Composition for forming an easily adhesive layer and hard coating film using the same

By using a polysiloxane compound having a hydroxyl group in the side chain and a light-transmitting resin on a cyclic olefin polymer base material, an easy-adhesive layer forming composition solves the problem of tightness between the cyclo olefin polymer base material and the hard coat layer. It solves the problem of poor adhesion and significantly improves the bending resistance and transmittance of the hard coating film.

CN115698213BActive Publication Date: 2024-10-11DONGWOO FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180038603.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-03
Filing Date
2021-05-27
Publication Date
2024-10-11
Estimated Expiration
2041-05-27

AI Technical Summary

Technical Problem

The poor adhesion between the cyclic olefin polymer substrate and the hard coat layer results in a decrease in the bending resistance of the hard coat film.

Method used

An easy-adhesive layer forming composition containing a polysiloxane compound with a hydroxyl group in the side chain, a translucent resin, a photoinitiator, and a solvent is used to improve adhesion through hydrogen bonding and secure a hard coat layer using a UV curing reaction. of tightness.

Benefits of technology

The bending resistance of the hard coating film is significantly improved, and it can be bent without breakage or hard coating peeling after 200,000 times, while maintaining excellent transmittance and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003966328470000081
    Figure BDA0003966328470000081
  • Figure BDA0003966328470000082
    Figure BDA0003966328470000082
  • Figure BDA0003966328470000083
    Figure BDA0003966328470000083
Patent Text Reader

Abstract

The present invention provides a composition for forming an easy-adhesion layer comprising a polysiloxane compound having a hydroxyl group on a side chain, a light-transmitting resin, a photoinitiator and a solvent, a hard coating film formed using the composition, and an image display device having the hard coating film. The composition for forming an easy-adhesion layer of the present invention comprises a polysiloxane compound having a hydroxyl group on a side chain and a light-transmitting resin, thereby improving the adhesion between a cycloolefin polymer substrate and a hard coating layer, thereby improving the bending resistance of the hard coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an easy-adhesion layer-forming composition and a hard coat film using the same, and more particularly to an easy-adhesion layer-forming composition capable of improving the adhesion between a cycloolefin polymer substrate and a hard coat layer, thereby improving the flex resistance of the hard coat film, a hard coat film formed using the same, and an image display device having the hard coat film. Background Art

[0002] The hard coat film is used for the purpose of surface protection in image display devices such as liquid crystal display devices, electroluminescent (EL) liquid crystal display devices, plasma displays (PD), and field emission displays (FED: Field Emission Display).

[0003] In recent years, as flexible materials such as plastics are used to replace traditional inflexible glass substrates, flexible display devices that can maintain display performance even when bent like paper are rapidly becoming the next generation of display devices. Research is being conducted on hard coating films that not only have high hardness and good scratch resistance, but also do not curl up at the film edges during the manufacturing process or in use, and have appropriate flexibility without cracking.

[0004] On the other hand, cycloolefin polymer (COP) is excellent in transparency, heat resistance, dimensional stability, low hygroscopicity, low birefringence and optical isotropy, and is expected to be used as a substrate for hard coating. However, unlike acrylic film or polyester film, cycloolefin polymer film has a small number of polar groups on the film surface, so the adhesion between the substrate film and the hard coating layer is poor.

[0005] Therefore, Korean Patent Publication No. 10-2017-0107995 discloses a hard coating film produced by an easy-adhesion layer containing a mixture of a polyolefin-based resin and a styrene acrylic resin.

[0006] However, the hard coat film has a problem that since the adhesion layer contains a resin component and has a low degree of crosslinking, it is difficult to achieve sufficient adhesion between the cycloolefin polymer substrate and the hard coat layer, and the flex resistance is reduced when used for the hard coat film. Summary of the invention

[0007] Technical issues

[0008] An object of the present invention is to provide an easily adhesive layer-forming composition capable of improving the adhesion between a cycloolefin polymer substrate and a hard coat layer.

[0009] Another object of the present invention is to provide a hard coating film formed by using the easily-adhesive layer-forming composition and having improved flex resistance.

[0010] Still another object of the present invention is to provide an image display device including the hard coat film.

[0011] Solution to the problem

[0012] In another aspect, the present invention provides an easily adhesive layer-forming composition including a polysiloxane compound having a hydroxyl group in a side chain, a light-transmitting resin, a photoinitiator, and a solvent.

[0013] In one embodiment of the present invention, the content of the polysiloxane compound having a hydroxyl group in a side chain may be 10 to 90% by weight relative to 100% by weight of the entire solid content in the easily adhesive layer forming composition.

[0014] In one embodiment of the present invention, the light-transmitting resin may include one or more selected from the group consisting of photocurable (meth)acrylate oligomers and monomers.

[0015] The easily adhesive layer-forming composition according to one embodiment of the present invention can be used between the cycloolefin polymer substrate and the hard coat layer.

[0016] In another aspect, the present invention provides a hard coating film comprising:

[0017] Cyclic olefin polymer substrate;

[0018] an easy-adhesion layer formed on at least one side of the cycloolefin polymer substrate; and

[0019] A hard coating layer formed on the easy-adhesion layer,

[0020] The easily adhesive layer is formed using the easily adhesive layer-forming composition.

[0021] The total light transmittance of the hard coat film of one embodiment of the present invention is 90% or more. After the hard coat film is repeatedly folded and unfolded 200,000 times with a curvature radius of 1 mm in a manner such that the hard coat surface faces inward, the hard coat film does not break or peel off.

[0022] In one embodiment of the present invention, the cycloolefin polymer substrate may be subjected to a hydrophilic treatment.

[0023] In one embodiment of the present invention, the hard coating layer may be formed using a hard coating composition including a light-transmitting resin, a photoinitiator, and a solvent.

[0024] In one embodiment of the present invention, the light-transmitting resin may include one or more selected from the group consisting of photocurable (meth)acrylate oligomers and monomers.

[0025] In yet another aspect, the present invention provides an image display device including the hard coat film.

[0026] In yet another aspect, the present invention provides a window of a flexible display device having the hard coating film.

[0027] In yet another aspect, the present invention provides a polarizing plate including the hard coat film.

[0028] In yet another aspect, the present invention provides a touch sensor including the hard coating film.

[0029] Effects of the Invention

[0030] The adhesive layer-forming composition of the present invention contains a polysiloxane compound having a hydroxyl group in a side chain and a light-transmitting resin, and can improve the adhesion between the cycloolefin polymer substrate and the hard coat layer, thereby improving the flex resistance of the hard coat film. DETAILED DESCRIPTION

[0031] Hereinafter, the present invention will be described in more detail.

[0032] One embodiment of the present invention relates to an easily adhesive layer-forming composition including a polysiloxane compound having a hydroxyl group in a side chain, a light-transmitting resin, a photoinitiator, and a solvent.

[0033] In one embodiment of the present invention, the polysiloxane compound having a hydroxyl group in a side chain is a component that imparts adhesion between the cycloolefin polymer substrate and the hard coat layer and is a compound having a polysiloxane skeleton and having a hydroxyl group in a side chain.

[0034] The polysiloxane compound having a hydroxyl group in the side chain can improve adhesion by forming hydrogen bonds between the hydroxyl groups in the molecule and the hydroxyl groups on the surface of the hydrophilically treated cycloolefin polymer substrate.

[0035] The polysiloxane compound having a hydroxyl group in the side chain is a polycondensate of hydrolyzable trialkoxysilane or tetraalkoxysilane and is not particularly limited as long as it has a hydroxyl group in the side chain. However, a polycondensate of tetraalkoxysilane is preferred from the viewpoint of ensuring adhesion.

[0036] Examples of the hydrolyzable trialkoxysilane include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane. Monoalkyltrialkoxysilanes such as silane; monoaryltrialkoxysilanes such as phenyltrimethoxysilane and phenyltriethoxysilane; monovinyltrialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane; monoaminoalkyltrialkoxysilanes such as γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane; monoepoxyalkyltrialkoxysilanes such as γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropyltriethoxysilane; mono(meth)acryloxyalkyltrialkoxysilanes such as γ-methacryloxypropyltrimethoxysilane and γ-methacryloxypropyltriethoxysilane, etc.

[0037] Examples of the hydrolyzable tetraalkoxysilane include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane and tetrabutoxysilane.

[0038] The polysiloxane compound having a hydroxyl group in the side chain may be a commercially available product or may be produced by a known polycondensation method and used.

[0039] Specifically, the polysiloxane compound having a hydroxyl group in the side chain can be obtained by adding a hydrolyzable trialkoxysilane or a tetraalkoxysilane to an alcohol solvent (eg, methanol, ethanol, etc.) and subjecting it to a condensation polymerization reaction in the presence of water and an acid catalyst (eg, hydrochloric acid, nitric acid, etc.).

[0040] Examples of commercially available products of the polysiloxane compound having a hydroxyl group in a side chain include COLCOAT N-103X and COLCOAT PX manufactured by COLCOAT.

[0041] The content of the polysiloxane compound having a hydroxyl group on the side chain may be 10 to 90% by weight, more preferably 15 to 80% by weight, relative to 100% by weight of the solid content in the easy-adhesion layer-forming composition. If the content of the polysiloxane compound having a hydroxyl group on the side chain is less than 10% by weight, it may not be able to form a sufficient bond with the cycloolefin-based substrate, resulting in poor adhesion. If it is greater than 90% by weight, it may not be able to form a sufficient bond with the hard coating layer, resulting in poor adhesion.

[0042] In one embodiment of the present invention, the light-transmitting resin is a photocurable resin, and the photocurable resin may include a photocurable (meth)acrylate oligomer and / or monomer.

[0043] As the above-mentioned light-curing (meth) acrylate oligomer, epoxy (meth) acrylate, carbamate (meth) acrylate, etc. are generally used, preferably carbamate (meth) acrylate. Carbamate (meth) acrylate can be made by reacting a (meth) acrylate having a hydroxyl group in the molecule with a compound having an isocyanate group in the presence of a catalyst. As a specific example of the (meth) acrylate having a hydroxyl group in the above-mentioned molecule, there are 2-hydroxyethyl (meth) acrylate, 2-hydroxyisopropyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, caprolactone ring-opening hydroxy acrylate, pentaerythritol tri (meth) acrylate, pentaerythritol tetra (meth) acrylate, dipentaerythritol penta (meth) acrylate, dipentaerythritol hexa (meth) acrylate, etc. Specific examples of the compound having an isocyanate group include 1,4-diisocyanatobutane, 1,6-diisocyanatohexane, 1,8-diisocyanatooctane, 1,12-diisocyanatododecane, 1,5-diisocyanato-2-methylpentane, trimethyl-1,6-diisocyanatohexane, 1,3-bis(isocyanatomethyl)cyclohexane, trans-1,4-cyclohexene diisocyanate, 4,4'-diisocyanatobutane, ...6-diisocyanatohexane, 1,6-diisocyanatohexane, 1,6-diisocyanatohexane, 1,6-diisocyanatohexane, 1,6-diisocyanatohexane, 1,6-diisocyanatohexane, 1,6-diisocyanatohe - methylenebis(cyclohexyl isocyanate), isophorone diisocyanate, toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, xylene-1,4-diisocyanate, tetramethylxylene-1,3-diisocyanate, 1-chloromethyl-2,4-diisocyanate, 4,4'-methylenebis(2,6-dimethylphenylisocyanate), 4,4'-oxybis(phenylisocyanate), trifunctional isocyanate derived from hexamethylene diisocyanate, trimethylolpropanol-added toluene diisocyanate, etc.

[0044] The above-mentioned monomers may be any commonly used monomers without limitation, and preferably have an unsaturated group such as a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group in the molecule as a photocurable functional group, and preferably have a (meth)acryloyl group.

[0045] Specific examples of the monomer having the (meth)acryloyl group include neopentyl glycol acrylate, 1,6-hexanediol di(meth)acrylate, propylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaglycerol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and dipentaerythritol tri(meth)acrylate. One or more is selected from the group consisting of alcohol penta(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol tri(meth)acrylate, tripentaerythritol hexa(meth)acrylate, bis(2-hydroxyethyl)isocyanurate di(meth)acrylate, hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxybutyl(meth)acrylate, isooctyl(meth)acrylate, isodecyl(meth)acrylate, stearyl(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, phenoxyethyl(meth)acrylate and isobornyl(meth)acrylate.

[0046] The photocurable (meth)acrylate oligomers and monomers exemplified above as the light-transmitting resin may be used alone or in combination of two or more.

[0047] The content of the light-transmitting resin is not particularly limited, and can be 1 to 80% by weight relative to 100% by weight of the solid content in the composition for forming an easy-adhesion layer. If the content of the light-transmitting resin is less than 1% by weight, it may not be able to form a sufficient bond with the hard coat layer, resulting in poor adhesion. If it is greater than 80% by weight, the content of the polysiloxane compound having a hydroxyl group in the side chain is relatively insufficient, so that it may not be able to form a sufficient bond with the cycloolefin polymer substrate, resulting in poor adhesion.

[0048] In one embodiment of the present invention, the photoinitiator can be used without limitation as long as it is a substance used in the art that can form free radicals by light irradiation, for example, hydroxyketones, aminoketones, hydrogen abstraction type photoinitiators, etc. can be used.

[0049] Specifically, the photoinitiator includes 2-methyl-1-[4-(methylthio)phenyl]2-morpholinoacetone-1, phenyl ketone, benzyl dimethyl ketal, 2-hydroxy-2-methyl-1-phenyl-1-ketone, 2,2-dimethoxy-2-phenyl-acetophenone, anthraquinone, fluorene, triphenylamine, carbazole, 3-methylacetophenone, 4-chloroacetophenone, 4,4-dimethoxyacetophenone, 4,4-diaminobenzophenone, 1-hydroxycyclohexyl phenyl ketone, benzophenone, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, etc. The photoinitiators exemplified above can be used alone or in combination of two or more.

[0050] The content of the photoinitiator is not particularly limited, and for example, the content may be 0.1 to 10% by weight, preferably 1 to 5% by weight, relative to 100% by weight of the solid content in the easy-adhesion layer-forming composition. If the content of the photoinitiator is less than 0.1% by weight, the curing speed of the composition may be slow, and the composition may not be cured, thereby reducing the mechanical properties of the coating. If the content of the photoinitiator is greater than 10% by weight, the coating may crack due to over-curing.

[0051] The above solvents can be used without limitation as long as they are used in the technical field. Specifically, alcohols (methanol, ethanol, isopropanol, butanol, methyl cellosolve, ethyl cellosolve, etc.) can be used; ketones (methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, dipropyl ketone, cyclohexanone, etc.) can be used; acetates (ethyl acetate, propyl acetate, n-butyl acetate, tert-butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, methoxybutyl acetate, methoxypentyl acetate, etc.) can be used; hexanes (hexane, heptane, octane, etc.); benzenes (benzene, toluene, xylene, etc.); ethers (diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, etc.) can be used. The above-exemplified solvents can be used alone or in combination of two or more.

[0052] The content of the solvent may be 10 to 95% by weight relative to 100% by weight of the entire composition for forming an easy-adhesion layer. When the content of the solvent is less than 10% by weight, not only is the viscosity high and the workability poor, but also the substrate film cannot be fully swollen. When the content of the solvent is greater than 95% by weight, a lot of time is required during the drying process, resulting in poor economic efficiency.

[0053] The easily-adhesive layer-forming composition according to one embodiment of the present invention may further contain a leveling agent in order to impart smoothness and coating properties to the coating film during coating.

[0054] The leveling agent may be a commercially available silicone leveling agent, fluorine leveling agent, acrylic polymer leveling agent, or the like. For example, BYK-306, BYK-307, BYK-310, BYK-313, BYK-323, BYK-331, BYK-333, BYK-337, BYK-371, BYK-373, BYK-375, BYK-377, BYK-378, BYK-3440, BYK-3570, BYK-UV3500, BYK-UV3530, BYK-UV3570 of BYK Chemical Company, TEGO Glide 410, TEGO Glide 411, TEGO Glide 415, TEGO Glide 420, TEGO Glide 432, TEGO Glide 433, TEGO Glide 434 of Tego Chemical Company may be used. 435, TEGO Glide440, TEGO Glide 450, TEGO Glide 455, TEGO Rad 2100, TEGO Rad 2200N, TEGO Rad 2250, TEGO Rad 2300, TEGO Rad 2500, FC-4430, FC-4432 of 3M Company, etc. The content of the leveling agent may be in the range of 0.1 to 3 wt % relative to 100 wt % of the entire composition for forming an easily adhesive layer.

[0055] The composition for forming an easy-adhesive layer of one embodiment of the present invention can be used between a cycloolefin polymer substrate and a hard coating layer. The composition for forming an easy-adhesive layer of one embodiment of the present invention comprises a polysiloxane compound having a hydroxyl group in a side chain and a light-transmitting resin, so that the adhesion can be ensured by hydrogen bonding between the hydroxyl group on the surface of the hydrophilically treated cycloolefin polymer substrate and the hydroxyl group of the polysiloxane, and at the same time, the unreacted light-transmitting resin of the easy-adhesive layer participates in the UV curing reaction when forming the hard coating layer, and the adhesion with the hard coating layer can be ensured. Therefore, the composition for forming an easy-adhesive layer of one embodiment of the present invention can be applied between a cycloolefin polymer substrate and a hard coating layer to provide a hard coating film with excellent bending resistance.

[0056] Therefore, one embodiment of the present invention relates to a hard coating film formed using the above-mentioned easily adhesive layer-forming composition.

[0057] A hard coating film according to one embodiment of the present invention includes:

[0058] Cyclic olefin polymer substrate;

[0059] an easy-adhesion layer formed on at least one side of the cycloolefin polymer substrate; and

[0060] A hard coating layer formed on the easy-adhesion layer,

[0061] The easily adhesive layer is formed using the easily adhesive layer forming composition.

[0062] The hard coating film of one embodiment of the present invention has excellent transmittance characteristics and bending resistance. Specifically, the total light transmittance of the hard coating film of one embodiment of the present invention is 90% or more, and the hard coating film is repeatedly folded and unfolded 200,000 times in a manner such that the hard coating surface faces inward and the curvature radius is 1 mm, and the hard coating film does not break or peel off.

[0063] The total light transmittance (Tt, %) is calculated by measuring the incident light intensity (T0) on the hard coat film and the total transmitted light intensity (T1) through the hard coat film using the following Mathematical Formula 1.

[0064] [Mathematical formula 1]

[0065] Total light transmittance (Tt, %) = (T1 / T0) × 100

[0066] The total light transmittance can be measured, for example, using a haze meter (manufactured by Murakami Co., Ltd.) according to the method described in the experimental examples described later.

[0067] In one embodiment of the present invention, the cycloolefin polymer substrate serves as a base substrate of the hard coating film, and contains a cycloolefin polymer (COP) and has excellent transparency.

[0068] The above COP is a general term for resins produced by polymerization of cyclic olefins as monomers, and specific examples thereof include: ring-opening (co)polymers of cyclic olefins; addition polymers of cyclic olefins; copolymers (usually random copolymers) of cyclic olefins and α-olefins such as ethylene or propylene; graft-modified products modified with unsaturated carboxylic acids or their derivatives; and hydrogenated products thereof. Specific examples of cyclic olefins include norbornene-based monomers.

[0069] Specifically, the COP may be a polymer obtained by subjecting one or more monomers represented by the following Chemical Formulas 1 to 3 to ring-opening polymerization and selectively hydrogenating the monomers.

[0070] [Chemical formula 1]

[0071]

[0072] [Chemical formula 2]

[0073]

[0074] [Chemical formula 3]

[0075]

[0076] The process of producing COP by ring-opening polymerization of one or more monomers represented by the above Chemical Formulae 1 to 3 can be easily carried out according to a common method.

[0077] For example, the polymerization process can be carried out using acetylacetonate palladium (II) [Pd (acac) 2 ] and tricyclohexylphosphine as polymerization catalysts and using dimethylanilinium tetrakiss (pentafluorophenyl) borate as a co-catalyst.

[0078] In one embodiment of the present invention, the COP can be produced by mixing other ring-opening polymerizable cyclic olefins other than the norbornene-based monomers without hindering the purpose of the present invention. Specific examples of such cyclic olefins include compounds having one reactive double bond, such as cyclopentene, cyclooctene, and 5,6-dihydrodicyclopentadiene.

[0079] The COP may be further hydrogenated after the ring-opening polymerization reaction. The hydrogenation may be carried out by reacting with hydrogen in the presence of a hydrogenation catalyst according to a method known in the art. The hydrogenation rate is preferably 90% or more, more preferably 95% or more, and further preferably 99% or more. The hydrogenation rate within the above range can provide excellent heat degradation resistance, light degradation resistance, etc.

[0080] There are various commercial products of the above-mentioned COP. Specific examples of the above-mentioned COP include "ZF-16", "ZEONEX" and "ZEONOR" manufactured by ZEON CORPORATION, "Arton" manufactured by JSR Corporation, "TOPAS" manufactured by TICONA Corporation, and "APEL" manufactured by Mitsui Chemicals, Inc.

[0081] As a method for forming a substrate film by the above-mentioned COP, any suitable molding method can be used. Its specific examples include compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding and leveling. Extrusion molding and leveling are preferred because the obtained film can have improved smoothness and good optical uniformity. Molding conditions can be appropriately selected according to the composition or type of the resin used, the characteristics expected for the optical film, etc.

[0082] The thickness of the cycloolefin polymer substrate is not particularly limited, and may be 10 to 1000 μm, specifically 20 to 150 μm. If the thickness of the transparent substrate is less than 10 μm, the strength of the film is reduced and the processability is deteriorated, and if it is greater than 1000 μm, the transparency is reduced and the weight of the hard coating film is increased.

[0083] In one embodiment of the present invention, the cycloolefin polymer substrate may be subjected to a hydrophilic treatment.

[0084] The hydrophilic treatment can be performed by a surface treatment method such as corona treatment or plasma treatment.

[0085] In one embodiment of the present invention, the easily adhesive layer is formed by applying the easily adhesive layer forming composition onto at least one surface of the cycloolefin polymer substrate and curing the composition.

[0086] The adhesive layer-forming composition according to one embodiment of the present invention can be applied to a substrate by a known method such as a die coater, air knife, reverse roll, spray coating, doctor blade, casting, gravure printing, micro gravure printing, or spin coating.

[0087] After the composition for forming an easy-adhesion layer is applied to a substrate, the solvent is evaporated and dried, and then irradiated with UV light for curing. The irradiation amount of the UV light can be about 10 to 500 mJ / cm 2 , more specifically 50 to 400 mJ / cm 2 .

[0088] At this time, the thickness of the formed easy-adhesion layer may be specifically 0.1 to 5 μm, and more specifically 0.3 to 3 μm. When the thickness of the easy-adhesion layer is within the above range, excellent adhesion and bending resistance can be obtained.

[0089] In one embodiment of the present invention, the hard coating layer may be formed using a hard coating composition including a light-transmitting resin, a photoinitiator, and a solvent.

[0090] The light-transmitting resin is a photocurable resin, and the light-curable resin may include a light-curable (meth)acrylate oligomer and / or monomer. In terms of adhesion with the easy-adhesion layer, the light-transmitting resin preferably includes one or more selected from the group consisting of a light-curable (meth)acrylate oligomer and a monomer having a (meth)acryloyl group.

[0091] As specific types of the photocurable (meth)acrylate oligomer and the monomer having a (meth)acryloyl group, the same types as those used in the easily adhesive layer-forming composition can be used.

[0092] Furthermore, as the monomer having a (meth)acryloyl group, a dendrimer having a (meth)acrylate terminal group can be used.

[0093] The dendritic compound having a (meth)acrylate terminal group has the following structural characteristics: the terminal of the branch structure is substituted with a (meth)acrylate group for UV curing, and the center is completely aliphatic and composed of three-dimensional ester bonds. Therefore, compared with general multifunctional acrylate monomers, the dendritic compound having a (meth)acrylate terminal group has a structural characteristic that it has more functional groups than molecular weight as the number of generations increases, and the functional groups are distributed at the terminal, so that the core part can help improve the bending characteristics during curing. As a result, a high-hardness hard coating film with improved curling and flexibility can be obtained.

[0094] The dendritic compound having a (meth)acrylate terminal group may be purchased from the market or may be produced by a method known in the art. For example, a dendritic compound having a high degree of branching and having a large number of (meth)acrylate groups substituted at the terminal may be obtained by using a specific polyol as a central skeleton and subjecting it to a condensation reaction with dimethylolpropionic acid to form a first-generation dendritic structure, and then subjecting the dimethylolpropionic acid to repeated condensation reactions as a molecular structure to grow to a second-generation or higher structure, and then subjecting acrylic acid to a condensation reaction with the terminal group.

[0095] The content of the light-transmitting resin is not particularly limited, and can be 1 to 80% by weight relative to 100% by weight of the hard coating composition as a whole. If it is less than 1% by weight, it is difficult to achieve sufficient hardness improvement, and when it is greater than 80% by weight, there is a problem of increased curling.

[0096] As the photoinitiator, the same photoinitiator as that used in the easily adhesive layer forming composition can be used.

[0097] The content of the photoinitiator may be 0.1 to 10% by weight, preferably 1 to 5% by weight, relative to 100% by weight of the entire hard coating composition. When the content of the photoinitiator is less than 0.1% by weight, the curing speed of the composition may be slow, and the composition may not be cured, resulting in reduced mechanical properties of the coating. When the content of the photoinitiator is greater than 10% by weight, the coating may crack due to over-curing.

[0098] As the solvent, the same solvent as that used in the above-mentioned easily adhesive layer-forming composition can be used.

[0099] In addition, the solvent may include a fluorine-based solvent. The fluorine-based solvent may play the following role: increase the solubility of the fluorine-containing UV-curable functional group compound described later, thereby not only maintaining the wettability of the manufactured hard coating film and the coating state of the film excellent, but also orienting the fluorine-based UV-curable functional group on the surface of the hard coating layer during the coating and drying process to form a high-concentration fluorine component layer on the surface of the manufactured hard coating layer.

[0100] As the above-mentioned fluorine-based solvent, perfluorohexylethyl alcohol, perfluoroether, perfluorohexane, etc. can be used. Commercially available products include HFE-7100, HFE-7300, HFE-7500, FC-3283, FC-40, FC-770 from 3M Company, C6FOH-BF from Nichia Company, etc., but are not limited to these.

[0101] The content of the solvent may be 5 to 90% by weight, preferably 7 to 85% by weight, relative to 100% by weight of the hard coating composition as a whole. When the content is less than 5% by weight, the viscosity is high and the workability is poor, and when the content is more than 90% by weight, it is difficult to adjust the coating thickness, and drying lines occur, resulting in poor appearance.

[0102] In one embodiment of the present invention, the hard coating composition may further include a compound containing a fluorine-based UV-curable functional group.

[0103] The fluorine-based UV-curable functional group-containing compound is a component that imparts antifouling properties and abrasion resistance, and is not particularly limited as long as it contains fluorine and has a UV-curable functional group.

[0104] The above-mentioned fluorine-containing UV-curable functional group compound can use one or more selected from the group consisting of perfluoroalkyl-containing (meth)acrylates, perfluoropolyether-containing (meth)acrylates, perfluorocycloaliphatic-containing (meth)acrylates and perfluoroaromatic-containing (meth)acrylates. In this case, it has the advantage of excellent durability of maintaining antifouling performance for a long time even after repeated use due to the formation of chemical bonds with the hard coat layer while showing excellent antifouling performance, so it is preferred.

[0105] Relative to 100 weight percent of the solid content in the hard coating composition, the content of the fluorine-containing UV-curable functional group compound can be 0.01 to 30 weight percent, preferably 0.01 to 20 weight percent, and more preferably 0.01 to 10 weight percent. When the content of the fluorine-containing UV-curable functional group compound is within the above range, it can impart excellent wear resistance and antifouling effects, so it is preferred. When the content of the UV-curable functional group compound is less than the above range, it may not be easy to fully achieve wear resistance or antifouling properties. When it is greater than the above range, the film hardness or scratch resistance may be reduced.

[0106] In addition to the above components, the hard coating composition may further include components generally used in the art, for example, a leveling agent, a UV stabilizer, a heat stabilizer, an antioxidant, a surfactant, a lubricant, an antifouling agent, and the like.

[0107] The hard coating film according to one embodiment of the present invention can be produced by applying the hard coating composition on the easy-adhesion layer formed on at least one surface of a cycloolefin polymer substrate and curing the hard coating composition to form a hard coating layer.

[0108] The hard coating composition can be applied (coating process) on the adhesive layer by appropriately using a known method such as a die coater, an air knife, a reverse roll, spraying, a doctor blade, casting, gravure printing, micro gravure printing, spin coating, or the like.

[0109] After the hard coating composition is applied to the easy-adhesion layer, it is dried at a temperature of 30 to 150° C. for 10 seconds to 1 hour, more specifically for 30 seconds to 30 minutes to evaporate the volatile matter, and then irradiated with UV light to cure. The irradiation amount of the UV light can be specifically about 0.01 to 10 J / cm 2 , more specifically 0.1 to 2 J / cm 2 .

[0110] At this time, the thickness of the formed hard coating layer may be specifically 2 to 30 μm, and more specifically 3 to 20 μm. When the thickness of the hard coating layer is within the above range, excellent hardness and bending resistance can be obtained.

[0111] One embodiment of the present invention relates to an image display device having the above-mentioned hard coating film. For example, the hard coating film of the present invention can be used as a window of an image display device, particularly a flexible display device or a foldable display device. In addition, the hard coating film of the present invention can also be attached to a polarizing plate, a touch sensor, etc. for use.

[0112] The hard coating film of one embodiment of the present invention can be used for a reflective type, a transmissive type, a semi-transmissive type LCD or an LCD of various driving modes such as a TN type, a STN type, an OCB type, a HAN type, a VA type, an IPS type, etc. In addition, the hard coating film of one embodiment of the present invention can also be used for various image display devices such as a plasma display, a field emission display, an organic EL display, an inorganic EL display, and electronic paper.

[0113] The present invention will be described in more detail below by way of examples, comparative examples and experimental examples. It is obvious to those skilled in the art that these examples, comparative examples and experimental examples are only used to illustrate the present invention, and the scope of the present invention is not limited thereto.

[0114] Production Example 1: Production of a composition for forming an easily adhesive layer

[0115] 60 parts by weight of a polysiloxane compound having a hydroxyl group in the side chain (COLCOAT, COLCOAT N-103X, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 33.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0116] Production Example 2: Production of a composition for forming an easily adhesive layer

[0117] 90 parts by weight of a polysiloxane compound having a hydroxyl group on the side chain (COLCOAT, COLCOAT N-103X, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 3.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0118] Production Example 3: Production of a composition for forming an easily adhesive layer

[0119] 60 parts by weight of a polysiloxane compound having a hydroxyl group on the side chain (COLCOAT, COLCOAT PX, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 33.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0120] Production Example 4: Production of a composition for forming an easily adhesive layer

[0121] 90 parts by weight of a polysiloxane compound having a hydroxyl group on the side chain (COLCOAT, COLCOAT PX, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 3.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0122] Production Example 5: Production of a composition for forming an easily adhesive layer

[0123] 100 parts by weight of a polysiloxane compound having a hydroxyl group in a side chain (COLCOAT, COLCOAT N-103X, solid content 2% by weight) was filtered through a filter made of PP material to prepare a composition for forming an easily adhesive layer.

[0124] Production Example 6: Production of a composition for forming an easily adhesive layer

[0125] 100 parts by weight of a polysiloxane compound having a hydroxyl group in a side chain (COLCOAT, COLCOAT PX, solid content 2% by weight) was filtered through a filter made of PP material to prepare a composition for forming an easily adhesive layer.

[0126] Production Example 7: Production of Composition for Forming an Adhesive Layer

[0127] 10 parts by weight of a polysiloxane compound having a hydroxyl group in the side chain (COLCOAT, COLCOAT N-103X, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 83.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0128] Production Example 8: Production of a composition for forming an easily adhesive layer

[0129] 10 parts by weight of a polysiloxane compound having a hydroxyl group in the side chain (COLCOAT, COLCOAT PX, solid content 2% by weight), 6 parts by weight of a trifunctional acrylate monomer (Miramer M340), 83.4 parts by weight of methyl ethyl ketone, 0.3 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts by weight of a leveling agent (BYK UV-3530) were mixed with a stirrer and filtered with a filter made of PP to prepare a composition for forming an easy-adhesion layer.

[0130] Production Example 9: Production of Hard Coating Composition

[0131] 23 parts by weight of 6-functional urethane acrylate (Shin-Nakamura Chemical, U-6LPA), 23 parts by weight of 14-functional acrylate (Osaka Organic Chemical, VISCOAT#1000), 5 parts by weight of fluorine-based solvent (Nikka, C6FOH-BF), 45 parts by weight of methyl ethyl ketone, 3.5 parts by weight of 1-hydroxycyclohexyl phenyl ketone and 0.5 parts by weight of a fluorine-containing UV-curable functional group compound (Shin-Etsu Corporation, KY-1203) were mixed with a stirrer and filtered with a PP filter to prepare a hard coating composition.

[0132] Example 1: Preparation of easy-adhesion film

[0133] The composition for forming an easily adhesive layer of the above-mentioned manufacturing example 1 was applied to a cycloolefin film (Zeon COP, ZF-14, 23 μm) which was subjected to corona treatment and whose surface water contact angle was adjusted to 65 degrees so that the thickness after curing would be 0.5 μm. After the solvent was dried, the film was irradiated with UV light with a cumulative amount of 300 mJ / cm in a nitrogen atmosphere. 2 , to produce an easy-to-bond film.

[0134] Example 2: Preparation of easy-adhesion film

[0135] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 2 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0136] Example 3: Preparation of easy-adhesion film

[0137] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 3 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0138] Example 4: Preparation of easy-adhesion film

[0139] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 4 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0140] Example 5: Preparation of hard coating film

[0141] The hard coating composition of the above-mentioned manufacturing example 9 was applied to the easy bonding layer of the easy bonding film prepared in the above-mentioned embodiment 1 so that the thickness after curing would be 5 μm, and after the solvent was dried, UV cumulative light was irradiated in a nitrogen atmosphere at a dose of 600 mJ / cm 2 , to produce a hard coating.

[0142] Example 6: Preparation of hard coating film

[0143] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Example 2 was used instead of the easy adhesion film produced in Example 1.

[0144] Example 7: Preparation of hard coating film

[0145] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Example 3 was used instead of the easy adhesion film produced in Example 1.

[0146] Example 8: Preparation of hard coating film

[0147] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Example 4 was used instead of the easy adhesion film produced in Example 1.

[0148] Comparative Example 1: Production of Easy Adhesion Film

[0149] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 5 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0150] Comparative Example 2: Production of Easy Adhesion Film

[0151] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 6 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0152] Comparative Example 3: Production of Easy Adhesion Film

[0153] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 7 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0154] Comparative Example 4: Production of Easy Adhesion Film

[0155] An easily adhesive film was produced by the same method as in Example 1, except that the easily adhesive layer-forming composition of Production Example 8 was used instead of the easily adhesive layer-forming composition of Production Example 1.

[0156] Comparative Example 5: Preparation of hard coating film

[0157] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Comparative Example 1 was used instead of the easy adhesion film produced in Example 1.

[0158] Comparative Example 6: Preparation of hard coating film

[0159] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Comparative Example 2 was used instead of the easy adhesion film produced in Example 1.

[0160] Comparative Example 7: Preparation of hard coating film

[0161] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Comparative Example 3 was used instead of the easy adhesion film produced in Example 1.

[0162] Comparative Example 8: Preparation of hard coating film

[0163] A hard coating film was produced by the same method as in Example 5, except that the easy adhesion film produced in Comparative Example 4 was used instead of the easy adhesion film produced in Example 1.

[0164] Experimental Example 1:

[0165] The physical properties of the films produced in the above-mentioned Examples and Comparative Examples were measured by the methods described below. The results are shown in Table 1 below.

[0166] (1) Adhesion

[0167] After the base film and glass were bonded with a transparent adhesive with the coated surface facing up, 100 regular quadrilateral cuts were made in the coated surface with a cutter at 1 mm intervals in the horizontal and vertical directions, and then the adhesion test was performed three times with Nichiban tape.

[0168] The evaluation results are expressed as "the number of quadrilaterals remaining (OK) after the adhesion test / 100".

[0169] (2) Total light transmittance (Tt) and haze

[0170] The total light transmittance (%) and haze (%) of the coating film were measured using a haze meter HM-150 manufactured by Murakami Co., Ltd.

[0171] (3) Water contact angle

[0172] The contact angle of water was measured using a contact angle meter DSA100 manufactured by KRUSS Co. The drop volume was set to 3 μl at room temperature.

[0173] (4) Wear resistance

[0174] The test was carried out using the wear test equipment of Dacheng Precision Co., Ltd. The coating surface was rubbed 3000 times with a wear test rubber and a 500g weight, and the contact angle was measured. At this time, as the evaluation standard, the case where the water contact angle was 100° or more was selected as the wear resistance qualified standard.

[0175] <Evaluation Criteria>

[0176] ○: Contact angle is 100° or more

[0177] ×: Contact angle less than 100°

[0178] (5) Reagent resistance

[0179] The test is carried out using the wear resistance measuring equipment of Dacheng Precision Co., Ltd. After dripping 99.9% ethanol on the coating surface, the area dripped with ethanol is wiped 3000 times with a wear test eraser and a 500g weight, and then the contact angle is measured. During the evaluation, ethanol is continuously dripped to prevent ethanol from volatilizing. After the evaluation is completed, the ethanol is removed and the water contact angle is measured. At this time, as the evaluation benchmark, the case where the water contact angle is 95° or more is selected as the qualified benchmark for reagent resistance.

[0180] <Evaluation Criteria>

[0181] ○: Contact angle is 95° or more

[0182] ×: Contact angle less than 95°

[0183] (6) Scratch resistance

[0184] After the base film and the glass were bonded together with a transparent adhesive so that the coated surface was on the upper side, a steel wool (#0000) was used to press the glass at a speed of 500 g / cm 2 After rubbing back and forth 10 times with a load of , the scratches were observed by the three-wavelength lamp transmission and reflection measurement unit. The scratch resistance was evaluated according to the following evaluation criteria.

[0185] <Evaluation Criteria>

[0186] ○: No scratches or 10 or fewer scratches were observed

[0187] ×: More than 10 scratches are seen

[0188] (7) Bending resistance

[0189] The film was folded and unfolded repeatedly 200,000 times with a curvature radius of 1 mm so that the hard coating layer was facing inward, and the film was observed for breakage and peeling of the hard coating layer. The bending resistance was evaluated according to the following evaluation criteria.

[0190] <Evaluation Criteria>

[0191] ○: No film breakage or hard coat peeling occurred

[0192] ×: Film breakage or hard coat peeling occurred

[0193] [Table 1]

[0194]

[0195] As shown in Table 1, it can be seen that the coating surfaces of the easy-adhesion films of Examples 1 to 4 produced using the easy-adhesion layer-forming compositions of Production Examples 1 to 4 containing a polysiloxane compound having a hydroxyl group in a side chain and a light-transmitting resin of the present invention have excellent adhesion. In addition, it can be confirmed that the hard coating films of Examples 5 to 8 in which a hard coating layer is formed on the easy-adhesion films of Examples 1 to 4 have excellent adhesion, as well as excellent water contact angle, abrasion resistance, chemical resistance, scratch resistance, and bending resistance.

[0196] On the other hand, it was confirmed that the adhesion of the coating surface of the easy-adhesive film of Comparative Examples 1 to 2 manufactured using the easy-adhesive layer-forming composition of Manufacturing Examples 5 to 6 containing a polysiloxane compound having a hydroxyl group on the side chain but not containing a light-transmitting resin was good, but the hard coating film of Comparative Examples 5 to 6 in which a hard coating layer was formed on the easy-adhesive film of Comparative Examples 1 to 2 not only deteriorated the adhesion of the coating surface, but also deteriorated the bending resistance. In addition, it was confirmed that the adhesion of the coating surface of the easy-adhesive film of Comparative Examples 3 to 4 manufactured using the easy-adhesive layer-forming composition of Manufacturing Examples 7 to 8 containing a small amount of polysiloxane compound having a hydroxyl group on the side chain was poor, and the hard coating film of Comparative Examples 7 to 8 in which a hard coating layer was formed on the easy-adhesive film of Comparative Examples 3 to 4 not only deteriorated the adhesion of the coating surface, but also deteriorated the bending resistance.

[0197] Above, specific parts of the present invention are described in detail. It is obvious to those skilled in the art that such specific description is only a preferred embodiment, and the scope of the present invention is not limited thereto. As long as one is skilled in the art, he or she should be able to make various applications and modifications within the scope of the present invention based on the above content.

[0198] Accordingly, the actual scope of the invention should be determined by the appended claims and their equivalents.

Claims

1. A hard coating film comprising: Cyclic olefin polymer substrate; an easy-adhesion layer formed on at least one side of the cycloolefin polymer substrate; and a hard coating layer formed on the easy-adhesion layer, The easy-adhesion layer is formed using an easy-adhesion layer-forming composition. The composition for forming an easily adhesive layer comprises a polysiloxane compound having a hydroxyl group in a side chain, a light-transmitting resin, a photoinitiator, and a solvent. The content of the polysiloxane compound having a hydroxyl group in a side chain is 10 to 90 wt % and the content of the light-transmitting resin is 1 to 80 wt % based on 100 wt % of the total solid content in the easily adhesive layer-forming composition.

2. The hard coating film according to claim 1, wherein the total light transmittance is 90% or more. The hard coating film was repeatedly folded and unfolded 200,000 times with a curvature radius of 1 mm so that the hard coating surface was folded inward, and no breakage or peeling of the hard coating occurred. The hard coating film according to claim 1 , wherein the cycloolefin polymer substrate is hydrophilically treated. 4 . The hard coating film according to claim 1 , wherein the hard coating layer is formed using a hard coating composition comprising a light-transmitting resin, a photoinitiator, and a solvent. 5 . The hard coating film according to claim 4 , wherein the light-transmitting resin comprises one or more selected from the group consisting of photocurable (meth)acrylate oligomers and monomers. 6 . An image display device comprising the hard coating film according to claim 1 . 7 . A window of a flexible display device, comprising the hard coating film according to claim 1 . A polarizing plate comprising the hard coating film according to claim 1. 9 . A touch sensor comprising the hard coating film according to claim 1 .