, and improve the utilization rate and layer height of welding wire.
Smart Images

Figure CN115673492B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum alloy magnetic field assisted CMT arc additive manufacturing device and method, belonging to the technical field of additive manufacturing. Background Art
[0002] In recent years, with the rapid development of aerospace, rail transit and other fields, traditional manufacturing methods can no longer meet the requirements of rapid manufacturing of large structural parts and complex parts. Additive manufacturing technology, as a new manufacturing technology, can achieve rapid manufacturing of complex parts. Cold metal transfer technology (CMT) is an improved type of gas metal arc welding based on droplet short-circuit transfer. Compared with traditional short-circuit transfer, the current in the short-circuit stage is very small, which reduces welding heat input, eliminates spatter caused by excessive current density, and improves wire utilization.
[0003] Aluminum alloys are widely used in the industrial field because of their light weight, easy processing, good fluidity, good weldability, and good electrical conductivity. There are many difficulties in the additive manufacturing process of aluminum alloys, such as poor surface quality, and defects such as pores, segregation, and cracks in the formed structure. Introducing a longitudinal magnetic field during arc additive manufacturing can cause the arc to rotate, causing the charged metal droplets to generate Lorentz force, changing the flow of the molten pool, thereby changing the crystallization of the molten pool, refining the grains, and improving the mechanical properties of the components. In addition, the fluidity of aluminum alloys is very good, resulting in a smaller weld thickness, which requires more welding wires to reach a higher height during the additive manufacturing process. Therefore, it is urgent to develop aluminum alloy arc additive manufacturing devices and methods to improve the quality and height of additive manufacturing. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an aluminum alloy magnetic field assisted CMT arc additive manufacturing device and method in view of the shortcomings of the prior art. The present invention can stir the molten pool to make the microstructure grains of the additively manufactured metal components more refined and the mechanical properties better. At the same time, it can effectively reduce the pores in the metal wall and effectively improve the utilization rate of the welding wire.
[0005] This solution is achieved through the following technical measures: an aluminum alloy magnetic field assisted CMT arc additive manufacturing device, which includes:
[0006] Two telescopic frames are symmetrically arranged, and the opposite ends of the two telescopic frames are detachably connected. The two telescopic frames are connected to form a gantry bracket, and the sleeve of the welding gun is passed through and fixed in the middle of the gantry bracket;
[0007] The main coil, the upper end of which is detachably fixed to the bottom of the sleeve, generates a longitudinal magnetic field when the main coil is energized, and the Lorentz force generated by the longitudinal magnetic field acts on the molten droplet and the molten pool;
[0008] There are two auxiliary coils, which are fixedly mounted on opposite ends of the two telescopic frames. When the telescopic frames are at their maximum length, the height positions of the two auxiliary coils correspond to the height positions of the arcs. The two auxiliary coils are connected to opposite currents to generate opposite magnetic fields, which generate two forces toward the arcs. The two opposite forces shrink the arc into an elliptical shape, and the lateral narrowing of the arc reduces the lateral melting amount of the welding wire and causes it to stack in height, thereby increasing the layer height.
[0009] Preferably, the lowest end of the main coil is flush with or higher than the bottom outlet of the sleeve.
[0010] Preferably, the main coil includes an electromagnetic core, an electromagnetic enameled coil and an exoskeleton, the electromagnetic core is a cylindrical iron core, the exoskeleton is sleeved and fixed on the outside of the electromagnetic core, and the electromagnetic enameled coil is wound on the exoskeleton; the top of the exoskeleton is symmetrically fixed with a plurality of arc-shaped fixing rings adapted to the shape of the sleeve along its circumferential center, a spacing is left between the opposite ends of two adjacent arc-shaped fixing rings, and ear plates are respectively fixed to the outer sides of the opposite ends of two adjacent arc-shaped fixing rings, and the two ear plates are fixedly connected by a bolt assembly.
[0011] Preferably, the electromagnet core is made of DT4C pure iron, the core material of the electromagnetic enameled coil is copper bare wire, the outer insulation material is polyester enameled wire, the outer skeleton is a high-temperature resistant plastic skeleton made of PPS; the telescopic frame is an aluminum alloy frame.
[0012] Preferably, the structure of the secondary coil is the same as that of the primary coil, and the size of the secondary coil is smaller than that of the primary coil.
[0013] Preferably, the telescopic frame comprises a top seat, two front and rear sliding brackets and two front and rear U-shaped brackets with openings facing each other, the opposite ends of the two top seats in the two telescopic frames are respectively integrally formed with connecting ear plates, the connecting ear plates of the two top seats are detachably connected by bolt assemblies, and the opposite ends of the two top seats are respectively provided with semicircular grooves adapted to the shape of the sleeve, the upper ends of the two sliding brackets are respectively fixedly connected to the front and rear ends of the bottom of one end of the top seat away from the sleeve, the lower ends of the two sliding brackets are respectively slidably connected to the two U-shaped brackets, and the sliding bracket and the U-shaped bracket are respectively provided with a plurality of screw holes along their length directions, the topmost screw hole in the U-shaped bracket and the corresponding screw hole on the sliding bracket are threadedly connected with bolts, and one end of the bolt extending out of the sliding bracket is threadedly connected with a locking nut; the bottoms of the opposite sides of the two U-shaped brackets are respectively integrally formed with square frames, and the two ends of the secondary coil are respectively fixed on the two square frames.
[0014] The present invention also provides an aluminum alloy magnetic field assisted CMT arc additive manufacturing method based on the aluminum alloy magnetic field assisted CMT arc additive manufacturing device, which comprises the following steps:
[0015] (1) According to the sleeve size of the welding gun, adjust the arc fixing ring at the upper end of the main coil so that the arc fixing ring is fixed on the sleeve of the welding gun;
[0016] (2) Fix the two secondary coils at the lower ends of the two telescopic frames respectively, adjust the two telescopic frames to the shortest, and select the placement position of the substrate. Before placing the substrate, use an angle grinder and a rust-removing wire brush to remove the oxide layer on the substrate;
[0017] (3) Fix the substrate with a fixture and adjust the length of the telescopic frame so that the secondary coil can act on the arc, and pre-process the substrate at the same time;
[0018] (4) Test the performance of the formed part and determine the forming parameters: adjust the arc current, voltage, welding speed, wire feeding speed and the excitation current of the main coil and auxiliary coil through multiple preliminary experiments;
[0019] (5) During the forming process, after each layer of weld is formed, a certain dwell time is reserved, and a steel brush is used to remove the oxide film on the newly formed weld before welding the next layer of weld.
[0020] Preferably, the arc current is 80-140A, the arc voltage range is 10.5-12.7V, the welding speed is 0.3-0.7m / min, the wire feeding speed is 4-7m / min, the excitation current of the main coil and the auxiliary coil is 1-6A and uses alternating current.
[0021] Preferably, the pretreatment work in step (3) is to clean the rust-removed substrate with an ultrasonic cleaner, air-dry with ethanol, and then preheat the substrate with a flamethrower to increase the temperature for forming the first two layers of welds.
[0022] Preferably, the residence time in step (5) is 0.5-5 min.
[0023] Beneficial effects of the present invention: In the aluminum alloy magnetic field assisted CMT arc additive manufacturing device and method of the present invention, the Lorentz force generated by the longitudinal magnetic field of the main coil affects the molten droplets and the molten pool, so that the microstructure grains of the metal components manufactured by additive manufacturing are more refined and the mechanical properties are better, and the pores in the metal wall can be effectively reduced; in addition, the two secondary coils are connected to opposite currents, which generate magnetic fields in opposite directions and two forces toward the arc. The two opposite forces narrow the arc and shrink it into an elliptical shape, narrow the lateral arc, reduce the amount of lateral melting of the welding wire, reduce the lateral metal flow, and stack it in height to increase the layer height. For metals with good fluidity, the higher the stacking, the greater the molten width and the lower the height, so the increase of the secondary coil can effectively improve the utilization rate of the welding wire. It can be seen that compared with the prior art, the present invention has outstanding substantial characteristics and significant progress, and the beneficial effects of its implementation are also obvious. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic structural diagram of the aluminum alloy magnetic field assisted CMT arc additive manufacturing device in the present invention.
[0025] Figure 2 Schematic diagram of the connection structure between the main coil and the sleeve Figure 1 .
[0026] Figure 3 Schematic diagram of the connection structure between the main coil and the sleeve Figure 2 .
[0027] Figure 4 It is a schematic diagram of the connection structure between the auxiliary coil and the telescopic frame.
[0028] Figure 5 The internal structure of the main coil Figure 1 .
[0029] Figure 6 The internal structure of the main coil Figure 2 .
[0030] Figure 7 The main coil is shown in Figure 1. Figure 1 .
[0031] Figure 8 The main coil is shown in Figure 1. Figure 2 .
[0032] Fig. 9 The function of the auxiliary coil is shown in Figure 2. Figure 1 .
[0033] Fig.10 The function of the auxiliary coil is shown in Figure 2. Figure 2 .
[0034] In the figure, 1-main coil, 2-telescopic frame, 3-secondary coil, 4-secondary coil, 5-arc-shaped fixing ring, 6-sleeve, 7-welding wire, 8-main coil wiring port, 9-threaded hole, 10-electromagnetic enameled coil, 11-bolt, 12-secondary coil fixing screw hole, 13-secondary coil wiring port, 14-screw hole, 15-electromagnetic core, 16-exoskeleton, 17-arc, 18-base plate, 19-top seat, 20-sliding bracket, 21-U-shaped bracket. DETAILED DESCRIPTION
[0035] In order to clearly illustrate the technical features of this solution, this solution is described below through specific implementation methods and in conjunction with the accompanying drawings.
[0036] An aluminum alloy magnetic field assisted CMT arc additive manufacturing device, comprising:
[0037] The telescopic frame 2 is an aluminum alloy frame and two of them are symmetrically arranged. The aluminum alloy frame is light in weight, which can avoid the problem of reduced stability of equipment installation due to excessive weight. The opposite ends of the two telescopic frames 2 are detachably connected. After the two telescopic frames 2 are connected, a gantry bracket is formed. The sleeve 6 of the welding gun is fixed through the middle of the gantry bracket.
[0038] The main coil 1, the upper end of the main coil 1 is detachably fixed to the bottom of the sleeve 6, such as Figure 2 As shown, the lowest end of the main coil 1 is flush with or higher than the bottom outlet of the sleeve 6 to avoid the arc 17 from burning the equipment during forming. When the main coil 1 is energized, a longitudinal magnetic field is generated, and the Lorentz force generated by the longitudinal magnetic field acts on the molten droplet and the molten pool;
[0039] There are two auxiliary coils, namely auxiliary coil 3 and auxiliary coil 4, which are fixedly mounted on opposite ends of two telescopic frames 2. The positions of auxiliary coil 3 and auxiliary coil 4 are adjusted according to the position of the arc, and the positions of auxiliary coil 3 and auxiliary coil 4 are adjusted by adjusting the length of the telescopic frame 2, such as Fig.10 As shown, when the telescopic frame 2 is at the maximum length, the height positions of the auxiliary coils 3 and 4 correspond to the height position of the arc 17. The auxiliary coils 3 and 4 are connected to opposite currents, generating opposite magnetic fields and two forces toward the arc. The two opposite forces shrink the arc 17 into an elliptical shape, and the lateral arc 17 becomes narrower, which reduces the amount of the welding wire 7 melted in the lateral direction and causes the welding wire 7 to stack in height, thereby increasing the layer height.
[0040] The main coil 1 includes an electromagnetic core 15, an electromagnetic enameled coil 10 and an outer frame 16. The electromagnetic core 15 is a cylindrical iron core. The outer frame 16 is fixed on the outer side of the electromagnetic core 15, and the electromagnetic enameled coil 10 is wound on the outer frame 16. The electromagnetic core 15 is made of DT4C pure iron. The DT4C pure iron material has low coercivity, high magnetic flux, high saturation magnetization intensity, and high cost performance. The wire core material of the electromagnetic enameled coil 10 is copper bare wire, and the outer insulation material is polyester enameled wire. The outer frame 16 is a high-temperature resistant plastic frame made of PPS; the top of the outer frame 16 is symmetrically fixed with a plurality of arc-shaped fixing rings 5 that are adapted to the shape of the sleeve 6 along its circumferential center, and a spacing is left between the opposite ends of the two adjacent arc-shaped fixing rings 5, and the outer sides of the opposite ends of the two adjacent arc-shaped fixing rings 5 are respectively fixed with ear plates, and the two ear plates are fixedly connected by a bolt assembly, and the arc-shaped fixing ring 5 is provided with a threaded hole 9 that is threadedly connected to the bolt assembly.
[0041] The function of the main coil 1 is that during the operation of the CMT machine, the longitudinal magnetic field is as follows Figure 7 As shown, the interaction with the particles in the arc 17 generates Lorentz force, causing the arc to rotate, increasing the preheating area of the weld, making more melting of the welding wire 7, and making better use of the wire. At the same time, the Lorentz force will also cause the molten droplet at the bottom of the elongated welding wire 7 to rotate, causing the spread of the weld to spread around and increase the weld width. In addition, according to the judgment of the Lorentz force, due to the combined effect of the magnetic field intensity component and the current component, as shown in FIG. Figure 8 As shown, a rotating force is generated in the molten pool, B is the magnetic field, the direction is perpendicular to the substrate 18, I is the current, and the arrow is the direction. At the same time, an alternating current is used to generate a periodic rotating force in the opposite direction in the molten pool, thereby stirring the molten pool, refining the grains, and making the mechanical properties of the organization stronger.
[0042] The structure of the secondary coil 3 and the secondary coil 4 is the same as that of the main coil 1, and the size of the secondary coil 3 and the secondary coil 4 is smaller than that of the main coil 1. The secondary coil 3 and the secondary coil 4 are connected to opposite currents to generate magnetic fields in opposite directions. Since the current of the arc 17 is downward, according to the left-hand rule, two forces toward the arc 17 are generated, causing the arc 17 to shrink and become elliptical. Since the arc 17 shrinks in both directions, the melting amount of the welding wire 7 in these two directions is reduced, and the stacking in the height direction increases the layer height. It should be noted that even if there is a preheating step for the substrate 18, the best time to use the secondary coil 3 and the secondary coil 4 is to adjust and use them after stacking the first few layers, because the temperature of the first few layers is relatively low and the spread of the weld is poor. At this time, the use of the secondary coil 3 and the secondary coil 4 will result in a narrower molten width, making the upper and lower performances of the entire metal wall inconsistent.
[0043] The telescopic frame 2 includes a top seat 19, two front and rear sliding brackets 20, and two front and rear U-shaped brackets 21 with openings facing each other. The opposite ends of the two top seats 19 in the two telescopic frames 2 are respectively integrally formed with connecting ear plates, and the connecting ear plates of the two top seats 19 are detachably connected by bolt assemblies, and the opposite ends of the two top seats 19 are respectively provided with semicircular grooves adapted to the shape of the sleeve, and the upper ends of the two sliding brackets 20 are respectively fixedly connected to the front and rear ends of the bottom of one end of the top seat 19 away from the sleeve 6, and the lower ends of the two sliding brackets 20 are respectively slidably connected to the two U-shaped brackets 21, and the upper edges of the sliding brackets 20 and the U-shaped brackets 21 are respectively connected to the two U-shaped brackets 21. A plurality of screw holes 14 are respectively provided in the length direction of the U-shaped bracket 21, and a bolt 11 is threadedly connected to the uppermost screw hole 14 in the U-shaped bracket 21 and the corresponding screw hole 14 on the sliding bracket 20. One end of the bolt 11 extending out of the sliding bracket 20 is threadedly connected to a locking nut. After the relative positions of the U-shaped bracket 21 and the sliding bracket 20 are adjusted to the right position, the relative positions of the U-shaped bracket 21 and the sliding bracket 20 can be fixed by using the bolt 11 and the locking nut. The bottoms of the opposite sides of the two U-shaped brackets 21 are respectively integrally formed with square frames, and the two ends of the secondary coil 3 and the secondary coil 4 are respectively fixed on the two square frames.
[0044] The present invention also provides an aluminum alloy magnetic field assisted CMT arc additive manufacturing method based on the aluminum alloy magnetic field assisted CMT arc additive manufacturing device, which comprises the following steps:
[0045] (1) According to the length of the sleeve 6 of the welding gun, adjust the position of the arc-shaped fixing ring 5 at the upper end of the main coil 1, insert the screw in the bolt assembly into the screw hole 9 of the arc-shaped fixing ring 5, and then tighten the nut in the bolt assembly to fix the arc-shaped fixing ring 5 on the sleeve 6 of the welding gun;
[0046] (2) Fix the auxiliary coil 3 and the auxiliary coil 4 at the lower ends of the two telescopic frames 2 respectively, adjust the two telescopic frames 2 to the shortest, and select the placement position of the substrate 18. Before placing the substrate 18, use an angle grinder and a rust-removing wire brush to remove the oxide layer on the substrate 18;
[0047] (3) Fix the substrate 18 with a fixture, and adjust the length of the telescopic frame 2 so that the secondary coil 3 and the secondary coil 4 can act on the arc 17. At the same time, pre-process the substrate 18. The pre-processing work is as follows: clean the rust-removed substrate 18 with an ultrasonic cleaner, air-dry with ethanol, and then preheat the substrate 18 with a flamethrower to increase the temperature of the first two layers of welds to avoid the metal wall of the component being wide at the top and narrow at the bottom due to the low temperature causing the metal to not spread;
[0048] (4) Testing the performance of the formed part and determining the forming parameters: Through multiple preliminary experiments, adjusting the current, voltage, welding speed, wire feeding speed of the arc 17 and the excitation current of the main coil 1, the auxiliary coil 3 and the auxiliary coil 4; the current of the arc 17 is 80-140A, the voltage range of the arc 17 is 10.5-12.7V, the welding speed is 0.3-0.7m / min, the wire feeding speed is 4-7m / min, and the excitation current of the main coil 1, the auxiliary coil 3 and the auxiliary coil 4 is 1-6A and uses AC current;
[0049] (5) During the forming process, after each layer of weld is formed, a certain dwell time of 0.5-5 minutes is reserved, and a steel brush is used to remove the oxide film on the newly formed weld before welding the next layer of weld. The dwell time has two functions: one is to provide sufficient cooling time for the metal to avoid heat accumulation and metal flow, which will damage the forming; the other is to provide sufficient time to remove the oxide layer on the newly formed weld to ensure the quality of the forming.
[0050] Technical features not described in the present invention can be implemented by existing technologies and will not be described in detail here. The present invention is not limited to the above specific embodiments, and changes, modifications, additions or substitutions made by ordinary technicians in the field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for manufacturing aluminum alloy by magnetic field-assisted CMT arc additive manufacturing. Its characteristics are: It is based on an aluminum alloy magnetic field assisted CMT arc additive manufacturing device, and the aluminum alloy magnetic field assisted CMT arc additive manufacturing device includes: Two telescopic frames are symmetrically arranged, and the opposite ends of the two telescopic frames are detachably connected. The two telescopic frames are connected to form a gantry bracket, and the sleeve of the welding gun is passed through and fixed in the middle of the gantry bracket; The main coil, the upper end of which is detachably fixed to the bottom of the sleeve, generates a longitudinal magnetic field when the main coil is energized, and the Lorentz force generated by the longitudinal magnetic field acts on the molten droplet and the molten pool; the main coil includes an outer frame, and the top of the outer frame is symmetrically fixed with a plurality of arc-shaped fixing rings adapted to the shape of the sleeve along its circumferential center; Two auxiliary coils are provided, and the two auxiliary coils are respectively fixedly mounted at opposite ends of the two telescopic frames. When the telescopic frames are at their maximum length, the height positions of the two auxiliary coils correspond to the height positions of the electric arcs. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method comprises the following steps: (1) According to the sleeve size of the welding gun, adjust the arc fixing ring at the upper end of the main coil so that the arc fixing ring is fixed on the sleeve of the welding gun; (2) Fix the two secondary coils at the lower ends of the two telescopic frames respectively, adjust the two telescopic frames to the shortest, and select the placement position of the substrate. Before placing the substrate, use an angle grinder and a rust-removing wire brush to remove the oxide layer on the substrate; (3) Fix the substrate with a fixture and adjust the length of the telescopic frame so that the secondary coil acts on the arc. At the same time, pre-process the substrate. The pre-processing work is to clean the rust-removed substrate with an ultrasonic cleaner, air-dry it with ethanol, and then preheat the substrate with a flamethrower to increase the temperature for forming the first two layers of welds. (4) Test the performance of the formed part and determine the forming parameters: adjust the arc current, voltage, welding speed, wire feeding speed and the excitation current of the main coil and auxiliary coil through multiple preliminary experiments; (5) During the forming process, after each layer of weld is formed, a certain dwell time is reserved, and a steel brush is used to remove the oxide film on the newly formed weld before welding the next layer of weld; The two auxiliary coils are connected to opposite currents, which generate opposite magnetic fields and two forces toward the arc. The two opposite forces cause the arc to shrink into an elliptical shape. The lateral arc becomes narrower, which reduces the amount of wire melted in the lateral direction and increases the layer height by stacking it in height. The best time to use the two auxiliary coils is to adjust them after stacking the first few layers.
2. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 1, Its characteristics are: The lowest end of the main coil is flush with or higher than the bottom outlet of the sleeve.
3. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 2, Its characteristics are: The main coil also includes an electromagnetic core and an electromagnetic enameled coil, wherein the electromagnetic core is a cylindrical iron core, the outer frame is fixedly mounted on the outer side of the electromagnetic core, and the electromagnetic enameled coil is wound on the outer frame; a spacing is left between the opposite ends of two adjacent arc-shaped fixing circles, and ear plates are respectively fixedly connected to the outer sides of the opposite ends of the two adjacent arc-shaped fixing circles, and the two ear plates are fixedly connected by a bolt assembly.
4. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 3, Its characteristics are: The electromagnet core is made of DT4C pure iron, the core material of the electromagnetic enameled coil is copper bare wire, the outer insulation material is polyester enameled wire, the outer frame is a high-temperature resistant plastic frame made of PPS; the telescopic frame is an aluminum alloy frame.
5. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 4, Its characteristics are: The structure of the secondary coil is the same as that of the primary coil, and the size of the secondary coil is smaller than that of the primary coil.
6. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 5, Its characteristics are: The telescopic frame comprises a top seat, two front and rear sliding brackets and two front and rear U-shaped brackets with openings facing each other, the opposite ends of the two top seats in the two telescopic frames are respectively integrally formed with connecting ear plates, the connecting ear plates of the two top seats are detachably connected by bolt assemblies, and the opposite ends of the two top seats are respectively provided with semicircular grooves adapted to the shape of the sleeve, the upper ends of the two sliding brackets are respectively fixedly connected to the front and rear ends of the bottom of one end of the top seat away from the sleeve, the lower ends of the two sliding brackets are respectively slidably connected to the two U-shaped brackets, and the sliding bracket and the U-shaped bracket are respectively provided with a plurality of screw holes along their length directions, the uppermost screw hole in the U-shaped bracket and the corresponding screw hole on the sliding bracket are threadedly connected with bolts, and one end of the bolt extending out of the sliding bracket is threadedly connected with a locking nut; the bottoms of the opposite sides of the two U-shaped brackets are respectively integrally formed with square frames, and the two ends of the secondary coil are respectively fixed on the two square frames.
7. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to any one of claims 1 to 6, Its characteristics are: The arc current is 80-140A, the arc voltage range is 10.5-12.7V, the welding speed is 0.3-0.7m / min, the wire feeding speed is 4-7m / min, the excitation current of the main coil and the auxiliary coil is 1-6A and uses alternating current.
8. The aluminum alloy magnetic field assisted CMT arc additive manufacturing method according to claim 7, Its characteristics are: The residence time in step (5) is 0.5-5 min.
Citation Information
Cited By
Device and method for assisting electric arc additive manufacturing by stable magnetic field
CN116460392A