PAN-based carbon fiber precursor oil

By using specific formulas and processes in carbon fiber raw fiber oil agents, the problems of emulsion instability and large particle size are solved, the performance of carbon fiber raw fiber is improved, and the needs of high-performance carbon fiber production are met.

CN115679480BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110828045.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-22
Publication Date
2024-11-01
Estimated Expiration
2041-07-22

AI Technical Summary

Technical Problem

In the prior art, the emulsion is unstable after emulsification of the carbon fiber oil agent, and the oil agent has a large particle size, which affects the performance of the carbon fiber proto-wire. In the production method, the use of modified silicone oil is relatively large, and the emulsion is difficult, which affects the stability of the emulsion.

Method used

Using PAN-based carbon fiber raw silk oil agent formula, including alkylphenol polyoxyethylene ether, quaternary ammonium antistatic agent, side chain amino modified polysiloxane, side chain polyether modified polysiloxane and side chain ring Oxygen modified polysiloxane, and through a specific mixing and stirring process, the acid addition sequence and temperature control, the average particle size of the oil agent is reduced and the emulsion stability is improved.

Benefits of technology

The high stability and uniform dispersion of the oil agent emulsion are achieved, the average particle size of the oil agent on the fiber surface is reduced, the performance of carbon fiber raw silk is improved, and the demand for high-performance carbon fiber production is met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115679480B_ABST
    Figure CN115679480B_ABST
Patent Text Reader

Abstract

The invention relates to a PAN-based carbon fiber precursor oil, which mainly solves the problems of high silicone oil content, high viscosity, difficulty in emulsification, poor uniformity, and large particle size of the carbon fiber precursor oil in the prior art. The invention adopts a PAN-based carbon fiber precursor oil, which comprises the following effective components by weight: 6 to 25 parts of alkylphenol polyoxyethylene ether; 10 to 25 parts of quaternary ammonium salt antistatic agent; 30 to 50 parts of side chain amino modified polysiloxane; 5 to 20 parts of side chain polyether modified polysiloxane; 5 to 15 parts of side chain epoxy modified polysiloxane; and 0.01 to 2 parts of acid, which solves the problem well and has excellent heat resistance, cohesion, smoothness and antistatic properties, and can be used for the production of PAN-based carbon fiber precursor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a PAN-based carbon fiber precursor oil agent and a production method thereof. Background Art

[0002] Carbon fiber is a brittle material, and defects are the main factor restricting its tensile strength. Among all kinds of defects, surface defects account for about 90% and are the source of fracture. Moreover, for defects of the same size, surface defects have a greater impact on tensile strength than internal defects.

[0003] Carbon fiber oil is an essential auxiliary agent for carbon fiber manufacturing and the most effective technology for inhibiting the formation of surface defects in carbon fiber. Its main function is to form a thin film of uniform thickness on the fiber surface to prevent surface defects caused by adhesion and doubling of the tow during the spinning process. It can also greatly reduce the friction and wear between the tow and the roller. During the pre-oxidation and low-temperature carbonization process, it can also prevent the fiber surface from being hot-adhesive or hot-doubling due to local overheating or tar production, thereby protecting the fiber surface from damage. The contribution rate of carbon fiber oil to improving the strength of carbon fiber is about 0.5 to 1.0 GPa. It is one of the key technologies for high-performance carbon fiber and has been monopolized by foreign countries for many years.

[0004] High-quality oil is the key to ensure the quality of oiling. The manufacture of carbon fiber, especially high-performance carbon fiber, has strict requirements on spinning oil. In particular, the average particle size of the oil after emulsification not only affects the stability of the oil emulsion, but also is closely related to the performance of the carbon fiber precursor and carbon fiber after oiling. If it is too large, the stability of the emulsion will deteriorate, and the stability of the oil film attached to the fiber surface will deteriorate, resulting in uneven oil adhesion; if the average particle size is too small, the oil will easily penetrate into the microporous defects on the surface of the precursor, making it difficult to volatilize, causing internal defects of the precursor and affecting the performance of the carbon fiber.

[0005] For example, Chinese patent document CN107503157A uses a self-designed modified silicone oil containing isopropyl alcohol and polyetheramine structure as the main component, and adds polyether modified silicone oil, antioxidant, polyquaternary ammonium salt and non-ionic surfactant to successfully prepare a carbon fiber oil suitable for dry-jet wet spinning process, which solves the problems of oil sticking and becoming brittle at high temperature in the traditional dry-jet wet spinning carbon fiber preparation process. However, the amount of modified silicone oil used in this method is large, and emulsification is difficult. The particle size of some oils even reaches 0.5um, which affects the stability of the emulsion. Summary of the invention

[0006] One of the technical problems to be solved by the present invention is the problem that the emulsion is unstable and the oil particle size is large after emulsification in the prior art. A PAN-based carbon fiber precursor oil is provided, which not only has good antioxidant and heat resistance, but also has high oil emulsion stability and a small average oil particle size. The oil is more evenly dispersed on the fiber surface, which can well meet the needs of polyacrylonitrile-based carbon fiber precursor production.

[0007] The second technical problem to be solved by the present invention is the production method of the above-mentioned oil agent.

[0008] The third technical problem to be solved by the present invention is the application of the above-mentioned oil agent.

[0009] To solve one of the above technical problems, the technical solution of the present invention is as follows:

[0010] PAN-based carbon fiber precursor oil, wherein the effective ingredients include the following components by weight:

[0011] Alkylphenol polyoxyethylene ether, 6-25 parts;

[0012] Quaternary ammonium salt antistatic agent, 10-25 parts;

[0013] Side chain amino-modified polysiloxane, 30-50 parts;

[0014] Side chain polyether modified polysiloxane, 5-20 parts;

[0015] Side chain epoxy modified polysiloxane, 5-15 parts;

[0016] Acid, 0.01 to 2 parts.

[0017] The addition of acid into the PAN-based carbon fiber precursor oil makes the oil emulsion more stable and the average particle size of the oil is greatly reduced.

[0018] As a non-limiting example, the alkylphenol polyoxyethylene ether can be 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, etc.

[0019] As a non-limiting example, the quaternary ammonium antistatic agent can be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, etc.

[0020] By way of non-limiting example, the side chain amino-modified polysiloxane can be 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, and the like.

[0021] As a non-limiting example, the side chain polyether modified polysiloxane can be 6 parts, 7 parts, 9 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, etc.

[0022] As non-limiting examples, the side chain epoxy-modified polysiloxane can be 6 parts, 7 parts, 9 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, and the like.

[0023] By way of non-limiting example, the acid can be 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, and the like.

[0024] In the above technical solution, the acid can be an inorganic acid or an organic acid. The inorganic acid is preferably sulfuric acid, and the organic acid is preferably carboxylic acid or organic sulfonic acid. The organic sulfonic acid is preferably an aromatic organic sulfonic acid. The aromatic organic sulfonic acid is preferably an alkylbenzene sulfonic acid, and further preferably, the alkyl group of the alkylbenzene sulfonic acid is a C1-C4 alkyl group. For example, but not limited to, acetic acid, p-toluenesulfonic acid, 2-methylbenzenesulfonic acid, 4-isopropylbenzenesulfonic acid, etc.

[0025] In the above technical solution, the alkylphenol polyoxyethylene ether is preferably selected from at least one of octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether.

[0026] In the above technical solution, the number of repeating units of ethylene oxide in the alkylphenol polyoxyethylene ether is preferably 2 to 8. For example, but not limited to, the number of repeating units of ethylene oxide in the alkylphenol polyoxyethylene ether is 3, 4, 5, 6, 7, etc.

[0027] In the above technical solution, it is preferred that the quaternary ammonium salt structure contains a quaternary ammonium cation group having the following structural formula 1:

[0028]

[0029] Wherein R is a C10-C20 hydrocarbon group (for example, but not limited to a C11 hydrocarbon group, a C12 hydrocarbon group, a C13 hydrocarbon group, a C14 hydrocarbon group, a C15 hydrocarbon group, a C16 hydrocarbon group, a C17 hydrocarbon group, a C18 hydrocarbon group, a C19 hydrocarbon group, etc.), preferably a straight-connected hydrocarbon group, preferably an alkyl group, preferably a primary alkyl group; R1-R3 are independently selected from C1-C3 hydrocarbon groups, and the sum of the carbon numbers of the three groups of R1, R2 and R3 is less than 6 (for example, but not limited to, the sum of the carbon numbers of the three groups of R1, R2 and R3 is 4, 5 or 6).

[0030] In the above technical solution, the anion in the quaternary ammonium salt structure is preferably X - 、CH3SO3 - 、CH3OSO3 - 、NO3 - or SO4 2- , X is a halogen atom.

[0031] In the above technical solution, the side chain amino-modified polysiloxane is preferably selected from at least one of the side chain monoamino-modified polysiloxane shown in the following structural formula 2 or the side chain diamino-modified polysiloxane shown in the following structural formula 3:

[0032]

[0033] wherein R4 is selected from an alkylene group having 2 to 10 carbon atoms (for example, but not limited to, R4 is selected from an alkylene group having 2 carbon atoms, an alkylene group having 3 carbon atoms, an alkylene group having 4 carbon atoms, an alkylene group having 5 carbon atoms, an alkylene group having 6 carbon atoms, an alkylene group having 7 carbon atoms, an alkylene group having 8 carbon atoms, an alkylene group having 9 carbon atoms, an alkylene group having 10 carbon atoms, etc.), and b / (a+b+c)=0.1-0.8 (for example, but not limited to, b / (a+b+c) is 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, etc.);

[0034]

[0035] wherein R5 and R6 are independently selected from alkylene groups having 2 to 10 carbon atoms (for example, but not limited to, R5 and R6 are independently selected from alkylene groups having 3 carbon atoms, R5 and R6 are independently selected from alkylene groups having 4 carbon atoms, R5 and R6 are independently selected from alkylene groups having 5 carbon atoms, R5 and R6 are independently selected from alkylene groups having 6 carbon atoms, R5 and R6 are independently selected from alkylene groups having 7 carbon atoms, R5 and R6 are independently selected from alkylene groups having 8 carbon atoms, R5 and R6 are independently selected from alkylene groups having 9 carbon atoms, etc.), and e / (d+e+f)=0.1-0.8 (for example, but not limited to, e / (d+e+f) is 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, etc.).

[0036] In the above technical solution, the side chain polyether-modified polysiloxane is preferably selected from at least one of the compounds shown in the following structural formula 4:

[0037]

[0038] wherein i / (h+i+j)=0.1-0.6 (for example, but not limited to, i / (h+i+j) is 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, etc.), R7 is an alkylene group having 2-10 carbon atoms (for example, but not limited to, R7 is an alkylene group having 2 carbon atoms, an alkylene group having 3 carbon atoms, an alkylene group having 4 carbon atoms, an alkylene group having 5 carbon atoms, an alkylene group having 6 carbon atoms, an alkylene group having 7 carbon atoms, an alkylene group having 8 carbon atoms, an alkylene group having 9 carbon atoms, etc.), and 2≤n6≤10 (for example, but not limited to, n6 is 3, 4, 5, 6, 7, 8, 9, etc.).

[0039] In the above technical solution, the side chain epoxy-modified polysiloxane is preferably selected from at least one of the compounds shown in the following structural formula 5:

[0040]

[0041] wherein m / (k+m+n)=0.1-0.8 (for example, but not limited to, m / (k+m+n) is 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, etc.), 1≤n7≤7 (for example, but not limited to, n7 is 2, 3, 4, 5, 6, etc.), 1≤n8≤5 (for example, but not limited to, n8 is 2, 3, 4, etc.).

[0042] In the above technical scheme, the raw silk oil agent preferably includes the active ingredient and water; more preferably, the active ingredient accounts for 10-30% of the total amount of the active ingredient and water by weight (for example, but not limited to 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%).

[0043] To solve the second technical problem of the present invention, the technical solution of the present invention is as follows:

[0044] The method for producing the PAN-based carbon fiber precursor oil comprises the following steps:

[0045] (1) mixing an antistatic agent with a side chain amino-modified polysiloxane, a side chain polyether-modified polysiloxane and a side chain epoxy-modified polysiloxane to obtain a mixture 1;

[0046] (2) mixing alkylphenol polyoxyethylene ether with acid and water to obtain mixture 2;

[0047] (3) Mix mixture 2 into mixture 1.

[0048] Compared with other acid addition sequences, the acid addition sequence in the production method makes the oil particles in the emulsion of the raw silk oil agent of the present invention finer and the emulsion has higher stability.

[0049] In the above technical scheme, the mixing temperature of mixture 2 into mixture 1 in step (3) is preferably 40-60°C, for example but not limited to 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C and the like.

[0050] In the above technical solution, the mixing process of mixing mixture 2 into mixture 1 in step (3) is preferably carried out under stirring and / or shearing conditions.

[0051] In the above technical solution, the preferred stirring rate is 50-500 r / min (for example but not limited to 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min).

[0052] In the above technical solution, the preferred stirring time is 2 to 5 h (for example but not limited to 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, etc.).

[0053] In the above technical solution, the shear rate is preferably 1000-20000 r / min (for example, but not limited to, the shear rate is 1500 r / min, 2000 r / min, 2500 r / min, 3000 r / min, 3500 r / min, 4000 r / min, 4500 r / min, 5000 r / min, 5500 r / min, 6000 r / min, 6500 r / min, 7000 r / min, 7500r / min, 8000r / min, 8500r / min, 9000r / min, 9500r / min, 10000r / min, 11000r / min, 12000r / mi n, 13000r / min, 14000r / min, 15000r / min, 16000r / min, 17000r / min, 18000r / min, 19000r / min, etc.).

[0054] In the above technical solution, the preferred shearing time is 1-4 h (for example but not limited to 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, etc.).

[0055] To solve the third technical problem of the present invention, the technical solution of the present invention is as follows:

[0056] The oil agent is used in the production of PAN-based carbon fiber precursor.

[0057] One of the technical keys of the present invention is the selection of the raw fiber oil formulation. The more preferred technical solution of the present invention is the order of adding the acid. The specific application method of the above-mentioned oil can be reasonably selected by those skilled in the art without having to make creative efforts. For example, when used in the production of PAN-based carbon fiber raw fibers, it needs to be diluted with water to the required concentration, generally 1 to 3%, and a two-step oiling process is used.

[0058] The average particle size may be expressed as a volume average particle size, a weight average particle size or a particle number average particle size. The average particle size in the present invention is a volume average particle size. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 This is the average particle size distribution diagram of the oil in Example 1. DETAILED DESCRIPTION

[0060] Example 1

[0061] 15 parts of hexadecyltrimethylammonium bromide, 20 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and viscosity at 25°C is 1080 cP), 20 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and viscosity at 25°C is 2300 cP), 15 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) were fully stirred and mixed to obtain mixture A. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of p-toluenesulfonic acid and some deionized water were fully stirred and mixed to obtain mixture B. At 50°C, slowly add mixture B to mixture A, stir for 3h at a stirring rate of 300r / min, shear for 3h at a shear rate of 5000r / min, mix the two and stir evenly, and finally prepare an oil with an effective concentration of 20%. The oil has good stability, the time required for stratification is 92 days, and the average particle size of the oil is 0.189μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil was prepared into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0062] Example 2

[0063] 15 parts of hexadecyltrimethylammonium bromide, 20 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and viscosity at 25°C is 1080 cP), 20 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and viscosity at 25°C is 2300 cP), 15 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) were fully stirred and mixed to obtain mixture A. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of 2-methylbenzenesulfonic acid and some deionized water were fully stirred and mixed to obtain mixture D. At 50°C, slowly add mixture D to mixture C, stir for 3h at a stirring rate of 300r / min, shear for 3h at a shear rate of 5000r / min, mix the two and stir evenly, and finally prepare an oil with an effective concentration of 20%. The oil has good stability, the time required for stratification is 89 days, and the average particle size of the oil is 0.191μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil was prepared into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0064] Example 3

[0065] 15 parts of hexadecyltrimethylammonium bromide, 25 parts of a side chain monoamino-modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and a viscosity of 1080 cP at 25°C), 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R6=C2H4, b / (a+b+c)=0.3, and a viscosity of 25°C of 2500 cP), and 20 parts of a side chain polyether-modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C6H 12 , b / (a+b+c)=0.5, 25℃ viscosity is 650cP) 15 parts, side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein R8=C6H 12, b / (a+b+c)=0.35, 25℃ viscosity is 1800cP) 9 parts, fully stirred and mixed to obtain mixture E. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of sulfuric acid and some deionized water are fully stirred and mixed to obtain mixture F. At a temperature of 40-60℃, mixture F is slowly added to mixture E, stirred for 3h, stirring speed is 300r / min, sheared for 3h, shear rate is 5000r / min, the two are mixed and stirred evenly, and finally formulated into an oil agent with an effective concentration of 20%. The oil agent has good stability, the time required for stratification is 35 days, and the average particle size of the oil agent is 0.325μm. For the convenience of statistics, the relevant data are listed in Tables 1 and 2. The formula oil agent is prepared into a 2% emulsion concentration for fiber oiling evaluation, and the obtained fiber is smooth, soft, without lint and adhesion.

[0066] Example 4

[0067] 15 parts of hexadecyltrimethylammonium bromide, 20 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and viscosity at 25°C is 1080 cP), 20 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and viscosity at 25°C is 2300 cP), 15 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) were fully stirred and mixed to obtain a mixture J. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of 4-isopropylbenzene sulfonic acid and some deionized water were fully stirred and mixed to obtain a mixture H. At 50°C, mixture H was slowly added to mixture J, stirred for 3 hours at a stirring rate of 300 r / min, sheared for 3 hours at a shear rate of 5000 r / min, and the two were mixed and stirred evenly, and finally formulated into an oil with an effective concentration of 20%. The oil had good stability, the time required for stratification was 91 days, and the average particle size of the oil was 0.190 μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil was formulated into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0068] Example 5

[0069] 15 parts of octadecyltrimethylammonium bromide, 40 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and viscosity at 25°C is 1080 cP), 15 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP), and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) are thoroughly stirred and mixed to obtain a mixture I. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of p-toluenesulfonic acid and some deionized water are fully stirred and mixed to obtain mixture J. At a temperature of 50°C, mixture J is slowly added to mixture I, stirred for 3 hours at a stirring rate of 300r / min, sheared for 3 hours at a shear rate of 5000r / min, and the two are mixed and stirred evenly, and finally formulated into an oil agent with an effective concentration of 20%. The oil agent has good stability, the time required for stratification is 86 days, and the average particle size of the oil agent is 0.193μm. For the convenience of statistics, the relevant data are listed in Tables 1 and 2. The formula oil agent is prepared into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber is smooth, soft, and has no lint and adhesion.

[0070] Example 6

[0071] 15 parts of hexadecyltrimethylammonium bromide, 40 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and viscosity at 25°C is 2300 cP), 15 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP), and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) are fully stirred and mixed to obtain a mixture K. 15 parts of nonylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of p-toluenesulfonic acid and some deionized water are fully stirred and mixed to obtain a mixture L. At a temperature of 50°C, the mixture L is slowly added to the mixture K, stirred for 3 hours at a stirring rate of 300r / min, sheared for 3 hours at a shear rate of 5000r / min, and the two are mixed and stirred evenly, and finally formulated into an oil agent with an effective concentration of 20%. The oil agent has good stability, the time required for stratification is 88 days, and the average particle size of the oil agent is 0.191μm. For the convenience of statistics, the relevant data are listed in Tables 1 and 2. The formula oil agent is prepared into a 2% emulsion concentration for fiber oiling evaluation, and the obtained fiber is smooth, soft, and has no lint and adhesion.

[0072] Example 7

[0073] 15 parts of hexadecyltrimethylammonium bromide, 20 parts of a side chain monoamino-modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and a viscosity of 1080 cP at 25°C), 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and a viscosity of 2300 cP at 25°C), and 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and a viscosity of 2300 cP at 25°C). 15 parts of chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 9.9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) were fully stirred and mixed to obtain a mixture M. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 0.1 parts of p-toluenesulfonic acid and some deionized water were fully stirred and mixed to obtain a mixture N. At 50°C, slowly add mixture N to mixture M, stir for 3h at a stirring rate of 300r / min, shear for 3h at a shear rate of 5000r / min, mix the two and stir evenly, and finally prepare an oil with an effective concentration of 20%. The oil has good stability, the time required for stratification is 81 days, and the average particle size of the oil is 0.195μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil was prepared into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0074] Example 8

[0075] 15 parts of hexadecyltrimethylammonium bromide, 15 parts of side chain monoamino modified polysiloxane 2 (as shown in structural formula 2, wherein R4=C4H8, b / (a+b+c)=0.5, and viscosity at 25°C is 1250 cP), 20 parts of side chain bisamino modified polysiloxane 2 (as shown in structural formula 3, wherein R5=R6=C3H6, e / (d+e+f)=0.4, and viscosity at 25°C is 2600 cP), and 20 parts of side chain polyether modified polysiloxane 2 (as shown in structural formula 4, wherein R7=C6H 12, n6=6, i(h+i+j)=0.55, 25℃ viscosity is 1100cP) 15 parts, side chain epoxy modified polysiloxane 2 (as shown in structural formula 5, wherein n7=5, n8=6, m / (k+m+n)=0.3, 25℃ viscosity is 1500cP) 14 parts, fully stirred and mixed to obtain mixture O. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of p-toluenesulfonic acid and some deionized water are fully stirred and mixed to obtain mixture P. At a temperature of 50℃, mixture P is slowly added to mixture O, stirred for 3h, stirring speed is 50r / min, sheared for 3h, shear speed is 1000r / min, the two are mixed and stirred evenly, and finally formulated into an oil with an effective concentration of 20%. The oil has good stability, the time required for stratification is 75 days, and the average particle size of the oil is 0.200μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formulated oil agent was prepared into a 2% emulsion concentration for fiber oiling evaluation, and the obtained fiber was smooth, soft, and free of lint and adhesion.

[0076] Example 9

[0077] 15 parts of hexadecyltrimethylammonium bromide, 15 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and viscosity at 25°C is 1080 cP), 20 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and viscosity at 25°C is 2300 cP), 10 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 9 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) were fully stirred and mixed to obtain a mixture Q. 20 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of p-toluenesulfonic acid and some deionized water were fully stirred and mixed to obtain a mixture R. At 50°C, the mixture R was slowly added to the mixture Q, stirred for 3 hours at a stirring rate of 300 r / min, sheared for 3 hours at a shear rate of 5000 r / min, and the two were mixed and stirred evenly, and finally formulated into an oil agent with an effective concentration of 20%. The oil agent had good stability, the time required for stratification was 79 days, and the average particle size of the oil agent was 0.199 μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil agent was formulated into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0078] Example 10

[0079] 15 parts of hexadecyltrimethylammonium bromide, 25 parts of a side chain monoamino-modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and a viscosity of 1080 cP at 25°C), 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R6=C2H4, b / (a+b+c)=0.3, and a viscosity of 25°C of 2500 cP), and 20 parts of a side chain polyether-modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C6H 12 , b / (a+b+c)=0.5, 25℃ viscosity is 650cP) 15 parts, side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein R8=C6H 12 , b / (a+b+c)=0.35, 25℃ viscosity is 1800cP) 9 parts, fully stirred and mixed to obtain mixture U. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 1 part of acetic acid and some deionized water are fully stirred and mixed to obtain mixture V. At a temperature of 40-60℃, mixture V is slowly added to mixture U, stirred for 3h, stirring speed is 300r / min, sheared for 3h, shear speed is 5000r / min, the two are mixed and stirred evenly, and finally formulated into an oil agent with an effective concentration of 20%. The oil agent has good stability, the time required for stratification is 23 days, and the average particle size of the oil agent is 0.370μm. For the convenience of statistics, the relevant data are listed in Tables 1 and 2. The formula oil agent is prepared into a 2% emulsion concentration for fiber oiling evaluation, and the obtained fiber is smooth, soft, without lint and adhesion.

[0080] Compared with Example 1, the difference in effect between p-toluenesulfonic acid and acetic acid is reflected.

[0081] Embodiment 11

[0082] 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20), 15 parts of hexadecyl trimethyl ammonium bromide, 25 parts of side chain monoamino modified polysiloxane 1 (as shown in structural formula 2, wherein R4 = C2H4, b / (a+b+c) = 0.4, and the viscosity at 25°C is 1080 cP), 20 parts of side chain bisamino modified polysiloxane 1 (as shown in structural formula 3, wherein R6 = C2H4, b / (a+b+c) = 0.3, and the viscosity at 25°C is 2500 cP), 20 parts of side chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7 = C6H 12 , b / (a+b+c)=0.5, 25℃ viscosity is 650cP) 15 parts, side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein R8=C6H 12, b / (a+b+c)=0.35, 25℃ viscosity is 1800cP) 9 parts, stir and mix thoroughly. At 40~60℃, slowly add deionized water, stir for 3h, stirring speed is 300r / min, shear for 3h, shear speed is 5000r / min, mix the two evenly, finally add 1 part of p-toluenesulfonic acid, finally prepare into 20% effective concentration oil, oil stability is good, stratification time is 41 days, oil average particle size is 0.331μm. For the convenience of statistics, relevant data are listed in Table 1 and Table 2. The formula oil is prepared into 2% emulsion concentration for fiber oiling evaluation, and the obtained fiber is smooth, soft, without lint and adhesion.

[0083] Compared with Example 1, it is shown that the effect of adding the acid to the silicone oil after mixing with the surfactant and water is better than the effect of adding them directly at the end without mixing.

[0084] Comparative Example 1

[0085] 15 parts of hexadecyltrimethylammonium bromide, 20 parts of a side chain monoamino-modified polysiloxane 1 (as shown in structural formula 2, wherein R4=C2H4, b / (a+b+c)=0.4, and a viscosity of 1080 cP at 25°C), 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and a viscosity of 2300 cP at 25°C), and 20 parts of a side chain bisamino-modified polysiloxane 1 (as shown in structural formula 3, wherein R5=R6=C2H4, e / (d+e+f)=0.3, and a viscosity of 2300 cP at 25°C). 15 parts of chain polyether modified polysiloxane 1 (as shown in structural formula 4, wherein R7=C2H4, n6=6, i(h+i+j)=0.55, and viscosity at 25°C is 800 cP) and 10 parts of side chain epoxy modified polysiloxane 1 (as shown in structural formula 5, wherein n7=5, n8=4, m / (k+m+n)=0.35, and viscosity at 25°C is 1800 cP) are fully stirred and mixed to obtain a mixture S. 15 parts of octylphenol polyoxyethylene ether 20 (20 represents the number of ethylene oxide addition is 20) and a certain amount of deionized water are fully stirred and mixed to obtain a mixture T. At 50°C, slowly add mixture T to mixture S, stir for 3h at a stirring rate of 300r / min, shear for 3h at a shear rate of 5000r / min, mix the two and stir evenly, and finally prepare an oil with an effective concentration of 20%. The oil has good stability, the time required for stratification is 7 days, and the average particle size of the oil is 0.502μm. For the convenience of statistics, the relevant data are listed in Table 1 and Table 2. The formula oil was prepared into a 2% emulsion concentration for fiber oiling evaluation, and the resulting fiber was smooth, soft, and free of lint and adhesion.

[0086] Compared with Example 1, the effects of adding acid and not adding acid are reflected.

[0087] Table 1

[0088]

[0089] Table 2

[0090]

[0091] Note a: The acid addition process is that after all the raw materials are added, 1 part of p-toluenesulfonic acid is added separately at the end.

Claims

1. PAN-based carbon fiber precursor oil, wherein the active ingredients include the following components by weight: Alkylphenol polyoxyethylene ether, 6-25 parts; Quaternary ammonium salt antistatic agent, 10-25 parts; Side chain amino-modified polysiloxane, 30-50 parts; Side chain polyether modified polysiloxane, 5-20 parts; Side chain epoxy modified polysiloxane, 5-15 parts; Acid, 0.01-2 parts; The acid is an aromatic organic sulfonic acid; The method for producing the PAN-based carbon fiber precursor oil comprises the following steps: (1) mixing an antistatic agent with a side chain amino-modified polysiloxane, a side chain polyether-modified polysiloxane and a side chain epoxy-modified polysiloxane to obtain a mixture 1; (2) mixing alkylphenol polyoxyethylene ether with acid and water to obtain mixture 2; (3) Mix mixture 2 into mixture 1.

2. The raw silk oil according to claim 1, characterized in that The acid is alkylbenzene sulfonic acid.

3. The raw silk oil according to claim 2, characterized in that The alkyl group of the alkylbenzene sulfonic acid is a C1-C4 alkyl group.

4. The raw silk oil according to claim 1, characterized in that The alkylphenol polyoxyethylene ether is selected from at least one of octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether.

5. The raw silk oil according to claim 4, characterized in that The number of repeating units of ethylene oxide in the alkylphenol polyoxyethylene ether is 2 to 8.

6. The raw silk oil according to claim 1, characterized in that The quaternary ammonium salt structure contains a quaternary ammonium cation group having the following structural formula 1: Wherein R is a C10-C20 hydrocarbon group; R1-R3 are independently selected from C1-C3 hydrocarbon groups, and the total carbon number of the three groups R1, R2 and R3 is less than 6.

7. The raw silk oil according to claim 6, characterized in that In the quaternary ammonium salt structure, R is a straight-chain hydrocarbon group.

8. The raw silk oil according to claim 7, characterized in that In the quaternary ammonium salt structure, R is an alkyl group.

9. The raw silk oil according to claim 8, characterized in that In the quaternary ammonium salt structure, R is a primary alkyl group.

10. The raw silk oil according to claim 1, characterized in that The anions in the quaternary ammonium salt structure are X-, CH3SO3 - 、CH3OSO3 - 、NO3 - or SO4 2- , X is a halogen atom.

11. The raw silk oil according to claim 1, characterized in that The side chain amino-modified polysiloxane is selected from at least one of the side chain monoamino-modified polysiloxane shown in the following structural formula 2 or the side chain diamino-modified polysiloxane shown in the following structural formula 3: wherein R4 is selected from an alkylene group having 2 to 10 carbon atoms, and b / (a+b+c)=0.1 to 0.8; wherein R5 and R6 are independently selected from an alkylene group having 2 to 10 carbon atoms, and e / (d+e+f)=0.1 to 0.8; And / or the side chain polyether modified polysiloxane is selected from at least one of the compounds shown in the following structural formula 4: wherein i / (h+i+j)=0.1-0.6, R7 is an alkylene group having 2-10 carbon atoms, 2≤n6≤10; And / or the side chain epoxy-modified polysiloxane is selected from at least one of the compounds shown in the following structural formula 5: Among them, m / (k+m+n)=0.1~0.8, 1≤n7≤7, 1≤n8≤5.

12. The raw silk oil according to claim 1, characterized in that The method comprises the active ingredient according to any one of claims 1 to 11 and water.

13. The raw silk oil according to claim 12, characterized in that The effective ingredients account for 10 to 30% of the total amount of the effective ingredients and water by weight.

14. The method for producing a PAN-based carbon fiber precursor oil according to any one of claims 1 to 13, comprising the following steps: (1) mixing an antistatic agent with a side chain amino-modified polysiloxane, a side chain polyether-modified polysiloxane and a side chain epoxy-modified polysiloxane to obtain a mixture 1; (2) mixing alkylphenol polyoxyethylene ether with acid and water to obtain mixture 2; (3) Mix mixture 2 into mixture 1.

15. The production method according to claim 14, characterized in that The mixing temperature of the mixture 2 into the mixture 1 in step (3) is 40-60°C.

16. The production method according to claim 14, characterized in that The mixing process of step (3) mixing mixture 2 into mixture 1 is carried out under stirring and / or shearing conditions.

17. The production method according to claim 16, characterized in that The mixing process of step (3) mixing mixture 2 into mixture 1 is carried out under stirring, and the stirring time is 2-5 hours.

18. The production method according to claim 16, characterized in that The mixing process of mixing mixture 2 into mixture 1 in step (3) is carried out under shearing, with a shear rate of 1000 to 20000 r / min and / or a shear time of 1 to 4 h.

19. The production method according to claim 16, characterized in that The stirring rate in step (3) is 50 to 500 r / min.

20. Use of the oil according to any one of claims 1 to 13 in the production of PAN-based carbon fiber precursor.