A method for desulfurizing light naphtha
By using manganese oxide molecular sieves to contact light naphtha at room temperature to 200°C, the problem that existing technology cannot effectively remove mercaptans from light naphtha is solved, and high-precision, high-sulfur capacity pumice is achieved. Naphtha mercaptan removal meets the stringent requirements of the light naphtha isomerization process.
Patent Information
- Application Number
- CN202110870183.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-07-30
AI Technical Summary
The existing technology cannot effectively remove mercaptans from light naphtha with high precision, high sulfur capacity, and low cost at low temperatures, and cannot meet the stringent requirements for sulfur content in the light naphtha isomerization process.
The manganese oxide molecular sieve is contacted with mercaptan-containing light naphtha at room temperature to 200°C, and the special crystal structure of the molecular sieve is used to catalytically convert through adsorption and combination to achieve the production of light naphtha with ultra-low sulfur content.
It achieves high-precision, high-sulfur capacity removal of light naphtha mercaptans at normal pressure, normal temperature or lower temperature, with low cost and simple process, and meets the sulfur content requirements of the light naphtha isomerization process.
Smart Images

Figure BDA0003188826270000091
Abstract
Description
Technical Field
[0001] The invention relates to a method for cleaning industrial oil products, in particular to a method for removing mercaptan from light naphtha components. Background Art
[0002] With the rapid development of my country's petrochemical industry, the production capacity of ethylene has increased year by year, which has led to the continuous increase of the by-product cracking carbon 5 and carbon 6 fractions of ethylene units, thus driving the comprehensive utilization of light naphtha in my country. In particular, affected by the heavy quality of petroleum raw materials, the sulfur content in light naphtha fractions has a tendency to gradually increase. The isomerization process of light naphtha fractions uses precious metal catalysts, which are particularly sensitive to sulfur. Sulfur elements will make the catalysts lose their activity and affect the service life and effect of the catalysts. Desulfurization technology has become an effective measure for its comprehensive utilization. The production of clean light naphtha fractions will create good and high-quality raw materials for downstream utilization. Among sulfides, mercaptan is an important sulfide. Its presence not only makes oil products smell bad, but also reduces the quality and stability of oil products, because mercaptan is an oxidation initiator, which can oxidize and superimpose unstable compounds in oil products to form colloidal substances. Mercaptan is also corrosive and can also cause corrosion of elemental sulfur. Therefore, in the production process of petroleum products, mercaptan must be removed from oil products. In addition, the light naphtha isomerization process requires that the sulfur content in the fraction be reduced to below 0.1 μg / g, which places more stringent requirements on the content of mercaptan sulfur.
[0003] Chinese patent CN1482210A provides a catalytic cracking gasoline adsorption refining technology, which uses two adsorbents to remove the polarity of sulfides in catalytic cracking gasoline. A mixture of aluminum oxide, iron oxide and molecular sieve is used as a carrier, and impregnated metal is used as an active phase to selectively adsorb mercaptan sulfur in gasoline. After selective deep desulfurization, the mercaptan sulfur content in gasoline is less than 10μg / g, and the total sulfur content is less than 300μg / g. Patent CN200410010353.6 heats low-quality gasoline to 20-220℃ and condenses at a volume space velocity of 0.1-10h -1 , it comes into contact with the adsorption desulfurizer under the conditions of normal pressure-0.5Mpa. The sulfur content of gasoline after desulfurization is reduced from 1290ppm to 800-400ppm, and the mercaptan sulfur content is reduced to below 10ppm.
[0004] The above analysis shows that the adsorption desulfurization technology can remove the mercaptan sulfur content of gasoline to below 10ppm, but it still cannot meet the requirement of the light naphtha component that the sulfur content is less than 0.1ppm. Therefore, it is of great significance to develop a method for removing mercaptans from light naphtha components at low temperatures with high precision, high sulfur capacity and low cost. Summary of the invention
[0005] The object of the present invention is to provide a method for removing sulfur from light naphtha to meet the requirements of the light naphtha isomerization process. To achieve the above object, the present invention specifically includes the following contents:
[0006] The invention provides a method for removing mercaptan from light naphtha, which comprises contacting a manganese oxide molecular sieve with a mercaptan-containing light naphtha raw material at room temperature to 200°C.
[0007] The method of the present invention can remove sulfur-containing substances in light naphtha at normal pressure, normal temperature or lower temperature, and purify sulfur-containing substances by adsorption combined with catalytic conversion using the special crystal structure of the molecular sieve to obtain light naphtha with ultra-low sulfur content. The manganese oxide molecular sieve used in the present invention has low cost, high desulfurization accuracy, high sulfur capacity, and high single-pass conversion rate. The production method is easy to operate, simple in process, and is conducive to industrial promotion. DETAILED DESCRIPTION
[0008] The technical scheme of the present invention is further described below according to specific embodiments. The protection scope of the present invention is not limited to the following embodiments, and these examples are listed only for illustrative purposes and are not intended to limit the present invention in any way. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition of this specification shall prevail.
[0009] The sulfur content described in the present invention is generally expressed as the mass content of sulfur element, generally using mass percentage or ppm as the unit of measurement. The light naphtha treated by the method described in the present invention is less than 0.1ppm, which meets the sulfur content requirements of subsequent processes.
[0010] The invention provides a method for removing mercaptan from light naphtha, which comprises contacting a manganese oxide molecular sieve with a mercaptan-containing light naphtha raw material at room temperature to 200°C.
[0011] According to the present invention, the contact conditions are conventional desulfurization conditions or milder conditions than conventional conditions, such as normal pressure, normal temperature to 150°C, and a mass ratio of manganese oxide molecular sieve to mercaptan-containing light naphtha raw material of 1 to 200: 1. The normal temperature in the present invention refers to an ambient temperature that does not require heating, generally 13-35°C, that is, the contact condition temperature range of the present invention can be 15 to 200°C, 20 to 200°C, etc. depending on the ambient temperature.
[0012] The present invention has no particular limitation on the source of the sulfur-containing light naphtha, the type and content of the mercaptan. For example, the mercaptan compound is selected from one or more of methyl mercaptan, ethyl mercaptan, propyl mercaptan, n-butyl mercaptan, 3-methyl-1-butyl mercaptan, and hexyl mercaptan. In some embodiments, the mass ratio of the mercaptan compound to the manganese oxide molecular sieve is 0.1 to 50:1.
[0013] According to the present invention, the place where the desulfurization adsorbent contacts the sulfur-containing light naphtha raw material is not particularly limited, and can be various reactors well known to those skilled in the art, preferably a fixed bed reactor, so that the sulfur-containing light naphtha raw material passes continuously and is quickly separated. During the contact process, the contact efficiency can be increased by various conventional methods to improve the desulfurization effect.
[0014] The manganese oxide molecular sieve of the present invention can be selected from one or more of birnessite, buserite, hydromanganite, ramsonite, cryptomelane and calansite.
[0015] The specific surface area and pore volume of the manganese oxide molecular sieve of the present invention are not particularly limited. Generally, the specific surface area can be 50-300m 2 / g, the pore volume can be 0.2-1.2cm 3 / g.
[0016] The present invention has no particular limitation on the source of the manganese oxide molecular sieve used, which can be a commercial reagent or prepared by itself from raw materials, as long as the composition and content meet the corresponding requirements of the present invention. In order to better implement the method of the present invention, the present invention provides a method for preparing the manganese oxide molecular sieve, which is specifically described as follows:
[0017] (1) subjecting an aqueous solution containing an oxidized manganese compound and a reduced manganese compound to a hydrothermal synthesis reaction; (2) collecting a solid product and washing, drying and calcining the solid product to obtain the manganese oxide molecular sieve.
[0018] Among them, the oxidized manganese compound and the reduced manganese compound in the present invention are relative terms; the oxidized manganese compound generally refers to a compound containing relatively high-valent manganese (such as Mn 7+ , Mn 6+ The reduced manganese compound generally refers to a compound containing relatively low-valent manganese (such as Mn 2+ For example, the oxidized manganese compound is selected from one or more of potassium permanganate, potassium manganate, and sodium permanganate, and the reduced manganese compound is selected from one or more of manganese sulfate, manganese nitrate, manganese acetate, and manganese chloride; preferably, the molar ratio of the oxidized manganese compound to the reduced manganese compound is (0.2-3):1.
[0019] The hydrothermal reaction in step (1) is carried out under conventional conditions in the art, for example, the temperature of the hydrothermal synthesis reaction is 60-200° C., preferably 80-150° C., and the reaction time is 1-36 h, preferably 2-24 h.
[0020] The precipitate obtained in step (1) can be washed as needed. Washing means washing the collected solid product with deionized water until the washing liquid is neutral (for example, the pH value is 6.5 to 7.5).
[0021] The drying and calcining in step (2) are conventional operations in the art, and there is no particular limitation on the relevant conditions. For example, the drying temperature in step (a-3) is 80 to 350° C., preferably 100 to 300° C., and the time is 1 to 24 hours, preferably 2 to 12 hours; the calcining temperature is 200 to 900° C., preferably 250 to 800° C., and the time is 0.5 to 12 hours, preferably 2 to 6 hours. The calcination can be carried out in an air atmosphere or in an inert gas atmosphere, preferably in an N2 atmosphere. Through the above steps, a manganese oxide molecular sieve can be obtained.
[0022] In order to further improve the performance of the desulfurization adsorbent, before the hydrothermal reaction in step (1), an acid is added to the aqueous solution to adjust the pH value of the aqueous solution to 0.2-3; the acid can be a common inorganic acid such as nitric acid, hydrochloric acid, sulfuric acid, or an organic acid such as acetic acid that can achieve the above purpose.
[0023] The method provided by the present invention can directly obtain light naphtha with ultra-low mercaptan content at a relatively low temperature. The manganese oxide molecular sieve has low cost and high desulfurization accuracy, high sulfur capacity and high single-pass conversion rate. The desulfurization method has convenient process and simple operation, which is conducive to industrial promotion.
[0024] The present invention is further described below by means of specific examples. These examples describe preferred implementation schemes but do not constitute limitations to the present invention. Any technician familiar with the profession may use the above-mentioned invention contents to change them into equivalent embodiments with equivalent changes.
[0025] Reagents, Instruments and Tests
[0026] Unless otherwise specified, all reagents used in the present invention are analytically pure and commercially available.
[0027] The model of the XRD diffractometer used in the present invention is an XRD-6000 X-ray powder diffractometer (Shimadzu, Japan), and the XRD test conditions are: Cu target, Kα ray (wavelength λ=0.154nm), tube voltage of 40kV, tube current of 200mA, and scanning speed of 10°(2θ) / min.
[0028] The H2S analysis instrument used in the present invention is a German SICK GMS810 hydrogen sulfide analyzer.
[0029] Preparation Example 1
[0030] Dissolve 3.17 g of potassium permanganate in 40.55 g of deionized water, heat and stir to dissolve to form a potassium permanganate solution, mix it with 5.78 g of 50 wt% manganese sulfate solution, add 6 ml of nitric acid to adjust the pH value of the solution to 1.0, stir evenly, and react at 130°C for 24 hours.
[0031] The generated brown precipitate was filtered and washed with deionized water for several times until the pH of the washing solution was 7, and then the solid product was dried at 120° C. overnight, and then calcined at 400° C. in an air atmosphere for 4 h to obtain manganese oxide molecular sieve A1: OMS-2-Hydro.
[0032] Preparation Example 2
[0033] According to the materials in Preparation Example 1, potassium permanganate solution was mixed with manganese sulfate solution and nitric acid and transferred to a flask equipped with a condenser. The mixture was reacted at 120° C. for 24 h. The other steps were the same as in Preparation Example 1 to obtain manganese oxide molecular sieve A2: OMS-2-Ref.
[0034] Preparation Example 3
[0035] The same steps as in Preparation Example 1 were used for preparation, except that the calcination temperature was different. Manganese oxide molecular sieve A3: OMS-2-Hydro-750 was obtained by calcining at 750° C. in an air atmosphere for 4 h.
[0036] Preparation Example 4
[0037] Manganese oxide molecular sieve was prepared by the same steps as in Preparation Example 1, except that the solid after the hydrothermal reaction was not calcined, to obtain manganese oxide molecular sieve A4: OMS-2-Hydro-750-No.
[0038] Preparation Example 5
[0039] Quickly mix 250 ml of 5.5 mol / L NaOH solution and 200 ml of 0.5 mol / L MnCl2 solution, introduce oxygen into the mixed solution at a flow rate of 50 L / h, and continuously stir the solution.
[0040] After reacting for 4 hours, the reaction solution was filtered with deionized water until the pH value of the solution was 7.0-7.5 and dried at 120°C, and then calcined at 400°C in an air atmosphere for 4 hours to obtain manganese oxide molecular sieve A5: manganese oxide δ-MnO2 (also known as birnessite).
[0041] Preparation Example 6
[0042] Quickly mix 250 ml of 5.5 mol / L NaOH solution and 200 ml of 0.5 mol / L MnCl2 solution, introduce oxygen into the mixed solution at a flow rate of 50 L / h, and continuously stir the solution.
[0043] After reacting for 4 hours, the reaction solution was filtered with deionized water to obtain a mixture with a pH value of 7.0-7.5, which was dispersed in 500 ml of a 1 mol / L MgCl2 solution, stirred for 12 hours, reacted at 100°C for 6 hours, washed and filtered again, dried at 120°C, and then calcined at 400°C in an air atmosphere for 4 hours to obtain manganese oxide molecular sieve A6: manganese oxide molecular sieve OMS-1.
[0044] Comparative Example 1
[0045] The existing commercial light naphtha desulfurization catalyst composed of zinc oxide + copper oxide (1:1 by mass) and manganese oxide D1 was selected.
[0046] XRD analysis was performed on the manganese oxides obtained in the preparation example and the preparation comparison example. A1-A4 all showed the characteristic peak of OMS-2, indicating that they had an OMS-2 molecular sieve structure. A5-A6 showed the characteristic peak of OMS-1, indicating that they had an OMS-1 molecular sieve structure. D1 did not show the characteristic peaks of OMS-1 and OMS-2.
[0047] Example
[0048] The manganese oxides of Preparation Examples 1 to 6 and Comparative Example 1 were evaluated for their desulfurization effects. The reaction process was as follows: 20 ml of oil was added to a reaction flask, different types of mercaptans were added to the reaction flask, stirred evenly, 0.2 g of manganese oxide was added, heated and stirred, and after the reaction was completed, the manganese oxide was filtered out to obtain a liquid product (Example 1 was an industrial oil product, and no additional mercaptan was required).
[0049] Example 1
[0050] Add 20 ml of industrial light naphtha mixed oil into the reaction flask, wherein the industrial light naphtha contains 1.0 ppm of mercaptans (calculated as the mass of sulfur element, including methyl mercaptan, ethyl mercaptan, and propyl mercaptan). Add it into the reaction flask and stir evenly. Add 0.2 g of manganese oxide A1 and stir and react at room temperature and normal pressure for 3 hours. After the reaction is completed, filter out the manganese oxide to obtain a liquid product, and calculate the concentration of methyl mercaptan in the liquid product after the adsorption reaction by gas chromatography.
[0051] Example 2
[0052] The adsorption conversion reaction was carried out by the same steps as in Example 1, except that the thiol content was different, the total thiol content was 11.78 ppm, and the manganese oxide A2 prepared in Preparation Example 2 was used as the adsorbent.
[0053] Example 3
[0054] The adsorption conversion reaction was carried out by the same steps as in Example 1, except that n-hexane was selected as the solvent, propyl mercaptan was used as the removed substance, and the manganese oxide A3 prepared in Preparation Example 3 was used as the adsorbent.
[0055] Example 4
[0056] The adsorption conversion reaction was carried out by the same steps as in Example 1, except that n-heptane was selected as the solvent, n-butyl mercaptan was used as the removed substance, and the manganese oxide A4 prepared in Preparation Example 4 was used as the adsorbent.
[0057] Example 5
[0058] The adsorption conversion reaction was carried out by the same steps as in Example 1, except that isopentane was selected as the solvent, 3-methyl-1-butanethiol was used as the removed substance, and the manganese oxide A5 prepared in Preparation Example 5 was used as the adsorbent.
[0059] Example 6
[0060] The adsorption conversion reaction was carried out by the same steps as in Example 1, except that n-octane was selected as the solvent, hexanethiol was used as the removed substance, and the manganese oxide A6 prepared in Preparation Example 6 was used as the adsorbent.
[0061] Comparative Example 1
[0062] The desulfurization reaction was carried out in the same steps as in Example 1, except that D1 was used as the desulfurizing agent, and the mass of the desulfurizing agent was 0.4 g.
[0063] The specific surface area, pore volume of manganese oxide, and sulfur concentration of the reaction products of Examples 1-6 and Comparative Example 1 are shown in Table 1.
[0064] Table 1.
[0065]
[0066] As can be seen from Table 1, the method of the present invention is significantly more effective than the prior art in removing mercaptans from light naphtha, and has a remarkable effect.
[0067] According to the physicochemical properties of manganese oxide molecular sieve, the special crystal structure of manganese oxide molecular sieve gives full play to its advantages in the field of liquefied gas desulfurization, so that it can have a higher desulfurization depth than the comparative example at normal temperature and pressure. At the same time, the preparation method of the manganese oxide molecular sieve used is simple, with good repeatability, which is conducive to industrial promotion.
[0068] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0069] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0070] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for desulfurizing light naphtha, comprising contacting a manganese oxide molecular sieve with a light naphtha feedstock containing mercaptans, wherein the contact conditions include: The pressure is normal pressure, the temperature is 15~150℃, and the volume space velocity is 0.1-100h -1 ; The manganese oxide molecular sieve is prepared by the following steps: (1) subjecting an aqueous solution containing an oxidized manganese compound and a reduced manganese compound to a hydrothermal synthesis reaction; (2) collecting the solid product and washing, drying and calcining the solid product to obtain the manganese oxide molecular sieve; The molar ratio of the oxidized manganese compound to the reduced manganese compound is (0.2-3):1; Before the hydrothermal synthesis reaction, the method further comprises adding an acid to the aqueous solution to adjust the pH value of the aqueous solution to 0.2-3; The temperature of the hydrothermal synthesis reaction is 60-200°C, and the reaction time is 1-36h; The drying temperature is 80-350° C., and the time is 1-24 hours. The calcination temperature is 200-900° C., and the time is 0.5-12 hours.
2. The method according to claim 1, wherein: The oxidized manganese compound is selected from one or more of potassium permanganate, potassium manganate, and sodium permanganate, and the reduced manganese compound is selected from one or more of manganese sulfate, manganese nitrate, manganese acetate, and manganese chloride.
3. The method according to claim 1, wherein: The contacting is carried out in a fixed bed reactor.