Special dispersion optical glass

By adjusting the proportions of components such as SiO2, Nb2O5, ZrO2, BaO, Na2O, etc., a special dispersion optical glass with a refractive index of 1.68 to 1.76 and an ABE number of 30 to 39 was developed, which solved the problem of cracking and easy-to-breaking of optical glass during processing and The problem of large thermal expansion coefficient achieves low thermal expansion coefficient and negative abnormal dispersion, meeting the application needs of high-end optoelectronic products.

CN115677209BActive Publication Date: 2024-12-03CDGM OPTICAL GLASS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211272912.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-18
Publication Date
2024-12-03
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Existing optical glasses are prone to rupture during processing, with a large coefficient of thermal expansion leading to poor thermal shock resistance, and it is difficult to achieve low relative partial dispersion and negative abnormal dispersion.

Method used

Special dispersion optical glass with SiO2, Nb2O5, ZrO2, BaO, Na2O and other components are used to adjust the proportion of each component to control the refractive index between 1.68 and 1.76, the Abbe number is between 30 and 39, and the relative part of the dispersion is below 0.7500. The thermal expansion coefficient is below 95×10-7/K, achieving low thermal expansion coefficient and negative abnormal dispersion.

Benefits of technology

It realizes the special dispersion optical glass used in high-end optoelectronic products, with the desired refractive index and Abbe number, and has a low thermal expansion coefficient and relative partial dispersion, meeting the application needs of high-end products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003895812190000131
    Figure BDA0003895812190000131
  • Figure BDA0003895812190000151
    Figure BDA0003895812190000151
  • Figure BDA0003895812190000171
    Figure BDA0003895812190000171
Patent Text Reader

Abstract

The present invention provides a special dispersion optical glass, the components of which are expressed in weight percentage and contain: SiO2: 26-42%; Nb2O5: 21-40%; ZrO2: 0.5-12%; BaO: 6-20%; Na2O: 3-18%, wherein (SiO2+Nb2O5) / BaO is 2.5-10.0. Through reasonable component design, the special dispersion optical glass obtained by the present invention has the desired refractive index and Abbe number, and also has a lower thermal expansion coefficient and relative partial dispersion P g,F , and negative anomalous dispersion, meeting the application requirements of high-end optoelectronic products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an optical glass, in particular to a special dispersion optical glass with lower relative partial dispersion, negative anomalous dispersion and lower thermal expansion coefficient. Background Art

[0002] In recent years, with the rapid development of smart phones, in-vehicle imaging, surveillance and security, optical glasses with a refractive index of 1.68 to 1.76 and an Abbe number of 30 to 39 have been widely used. In order to increase the degree of freedom in the design of optical systems, optical glasses are expected to have a variety of different properties. Therefore, optical glasses with properties suitable for eliminating or minimizing the residual chromatic aberration of the secondary spectrum have attracted much attention, especially those with low relative partial dispersion (P g,F ) and negative anomalous dispersion optical glass. On the other hand, due to the large thermal expansion coefficient, optical glass is prone to breakage during processing, reducing the yield rate of glass processing. At the same time, the large thermal expansion coefficient will cause the glass to have poor thermal shock resistance, thus limiting the application of optical glass.

[0003] Therefore, a product with a lower thermal expansion coefficient, a refractive index of 1.68 to 1.76, an Abbe number of 30 to 39, and a lower relative partial dispersion (P g,F ) and negative anomalous dispersion, which are of great significance to the development of optoelectronics. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for providing ... g,F ) is a special dispersion optical glass with low chromatic anomalous dispersion and negative dispersion.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] (1) Special dispersion optical glass, the components of which, expressed in weight percentage, contain: SiO2: 26-42%; Nb2O5: 21-40%; ZrO2: 0.5-12%; BaO: 6-20%; Na2O: 3-18%, wherein (SiO2+Nb2O5) / BaO is 2.5-10.0.

[0007] (2) The special dispersion optical glass according to (1), wherein the components, expressed in weight percentage, further contain: B2O3: 0-10%; and / or MgO: 0-6%; and / or CaO: 0-10%; and / or SrO: 0-6%; and / or Li2O: 0-5%; and / or K2O: 0-8%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or TiO2: 0-5%; and / or ZnO: 0-8%; and / or Ln2O3: 0-5%; and / or Al2O3: 0-5%; and / or a clarifier: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0008] (3) Special dispersion optical glass, containing SiO2, Nb2O5, ZrO2, BaO, and Na2O, wherein the composition is expressed in weight percentage, (SiO2+Nb2O5) / BaO is 2.5 to 10.0, and the refractive index of the special dispersion optical glass is n d is 1.68~1.76, Abbe number v d 30~39, relative partial dispersion P g,F Less than 0.7500, relative partial dispersion deviation value ΔP g,F is less than 0, the thermal expansion coefficient α -30 / 70℃ 95×10 -7 / K or less.

[0009] (4) The special dispersion optical glass according to (3), wherein the components, expressed in weight percentage, include: SiO2: 26-42%; and / or Nb2O5: 21-40%; and / or ZrO2: 0.5-12%; and / or BaO: 6-20%; and / or Na2O: 3-18%; and / or B2O3: 0-10%; and / or MgO: 0-6%; and / or CaO: 0-10%; and / or SrO: 0-6%; and / or Li2O: 0-5%; and / or K 2O: 0-8%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or TiO2: 0-5%; and / or ZnO: 0-8%; and / or Ln2O3: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0010] (5) The special dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: RO: 7-35%, preferably RO: 11-30%, more preferably RO: 13-25%; and / or RO / SiO2 is 0.2-1.2, preferably RO / SiO2 is 0.25-1.0, more preferably RO / SiO2 is 0.3-0.8, and further preferably RO / SiO2 is 0.4-0.7; and / or RO / Nb2O5 is 0.2-1.5, preferably RO / Nb2O5 is 0.3-1.2, more preferably RO / Nb2O5 is 0.4-1.0, and further preferably RO / Nb2O5 is 0.4-0.8, wherein RO is the total content of MgO, CaO, SrO and BaO.

[0011] (6) The special dispersion optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following seven conditions:

[0012] 1) B2O3 / SiO2 is less than 0.3, preferably B2O3 / SiO2 is less than 0.25, more preferably B2O3 / SiO2 is less than 0.2, and further preferably B2O3 / SiO2 is 0.01 to 0.15;

[0013] 2) B2O3 / BaO is 1.4 or less, preferably B2O3 / BaO is 1.0 or less, more preferably B2O3 / BaO is 0.8 or less, and further preferably B2O3 / BaO is 0.1 to 0.5;

[0014] 3) (ZrO2+ZnO) / BaO is 0.05 to 1.5, preferably (ZrO2+ZnO) / BaO is 0.1 to 1.0, more preferably (ZrO2+ZnO) / BaO is 0.15 to 0.8, and further preferably (ZrO2+ZnO) / BaO is 0.2 to 0.6;

[0015] 4) (SiO2 + Nb2O5) / BaO is 3.0 to 8.0, preferably (SiO2 + Nb2O5) / BaO is 3.5 to 7.0, and more preferably (SiO2 + Nb2O5) / BaO is 4.0 to 6.0;

[0016] 5) (BaO+CaO) / Na2O is 0.5 to 5.0, preferably (BaO+CaO) / Na2O is 0.8 to 4.0, more preferably (BaO+CaO) / Na2O is 1.0 to 3.0, and further preferably (BaO+CaO) / Na2O is 1.2 to 2.5;

[0017] 6) (Na2O + Nb2O5) / SiO2 is 0.6 to 2.0, preferably (Na2O + Nb2O5) / SiO2 is 0.7 to 1.7, more preferably (Na2O + Nb2O5) / SiO2 is 0.8 to 1.5, and further preferably (Na2O + Nb2O5) / SiO2 is 1.0 to 1.5;

[0018] 7) (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.5, preferably (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.3, more preferably (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.2, and further preferably (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is 0.01~0.15.

[0019] (7) The special dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 28-40%, preferably SiO2: 30-37%; and / or B2O3: 0-6%, preferably B2O3: 0.5-5%; and / or Nb2O5: 25-35%, preferably Nb2O5: 27-33%; and / or ZrO2: 1-10%, preferably ZrO2: 2-8%; and / or BaO: 8-18%, preferably BaO: 10-16%; and / or MgO: 0-3%, preferably MgO: 0-1%; and / or CaO: 0.5-8%, preferably CaO: 1-6%; and / or SrO: 0-3%, preferably SrO: 0-1%; and / or Na2O: 5-15%, preferably Na2O: 7-13%; and / or Li2O: 0-3%, Li2O: 0-2% is preferred; and / or K2O: 0-5%, preferably K2O: 0-3%; and / or WO3: 0-3%, preferably WO3: 0-1%; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%; and / or TiO2: 0-3%, preferably TiO2: 0-1%; and / or ZnO: 0-4%, preferably ZnO: 0-1%; and / or Ln2O3: 0-3%. 3%, preferably Ln2O3: 0-1%; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%; and / or clarifier: 0-0.8%, preferably clarifier: 0-0.5%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0020] (8) The special dispersion optical glass according to any one of (1) to (4), wherein its components do not contain TiO2; and / or do not contain WO3; and / or do not contain Ta2O5; and / or do not contain ZnO; and / or do not contain Ln2O3; and / or do not contain Li2O; and / or do not contain Al2O3, and the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3.

[0021] (9) The special dispersion optical glass according to any one of (1) to (4), wherein the refractive index n of the special dispersion optical glass is d is 1.68 to 1.76, preferably 1.69 to 1.75, more preferably 1.70 to 1.74, further preferably 1.705 to 1.735, and / or the Abbe number v d It is 30 to 39, preferably 31 to 38, more preferably 32 to 37, and further preferably 33.50 to 36.50.

[0022] (10) The relative partial dispersion P of the special dispersion optical glass according to any one of (1) to (4) g,F is 0.7500 or less, preferably 0.7000 or less, more preferably 0.6500 or less, further preferably 0.6000 or less, and / or the relative partial dispersion deviation value ΔP g,F It is less than 0, preferably -0.0001 or less, more preferably -0.0005 or less, and further preferably -0.0010 or less.

[0023] (11) The density ρ of the special dispersion optical glass according to any one of (1) to (4) is 3.8 g / cm 3 Below, preferably 3.7 g / cm 3 Below, more preferably 3.6g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 95×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less; and / or λ 80 Less than or equal to 400nm, preferably λ 80 Less than or equal to 390nm, more preferably λ 80 Less than or equal to 385nm; and / or λ5 less than or equal to 350nm, preferably λ5 less than or equal to 340nm, more preferably λ5 less than or equal to 335nm; and / or weather resistance CR is 2 or more, preferably 1; and / or acid resistance stability D A 2 or more, preferably 1; and / or water resistance stability D W2 or more, preferably 1; and / or Knoop hardness H K 500×10 7 Pa or more, preferably 510×10 7 Pa or more, more preferably 520×10 7 Pa or above; and / or wear degree F A 180 to 220, preferably 185 to 215, more preferably 190 to 210; and / or Young's modulus E is 8000×10 7 ~11000×10 7 Pa, preferably 8500×10 7 ~10500×10 7 Pa, more preferably 9000×10 7 ~10000×10 7 Pa.

[0024] (12) A glass preform made of any one of the special dispersion optical glasses described in (1) to (11).

[0025] (13) An optical element is made of any one of the special dispersion optical glasses described in (1) to (11), or is made of the glass preform described in (12).

[0026] (14) An optical instrument comprising the special dispersion optical glass described in any one of (1) to (11) and / or the optical element described in (13).

[0027] The beneficial effects of the present invention are as follows: through reasonable component design, the special dispersion optical glass obtained by the present invention has a desired refractive index and Abbe number, and also has a lower thermal expansion coefficient and relative partial dispersion (P g,F ), as well as negative anomalous dispersion, meet the application of high-end optoelectronic products. DETAILED DESCRIPTION

[0028] The following is a detailed description of the embodiments of the special dispersion optical glass of the present invention, but the present invention is not limited to the following embodiments and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although the repeated description may be appropriately omitted, the main purpose of the invention is not limited thereto. In this article, the special dispersion optical glass of the present invention is sometimes referred to as optical glass or glass.

[0029] [Special dispersion optical glass]

[0030] The following is an explanation of the range of each component (ingredient) of the special dispersion optical glass of the present invention. In the present invention, unless otherwise specified, the content and total content of each component are all expressed in weight percentage (wt%), that is, the content and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts and hydroxides used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.

[0031] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values ​​listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0032] <Essential Components and Optional Components>

[0033] SiO2 is an essential component of the optical glass of the present invention, and is the skeleton of the optical glass of the present invention. It can improve the acid resistance and viscosity of the glass and reduce the abrasiveness of the glass. In the present invention, the above effects are obtained by containing more than 26% SiO2, preferably more than 28% SiO2, and more preferably more than 30% SiO2. On the other hand, if the content of SiO2 is too much, the melting performance of the glass deteriorates, the high temperature viscosity increases, and inclusions such as bubbles or stones are likely to appear in the glass. Therefore, the upper limit of the content of SiO2 in the present invention is 42%, preferably 40%, and more preferably 37%.

[0034] B2O3 has the effect of improving the thermal stability and melting property of glass, but when its content is higher than 10%, the chemical stability, weather resistance and devitrification resistance of glass decrease. Therefore, the content of B2O3 in the present invention is 0-10%, preferably 0-6%, and more preferably 0.5-5%.

[0035] In some embodiments, the ratio B2O3 / SiO2 between the content of B2O3 and the content of SiO2 is controlled to be below 0.3, which is beneficial to improving the weather resistance and Young's modulus of the glass and improving the light transmittance of the glass. Therefore, preferably B2O3 / SiO2 is below 0.3, more preferably B2O3 / SiO2 is below 0.25, further preferably B2O3 / SiO2 is below 0.2, and further preferably B2O3 / SiO2 is 0.01 to 0.15.

[0036] ZrO2 can increase the refractive index of glass, improve the chemical stability of glass, adjust short-wave special dispersion, and reduce the ΔP of glass.g,F If the content is too high, the glass will be difficult to melt, the melting temperature will rise, and inclusions will appear inside the glass and the light transmittance will decrease. Therefore, the content of ZrO2 is 0.5-12%, preferably 1-10%, and more preferably 2-8%.

[0037] In some embodiments, the content of alkaline earth metal oxide RO (RO is the total content of MgO, CaO, SrO, and BaO) is controlled within the range of 7 to 35%, so that the glass can more easily obtain the desired optical constants and optimize the chemical stability and abrasion resistance of the glass. Therefore, RO is preferably 7 to 35%, more preferably 11 to 30%, and further preferably 13 to 25%.

[0038] In some embodiments, the ratio of RO to SiO2, RO / SiO2, is controlled within the range of 0.2 to 1.2, which can improve the hardness of the glass and prevent the chemical stability of the glass from deteriorating. Therefore, RO / SiO2 is preferably 0.2 to 1.2, and more preferably RO / SiO2 is 0.25 to 1.0. Furthermore, controlling RO / SiO2 within the range of 0.3 to 0.8 can further optimize the abrasiveness and Young's modulus of the glass. Therefore, RO / SiO2 is further preferably 0.3 to 0.8, and RO / SiO2 is further preferably 0.4 to 0.7.

[0039] MgO can reduce the relative partial dispersion of glass, but when the MgO content is too high, the refractive index of the glass is difficult to meet the design requirements, and the anti-crystallization performance and stability of the glass are reduced. Therefore, the MgO content is limited to 0-6%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that MgO is not contained.

[0040] CaO can adjust the optical constants of glass, improve the chemical stability of glass, improve the processing performance of glass, reduce the high temperature viscosity and surface tension of glass, and reduce the difficulty of glass production. If its content is too high, the resistance to devitrification of glass will be reduced. Therefore, the content of CaO is 0-10%, preferably 0.5-8%, and more preferably 1-6%.

[0041] SrO can adjust the refractive index and Abbe number of glass, but if its content is too high, the chemical stability of the glass will decrease, and the cost of the glass will also increase rapidly. Therefore, the content of SrO is limited to 0-6%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that SrO is not contained.

[0042] BaO can increase the refractive index, melting property and thermal stability of glass, improve the abrasiveness and light transmittance of glass, but if its content is too high, the density of glass increases and the resistance to devitrification decreases. Therefore, the content of BaO is 6 to 20%, preferably 8 to 18%, and more preferably 10 to 16%.

[0043] In some embodiments, the ratio B2O3 / BaO between the content of B2O3 and the content of BaO is controlled to be less than 1.4, which can improve the chemical stability and Young's modulus of the glass and prevent the hardness of the glass from deteriorating. Therefore, preferably B2O3 / BaO is less than 1.4, more preferably B2O3 / BaO is less than 1.0, further preferably B2O3 / BaO is less than 0.8, and further preferably B2O3 / BaO is 0.1 to 0.5.

[0044] Nb2O5 is a high-refractive and high-dispersion component that can increase the refractive index, dispersion and devitrification resistance of glass, reduce the thermal expansion coefficient of glass, and does not significantly increase P g,F Value and ΔP g,F If the content of Nb2O5 is too high, the thermal stability and weather resistance of the glass will decrease, and the light transmittance will decrease. Therefore, the content of Nb2O5 is in the range of 21 to 40%, preferably 25 to 35%, and more preferably 27 to 33%.

[0045] In some embodiments, the ratio of RO to Nb2O5, RO / Nb2O5, is controlled within the range of 0.2 to 1.5, which can reduce the density of the glass while increasing the light transmittance of the glass. Therefore, RO / Nb2O5 is preferably 0.2 to 1.5, and more preferably RO / Nb2O5 is 0.3 to 1.2. Furthermore, controlling RO / Nb2O5 within the range of 0.4 to 1.0 can further optimize the abrasiveness and thermal expansion coefficient of the glass. Therefore, RO / Nb2O5 is further preferably 0.4 to 1.0, and RO / Nb2O5 is further preferably 0.4 to 0.8.

[0046] In some embodiments, the ratio of the total content of SiO2 and Nb2O5 (SiO2+Nb2O5) to the content of BaO ((SiO2+Nb2O5) / BaO) is controlled within the range of 2.5 to 10.0, so that the glass can have a lower P g,F Value and ΔP g,Fvalue, while reducing the thermal expansion coefficient of the glass. Therefore, it is preferred that (SiO2+Nb2O5) / BaO is 2.5-10.0, and it is more preferred that (SiO2+Nb2O5) / BaO is 3.0-8.0. Furthermore, by controlling (SiO2+Nb2O5) / BaO within the range of 3.5-7.0, the abrasion resistance and weather resistance of the glass can be further optimized. Therefore, it is further preferred that (SiO2+Nb2O5) / BaO is 3.5-7.0, and it is further preferred that (SiO2+Nb2O5) / BaO is 4.0-6.0.

[0047] Li2O can lower the transition temperature of glass, adjust the high temperature viscosity of glass, and improve the melting property of glass, but a high content of Li2O is detrimental to the chemical stability and cost efficiency of glass. Therefore, the content of Li2O in the present invention is 5% or less, preferably 3% or less, and more preferably 2% or less. In some embodiments, it is further preferred that Li2O is not contained.

[0048] Na2O can improve the melting property of glass and improve the melting effect of glass. It also helps to reduce the P g,F Value and ΔP g,F In the present invention, the above effect is obtained by containing more than 3% Na2O. If the content of Na2O exceeds 18%, the chemical stability and weather resistance of the glass are reduced, so the content of Na2O is 3-18%, preferably 5-15%, and more preferably 7-13%.

[0049] In some embodiments, the ratio of the total content of Na2O and Nb2O5 Na2O+Nb2O5 to the content of SiO2 (Na2O+Nb2O5) / SiO2 is controlled within the range of 0.6 to 2.0, so that the glass can have a lower P g,F Value and ΔP g,F value, while optimizing the abrasion resistance of the glass. Therefore, it is preferred that (Na2O+Nb2O5) / SiO2 is 0.6-2.0, and it is more preferred that (Na2O+Nb2O5) / SiO2 is 0.7-1.7. Furthermore, controlling (Na2O+Nb2O5) / SiO2 within the range of 0.8-1.5 can further improve the weather resistance of the glass and prevent the density of the glass from increasing. Therefore, it is further preferred that (Na2O+Nb2O5) / SiO2 is 0.8-1.5, and it is further preferred that (Na2O+Nb2O5) / SiO2 is 1.0-1.5.

[0050] In some embodiments, the ratio of the total content of BaO and CaO (BaO+CaO) to the content of Na2O ((BaO+CaO) / Na2O) is controlled within the range of 0.5 to 5.0, so that the glass can have a lower Pg,F Value and ΔP g,F value, while improving the chemical stability of the glass and preventing the glass density from rising. Therefore, it is preferred that (BaO+CaO) / Na2O is 0.5-5.0, and it is more preferred that (BaO+CaO) / Na2O is 0.8-4.0. Furthermore, by controlling (BaO+CaO) / Na2O within the range of 1.0-3.0, the Young's modulus and weather resistance of the glass can be further optimized. Therefore, it is further preferred that (BaO+CaO) / Na2O is 1.0-3.0, and it is further preferred that (BaO+CaO) / Na2O is 1.2-2.5.

[0051] K2O has the effect of improving the thermal stability and melting property of glass, but if its content exceeds 8%, the devitrification resistance and chemical stability of glass deteriorate. Therefore, in the present invention, the content of K2O is 0 to 8%, preferably 0 to 5%, and more preferably 0 to 3%.

[0052] WO3 can improve the refractive index and mechanical strength of glass. If the content of WO3 exceeds 5%, the thermal stability of glass decreases and the resistance to devitrification decreases. Therefore, the upper limit of WO3 content is 5%, preferably 3%, and more preferably 1%. In some embodiments, it is further preferred that WO3 is not contained.

[0053] Ta2O5 has the effect of increasing the refractive index and improving the devitrification resistance of glass, but if its content is too high, the thermal stability of the glass will decrease, the density will increase, and the optical constants will be difficult to control within the desired range; on the other hand, compared with other components, Ta2O5 is very expensive, and its usage should be minimized from the perspective of practicality and cost. Therefore, the content of Ta2O5 in the present invention is limited to 0-5%, preferably 0-3%, more preferably 0-1%, and it is further preferred that Ta2O5 is not contained.

[0054] TiO2 has the function of increasing the refractive index and dispersion of glass. A proper amount of it can make the glass more stable and reduce the viscosity of the glass. If the content of TiO2 exceeds 5%, the tendency of glass crystallization increases, the transition temperature rises, and the P g,F Value and ΔP g,F Therefore, in the present invention, the content of TiO2 is 5% or less, preferably 3% or less, more preferably 1% or less, and even more preferably no TiO2 is contained.

[0055] In some embodiments, the ratio (B2O3+Li2O+TiO2) / (BaO+Nb2O5) between the total content of B2O3, Li2O, and TiO2 (B2O3+Li2O+TiO2) and the total content of BaO and Nb2O5 (BaO+Nb2O5) is controlled to be below 0.5, which can improve the chemical stability of the glass and prevent the light transmittance of the glass from decreasing. Therefore, it is preferred that (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is below 0.5, and it is more preferred that (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is below 0.3. Furthermore, by controlling (B2O3+Li2O+TiO2) / (BaO+Nb2O5) to be below 0.2, the hardness and thermal expansion coefficient of the glass can be further optimized. Therefore, it is further preferred that (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.2, and it is further preferred that (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is 0.01 to 0.15.

[0056] ZnO can adjust the refractive index and dispersion of glass, reduce the high temperature viscosity and transition temperature of glass, so that glass can be melted at a lower temperature, thereby improving the light transmittance of glass. If the content of ZnO is too high, the difficulty of glass molding increases, the anti-crystallization performance deteriorates, and it is not conducive to the glass to obtain negative anomalous dispersion. Therefore, the content of ZnO is 0 to 8%, preferably 0 to 4%, and more preferably 0 to 1%. In some embodiments, it is further preferred that ZnO is not contained.

[0057] In some embodiments, the ratio of the total content of ZrO2 and ZnO ZrO2+ZnO to the content of BaO (ZrO2+ZnO) / BaO is controlled within the range of 0.05 to 1.5, so that the glass can have a lower P g,F Value and ΔP g,F value, while preventing the Young's modulus of the glass from deteriorating. Therefore, it is preferred that (ZrO2+ZnO) / BaO is 0.05-1.5, and it is more preferred that (ZrO2+ZnO) / BaO is 0.1-1.0. Furthermore, by controlling (ZrO2+ZnO) / BaO within the range of 0.15-0.8, the thermal expansion coefficient of the glass can be further reduced and the hardness of the glass can be increased. Therefore, it is further preferred that (ZrO2+ZnO) / BaO is 0.15-0.8, and it is further preferred that (ZrO2+ZnO) / BaO is 0.2-0.6.

[0058] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3) is a component that improves the refractive index and chemical stability of glass. By controlling the content of Ln2O3 to 5% or less, the devitrification resistance of glass can be prevented from decreasing. Preferably, the upper limit of the content range of Ln2O3 is 3%, and more preferably, the upper limit is 1%. In some embodiments, it is further preferred that Ln2O3 is not contained.

[0059] Al2O3 can improve the chemical stability of glass, but when its content exceeds 5%, the melting property and light transmittance of glass deteriorate. Therefore, the content of Al2O3 in the present invention is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. In some embodiments, it is further preferred that Al2O3 is not contained.

[0060] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO, SnO2, and CeO2 as a clarifier, the clarification effect of the glass can be improved and the bubble degree of the glass can be improved. The content of the clarifier is preferably 0-0.8%, and the content of the clarifier is more preferably 0-0.5%. When the content of Sb2O3 exceeds 1%, the clarification performance of the glass tends to decrease. At the same time, due to its strong oxidizing effect, it promotes the corrosion of the platinum or platinum alloy vessel for melting glass and the deterioration of the forming mold. Therefore, the content of Sb2O3 is preferably 0-1%, more preferably 0-0.8%, and further preferably 0-0.5%. SnO and SnO2 can also be used as clarifiers, but when their content exceeds 1%, the tendency of glass coloring increases, or when the glass is heated, softened, and molded again, Sn will become the starting point of crystal nucleation, resulting in a tendency of devitrification. Therefore, the content of SnO2 in the present invention is preferably 0-1%, more preferably 0-0.8%, and further preferably 0-0.5%; the content of SnO is preferably 0-1%, more preferably 0-0.8%, and further preferably 0-0.5%. The role and content ratio of CeO2 are consistent with those of SnO2, and its content is preferably 0-1%, more preferably 0-0.8%, further preferably 0-0.5%, and further preferably no CeO2 is contained.

[0061] <Components that should not be contained>

[0062] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.

[0063] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.

[0064] In order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.

[0065] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.

[0066] Next, the properties of the special dispersion optical glass of the present invention will be described.

[0067] <Refractive Index and Abbe Number>

[0068] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.

[0069] In some embodiments, the refractive index (n d ) has a lower limit of 1.68, preferably 1.69, more preferably 1.70, and further preferably 1.705. In some embodiments, the refractive index (n d ) has an upper limit of 1.76, a preferred upper limit of 1.75, a more preferred upper limit of 1.74, and a further preferred upper limit of 1.735.

[0070] In some embodiments, the Abbe number (ν d ) has a lower limit of 30, preferably 31, more preferably 32, and further preferably 33.50. In some embodiments, the Abbe number (ν d ) has an upper limit of 39, a preferred upper limit of 38, a more preferred upper limit of 37, and a further preferred upper limit of 36.50.

[0071] <density>

[0072] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.

[0073] In some embodiments, the density (ρ) of the special dispersion optical glass of the present invention is 3.8 g / cm 3 Below, preferably 3.7 g / cm 3 Below, more preferably 3.6g / cm 3 the following.

[0074] <Coefficient of Thermal Expansion>

[0075] Thermal expansion coefficient of optical glass (α -30 / 70℃ ) The data at -30~70℃ were tested according to the method specified in GB / T7962.16-2010.

[0076] In some embodiments, the thermal expansion coefficient (α -30 / 70℃ ) is 95×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less.

[0077] <Color>

[0078] The short-wave transmission spectrum characteristics of the special dispersion optical glass of the present invention are expressed by the coloring degree (λ 80 and λ5). 80 It refers to the wavelength when the glass transmittance reaches 80%. 80 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 80%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in The amount expressed by λ also includes the transmittance of the surface reflection loss on the above surface of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, in glass, λ 80 A small value of means that the glass itself is less colored and has a high light transmittance.

[0079] In some embodiments, the λ of the special dispersion optical glass of the present invention is 80 Less than or equal to 400nm, preferably λ 80 Less than or equal to 390nm, more preferably λ 80Less than or equal to 385nm.

[0080] In some embodiments, the λ5 of the special dispersion optical glass of the present invention is less than or equal to 350 nm, preferably λ5 is less than or equal to 340 nm, and more preferably λ5 is less than or equal to 335 nm.

[0081] <Weather resistance>

[0082] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test box with a saturated water vapor environment of 90% relative humidity, alternately cycle every 1 hour at 40-50°C, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:

[0083] Table 1.

[0084]

[0085] In some embodiments, the weather resistance (CR) of the special dispersion optical glass of the present invention is Class 2 or higher, preferably Class 1.

[0086] <Knoop hardness>

[0087] Knoop hardness of optical glass (H K ) The test shall be carried out according to the test method specified in GB / T7962.18-2010.

[0088] In some embodiments, the Knoop hardness (H K ) is 500×10 7 Pa or more, preferably 510×10 7 Pa or more, more preferably 520×10 7 Pa or above.

[0089] <Relative partial dispersion and relative partial dispersion deviation value>

[0090] The relative partial dispersion (P g,F ) and relative partial dispersion deviation (ΔP g,F ) origin.

[0091] The relative partial dispersion for wavelengths x and y is expressed by the following equation (1):

[0092] P x,y =(n x -n y ) / (n F -n C ) (1)

[0093] According to the Abbe number formula, for most so-called "normal glasses" (H-K6 and F4 are selected as "normal glasses" below), the following formula (2) is valid:

[0094] P x,y =m x,y ·v d +b x,y (2)

[0095] This linear relationship is based on P x,y is the vertical coordinate, v d It is represented by the horizontal axis, where m x,y is the slope, b x,y is the intercept.

[0096] As is known to all, the correction of the secondary spectrum, i.e. the achromatization of more than two wavelengths, requires at least one glass that does not conform to the above formula (2) (i.e. its P x,y The deviation value deviates from Abbe's empirical formula), and its deviation value is expressed as ΔP x,y If it is expressed, then each P x,y -v d The point is shifted by ΔP relative to the "normal line" that conforms to the above formula (2) x,y Quantity, so that the ΔP of each glass x,y The value can be obtained using the following formula (3):

[0097] P x,y =m x,y ·v d +b x,y +ΔP x,y (3)

[0098] Therefore, ΔP x,y It quantitatively represents the deviation characteristics of special dispersion compared with "normal glass".

[0099] Therefore, the relative partial dispersion (P g,F ) and relative partial dispersion deviation (ΔP g,F ) is calculated as follows (4) and (5):

[0100] P g,F =(n g -n F ) / (n F -n C ) (4)

[0101] ΔP g,F =P g,F -0.6457+0.001703v d (5)

[0102] In some embodiments, the relative partial dispersion (P g,F ) is 0.7500 or less, preferably 0.7000 or less, more preferably 0.6500 or less, and further preferably 0.6000 or less.

[0103] In some embodiments, the relative partial dispersion deviation value (ΔP g,F ) is less than 0, preferably -0.0001 or less, more preferably -0.0005 or less, and further preferably -0.0010 or less.

[0104] <Abrasion>

[0105] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:

[0106] F A =V / V0×100=(W / ρ) / (W0 / ρ0)×100

[0107] Where: V—volume wear of the sample being tested;

[0108] V0—Volume loss of standard sample;

[0109] W—mass wear loss of the sample being tested;

[0110] W0—standard sample mass wear;

[0111] ρ—density of the sample being tested;

[0112] ρ0—standard sample density.

[0113] In some embodiments, the abrasiveness (F A ) has a lower limit of 180, preferably 185, and more preferably 190, and the abrasion degree (F A ) has an upper limit of 220, a preferred upper limit of 215, and a more preferred upper limit of 210.

[0114] <Water resistance stability>

[0115] Water resistance stability of optical glass (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0116] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.

[0117] <Acid resistance stability>

[0118] Acid resistance stability of optical glass (D A ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0119] In some embodiments, the acid resistance stability (D A ) is 2 or more types, preferably 1 type.

[0120] <Young's modulus>

[0121] Young's modulus (E) is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.

[0122]

[0123] G=V S 2 ρ

[0124] Where: E is Young's modulus, Pa;

[0125] G is the shear modulus, Pa;

[0126] V T is the shear wave velocity, m / s;

[0127] V S is the longitudinal wave velocity, m / s;

[0128] ρ is the glass density, g / cm 3 .

[0129] In some embodiments, the lower limit of the Young's modulus (E) of the special dispersion optical glass of the present invention is 8000×10 7 Pa, the preferred lower limit is 8500×10 7 Pa or more, and the lower limit is more preferably 9000×10 7 Pa or above.

[0130] In some embodiments, the upper limit of the Young's modulus (E) of the special dispersion optical glass of the present invention is 11000×10 7 Pa, the upper limit is preferably 10500×10 7 Pa, and the upper limit is more preferably 10000×10 7 Pa.

[0131] [Method for producing optical glass]

[0132] The manufacturing method of the special dispersion optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, etc.), boric acid, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1200-1500°C for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.

[0133] [Glass preforms and optical components]

[0134] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.

[0135] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.

[0136] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.

[0137] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.

[0138] [Optical instruments]

[0139] The optical element formed by the special dispersion optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.

[0140] Example

[0141] <Special dispersion optical glass example>

[0142] In order to further clearly illustrate and describe the technical solutions of the present invention, the following non-limiting examples are provided.

[0143] This embodiment adopts the above optical glass manufacturing method to obtain special dispersion optical glass having the composition shown in Tables 2 to 4. In addition, the characteristics of each glass are measured by the test method described in the present invention, and the measurement results are shown in Tables 2 to 4.

[0144] Table 2.

[0145]

[0146]

[0147] Table 3.

[0148]

[0149]

[0150]

[0151] Table 4.

[0152]

[0153]

[0154] <Glass Preform Example>

[0155] The glass obtained from special dispersion optical glass embodiments 1 to 24# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, double convex lenses, double concave lenses, plano-convex lenses, and plano-concave lenses.

[0156] <Optical Element Embodiment>

[0157] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.

[0158] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.

[0159] <Optical Instrument Embodiment>

[0160] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.

Claims

1. Special dispersion optical glass, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 30-42%; Nb2O5: 25-40%; ZrO2: 0.5-12%; BaO: 6-20%; Na2O: 3-18%; Li2O: 0-5%, among which (SiO2+Nb2O5) / BaO is 2.5-6.0, (BaO+CaO) / Na2O is 0.5-5.0, and B2O3 / BaO is 0.047-1.

4.

2. The special dispersion optical glass according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: B2O3: 0.5-10%; and / or MgO: 0-6%; and / or CaO: 0-10%; and / or SrO: 0-6%; and / or K2O: 0-8%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or TiO2: 0-5%; and / or ZnO: 0-8%; and / or Ln2O3: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

3. Special dispersion optical glass, characterized in that: Contains SiO2, Nb2O5, ZrO2, BaO, and Na2O, and the components are expressed in weight percentage as follows: (SiO2+Nb2O5) / BaO is 2.5-6.0, (BaO+CaO) / Na2O is 0.5-5.0, and B2O3 / BaO is 0.047-1.

4. The refractive index of the special dispersion optical glass is n d is 1.68~1.76, Abbe number v d 30~39, relative partial dispersion P g,F Less than 0.7500, relative partial dispersion deviation value ΔP g,F is less than 0, the thermal expansion coefficient α -30 / 70℃ 95×10 -7 / K or less.

4. The special dispersion optical glass according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 30-42%; and / or Nb2O5: 25-40%; and / or ZrO2: 0.5-12%; and / or BaO: 6-20%; and / or Na2O: 3-18%; and / or B2O3: 0.5-10%; and / or MgO: 0-6%; and / or CaO: 0-10%; and / or SrO: 0-6%; and / or Li2O: 0-5%; and / or K2O: 0-8%; and / or WO3: 0-5%; and / or Ta2O5: 0-5%; and / or TiO2: 0-5%; and / or ZnO: 0-8%; and / or Ln2O3: 0-5%; and / or Al2O3: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

5. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: RO: 7-35%; and / or RO / SiO2 is 0.2-1.2; and / or RO / Nb2O5 is 0.2-1.5, wherein RO is the total content of MgO, CaO, SrO and BaO.

6. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: RO: 11-30%; and / or RO / SiO2 is 0.25-1.0; and / or RO / Nb2O5 is 0.3-1.2, wherein RO is the total content of MgO, CaO, SrO and BaO.

7. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: RO: 13-25%; and / or RO / SiO2 is 0.3-0.8; and / or RO / Nb2O5 is 0.4-1.0, wherein RO is the total content of MgO, CaO, SrO and BaO.

8. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: RO / SiO2 is 0.4-0.7; and / or RO / Nb2O5 is 0.4-0.8, and RO is the total content of MgO, CaO, SrO and BaO.

9. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following five conditions: 1) B2O3 / SiO2 is less than 0.3; 2) (ZrO2+ZnO) / BaO is 0.05~1.5; 3) (SiO2+Nb2O5) / BaO is 3.0-6.0; 4) (Na2O+Nb2O5) / SiO2 is 0.6 to 2.0; 5) (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.

5.

10. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 7 conditions: 1) B2O3 / SiO2 is less than 0.25; 2) B2O3 / BaO is 0.047 to 1.0; 3) (ZrO2+ZnO) / BaO is 0.1~1.0; 4) (SiO2+Nb2O5) / BaO is 3.5 to 6.0; 5) (BaO+CaO) / Na2O is 0.8~4.0; 6) (Na2O+Nb2O5) / SiO2 is 0.7 to 1.7; 7) (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.

3.

11. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 7 conditions: 1) B2O3 / SiO2 is less than 0.2; 2) B2O3 / BaO is 0.047 to 0.8; 3) (ZrO2+ZnO) / BaO is 0.15~0.8; 4) (SiO2+Nb2O5) / BaO is 4.0-6.0; 5) (BaO+CaO) / Na2O is 1.0~3.0; 6) (Na2O+Nb2O5) / SiO2 is 0.8 to 1.5; 7) (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is less than 0.

2.

12. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 6 conditions: 1) B2O3 / SiO2 is 0.01 to 0.15; 2) B2O3 / BaO is 0.1 to 0.5; 3) (ZrO2+ZnO) / BaO is 0.2~0.6; 4) (BaO+CaO) / Na2O is 1.2~2.5; 5) (Na2O+Nb2O5) / SiO2 is 1.0 to 1.5; 6) (B2O3+Li2O+TiO2) / (BaO+Nb2O5) is 0.01~0.

15.

13. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 30-40%; and / or B2O3: 0.5-6%; and / or Nb2O5: 25-35%; and / or ZrO2: 1-10%; and / or BaO: 8-18%; and / or MgO: 0-3%; and / or CaO: 0.5-8%; and / or SrO: 0-3%; and / or Na2O: 5-15%; and / or Li2O: 0-3%; and / or K2O: 0-5%; and / or WO3: 0-3%; and / or Ta2O5: 0-3%; and / or TiO2: 0-3%; and / or ZnO: 0-4%; and / or Ln2O3: 0-3%; and / or Al2O3: 0-3%; and / or clarifier: 0-0.8%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

14. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The components are expressed in weight percentage, wherein: SiO2: 30-37%; and / or B2O3: 0.5-5%; and / or Nb2O5: 27-33%; and / or ZrO2: 2-8%; and / or BaO: 10-16%; and / or MgO: 0-1%; and / or CaO: 1-6%; and / or SrO: 0-1%; and / or Na2O: 7-13%; and / or Li2O: 0-2%; and / or K2O: 0-3%; and / or W O3: 0-1%; and / or Ta2O5: 0-1%; and / or TiO2: 0-1%; and / or ZnO: 0-1%; and / or Ln2O3: 0-1%; and / or Al2O3: 0-1%; and / or clarifier: 0-0.5%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

15. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components do not contain TiO2; and / or do not contain WO3; and / or do not contain Ta2O5; and / or do not contain ZnO; and / or do not contain Ln2O3; and / or do not contain Li2O; and / or do not contain Al2O3, and the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and Lu2O3.

16. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the special dispersion optical glass d 1.68~1.76; and / or Abbe number v d It is 30 to 39.

17. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the special dispersion optical glass d 1.69 to 1.75; and / or Abbe number v d It is 31 to 38.

18. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the special dispersion optical glass d 1.70~1.74; and / or Abbe number v d It is 32 to 37.

19. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the special dispersion optical glass d 1.705~1.735; and / or Abbe number v d It is 33.50~36.

50.

20. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The relative partial dispersion P of the special dispersion optical glass g,F is less than 0.7500; and / or relative partial dispersion deviation value ΔP g,F is less than 0.

21. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The relative partial dispersion P of the special dispersion optical glass g,F is less than 0.7000; and / or relative partial dispersion deviation value ΔP g,F Below -0.0001.

22. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The relative partial dispersion P of the special dispersion optical glass g,F is less than 0.6500; and / or relative partial dispersion deviation value ΔP g,F Below -0.0005.

23. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The relative partial dispersion P of the special dispersion optical glass g,F is less than 0.6000; and / or relative partial dispersion deviation value ΔP g,F Below -0.0010.

24. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The density ρ of the special dispersion optical glass is 3.8 g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 95×10 -7 / K or less; and / or λ 80 Less than or equal to 400nm; and / or λ5 less than or equal to 350nm; and / or weather resistance CR is 2 or above; and / or acid resistance stability D A Class 2 or above; and / or water resistance stability D W Class 2 or above; and / or Knoop hardness H K 500×10 7 Pa or above; and / or wear degree F A 180 to 220; and / or Young's modulus E is 8000×10 7 ~11000×10 7 Pa.

25. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The density ρ of the special dispersion optical glass is 3.7 g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 90×10 -7 / K or less; and / or λ 80 Less than or equal to 390nm; and / or λ5 less than or equal to 340nm; and / or weather resistance CR is Class 1; and / or acid resistance stability D A Class 1; and / or water resistance stability D W Class 1; and / or Knoop hardness H K 510×10 7 Pa or above; and / or wear degree F A 185-215; and / or Young's modulus E is 8500×10 7 ~10500×10 7 Pa.

26. The special dispersion optical glass according to any one of claims 1 to 4, characterized in that: The density ρ of the special dispersion optical glass is 3.6 g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less; and / or λ 80 Less than or equal to 385nm; and / or λ5 less than or equal to 335nm; and / or Knoop hardness H K 520×10 7 Pa or above; and / or wear degree F A 190 to 210; and / or Young's modulus E is 9000×10 7 ~10000×10 7 Pa.

27. A glass preform, characterized in that: It is made of the special dispersion optical glass described in any one of claims 1 to 26.

28. An optical element, characterized in that It is made of the special dispersion optical glass described in any one of claims 1 to 26, or is made of the glass preform described in claim 27.

29. An optical instrument, characterized in that Contains the special dispersion optical glass according to any one of claims 1 to 26, and / or contains the optical element according to claim 28.