Deformable chromium-containing cobalt-based alloy with improved resistance to galling and chloride-induced crevice corrosion
By adjusting the composition and hot working process of cobalt-based alloys, reducing the nickel content and increasing the nitrogen content, the problems of scratches and crevice corrosion in harsh environments have been solved, achieving higher wear resistance and corrosion resistance, and making it suitable for various product forms.
Patent Information
- Application Number
- CN202180041176.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-11
- Filing Date
- 2021-05-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-05-10
AI Technical Summary
Existing cobalt-based alloys are not sufficiently resistant to scratches and chloride-induced crevice corrosion in harsh environments, especially under high-load, low-speed metal-to-metal sliding conditions and in the presence of chlorides, which lead to wear and corrosion problems.
By adjusting the composition of the cobalt-based alloy, reducing the nickel content to below 3.17% by weight, and increasing the nitrogen content to 0.262 to 0.278% by weight, combined with appropriate hot working processes, a metastable FCC solid solution structure is formed to improve the alloy's scratch resistance and crevice corrosion resistance.
It significantly improves the alloy's resistance to scratches and its tolerance to chloride-induced crevice corrosion, effectively protecting materials in harsh environments and is suitable for various product forms such as castings, weldments, and powder products.
Smart Images

Figure CN115698351B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to cobalt-based corrosion-resistant and wear-resistant alloys. Background Art
[0002] For more than a century, industry has used cobalt-based alloys containing chromium to solve wear problems in severe conditions, namely in corrosive liquids and gases.
[0003] During this time, two main (wear-resistant) types have developed, one containing tungsten and significant levels of carbon (about 1 to 3 weight percent), and the other containing molybdenum and a much lower carbon content. The former alloys exhibit a large amount of carbides in their microstructure, which results in high bulk hardness, excellent resistance to low-stress (scratch) wear, but low ductility. The latter alloys exhibit only small amounts of carbides (if any). Therefore, they are not as hard, but have greater ductility and corrosion resistance.
[0004] Mention should be made of a related group of chromium-containing cobalt-based alloys, designed primarily for high strength at high temperatures and for use in aircraft gas turbine engines, as it is also derived from the above materials.
[0005] Despite popular belief, bulk hardness is not necessarily a good measure of general wear resistance. In fact, there are some wear modes that are more controlled by the nature of the cobalt-rich matrix (rather than by the presence of carbides in the microstructure); these include galling (high load / low speed metal-to-metal sliding), cavitation (caused by the collapse of near-surface bubbles in turbulent liquids), and droplet erosion.
[0006] As for the patent history of cobalt-based alloys containing chromium, the first such alloy was described by Elwood Haynes in U.S. Pat. No. 873,745 (Dec. 17, 1907). U.S. Pat. No. 1,057,423 (Apr. 1, 1913) by the same inventors claimed alloys of cobalt, chromium and tungsten, paving the way for the development of the first major type (associated with the STELLITE trademark). The earliest U.S. patent disclosing the second major type of cobalt-based alloy containing chromium was U.S. Pat. No. 1,958,446 (May 15, 1934), in which Charles H. Prange described the use of such alloys as cast dentures.
[0007] These early alloys were typically used as castings or weld overlays. Deformation and powder metallurgy (P / M) products of some alloys became available in the mid-20th century.
[0008] To understand the role of various alloying elements in cobalt-based alloys, it is important to understand the changes that can occur in the atomic structure of pure cobalt and many of its alloys. At temperatures below about 420°C / 788°F, the stable atomic structure of pure cobalt is hexagonal close-packed (HCP). At higher temperatures (up to the melting point), it is face-centered cubic (FCC). Elements such as nickel, iron, and carbon (within their restricted solubility range) are known to lower the transformation (or phase change) temperature; that is, they extend the temperature range of the FCC structure. Conversely, elements such as chromium, molybdenum, and tungsten increase the transformation temperature (TT); that is, they extend the temperature range of the HCP structure.
[0009] The transformation of cobalt and its alloys from HCP to FCC (and vice versa) by thermal means is slow, so these materials tend to exhibit a metastable FCC form at or near room temperature, when cooled from their molten state, or when cooled after a period exceeding TT. However, the application of mechanical stress at temperatures below TT leads to the rapid formation of HCP regions within the metastable FCC structure. Such regions with a lamellar appearance (during metallographic examination) are believed to arise from the coalescence of stacking faults within the metastable FCC structure. The driving force for this stress-induced metastable FCC to HCP transformation at a given temperature is controlled by TT (i.e., the higher the TT, the greater the tendency).
[0010] The influence of TT on the wear behavior of cobalt and its alloys is known to be significant, since the appearance of HCP lamellae under mechanical stress leads to rapid work hardening, an important property for resistance to plastic deformation. Thus, chromium, molybdenum and tungsten are known to be beneficial to wear resistance, especially resistance to galling, cavitation erosion and droplet erosion. In contrast, nickel, iron and carbon (at low levels, within their soluble range) should be detrimental to wear resistance on the surface.
[0011] Chromium, molybdenum and tungsten also contribute to the resistance of such materials to aqueous corrosion. As with stainless steel and nickel-based alloys, chromium provides passivation (protective surface film) in oxidizing acid solutions, while molybdenum and tungsten increase the nobility of cobalt and its alloys in reducing solutions, where the cathodic reaction is hydrogen evolution.
[0012] The prior art most relevant to the present invention is U.S. Pat. No. 5,002,731 (March 26, 1991), the inventors being Paul Crook, Aziz I. Asphahani and Steven J. Matthews. The commercial embodiment of the patent is called ULTIMET alloy. U.S. Pat. No. 5,002,731 discloses a cobalt-based alloy containing large amounts of chromium, nickel, iron, molybdenum, tungsten, silicon, manganese, carbon and nitrogen. It reveals the unexpected benefits of carbon for both cavitation resistance and corrosion resistance (enhanced by the presence of similar levels of nitrogen). In addition, it reveals that the effect of nickel on cavitation is not strong at least in the content range of 5.3 to 9.8 wt%. The experimental deformation materials used in the discovery of Crook et al. were manufactured by vacuum induction melting, electroslag remelting, hot forging and hot rolling (into sheets and plates) and subsequent solution annealing. Interestingly, a maximum nitrogen content of 0.12 wt% is required because a higher content of 0.19 wt% causes cracking problems during deformation processing.
[0013] Research on the relevant prior art has revealed chromium-containing cobalt-based alloys designed specifically for powder metallurgy processing and used in the biomedical field. The chromium and molybdenum content of an example described in U.S. Patent No. 5,462,575 is similar to that of ULTIMET alloy (a commercial embodiment of U.S. Patent No. 5,002,731) and the alloy of the present invention. However, it does not contain tungsten and requires a special relationship between carbon and nitrogen. More importantly, U.S. Patent No. 5,462,575 requires that aluminum (and other metals that form oxides, such as magnesium, calcium, yttrium, lanthanum, titanium and zirconium) be maintained at extremely low levels (i.e., the sum of these elements should not exceed about 0.01 weight %).
[0014] The material property involved in this discovery is resistance to galling and crevice corrosion. Galling is the term used for damage caused by metal-on-metal sliding under extremely high loads and in the absence of lubrication. It is characterized by total plastic deformation of one or both surfaces, adhesion between the surfaces, and (in most cases) material transfer from one surface to the other. Most stainless steels are particularly susceptible to this form of wear and tend to completely seize under galling test conditions.
[0015] Chloride-induced crevice corrosion occurs in crevices or narrow gaps between structural components or beneath deposits on the surface in the presence of chloride-containing solutions. This attack is associated with the following: local accumulation of positive charges, and the attraction of negatively charged chloride ions to the gaps, which then form hydrochloric acid. This acid accelerates the attack so that the process becomes autocatalytic. Crevice corrosion testing is also a good indicator of chloride-induced pitting corrosion. Summary of the invention
[0016] We have found that the combination of relatively low nickel content and relatively high nitrogen content significantly improves the galling resistance and resistance to chloride-induced crevice corrosion of deformation, chromium-containing, cobalt-based alloys that also contain nickel, iron, molybdenum, tungsten, silicon, manganese, aluminum, carbon and nitrogen. The positive effect on crevice corrosion resistance of reducing the nickel content to 3.17 wt. % and then further to 1.07 wt. % was completely unexpected because at these lower nickel contents, alloys with nitrogen contents of up to 0.278 wt. % can be hot forged and hot rolled into products without difficulty. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a graph of the crevice corrosion and galling test results reported in Table 2 DETAILED DESCRIPTION
[0018] The experimental alloys related to this discovery were produced by vacuum induction melting (VIM) followed by electroslag remelting (ESR) to produce billets of material suitable for hot working. Prior to hot working (i.e., hot forging and hot rolling), the billets were homogenized at 1204°C / 2200°F. Based on existing experience with this type of alloy, a hot working start temperature of 1204°C / 2200°F was used for all experimental alloys. Annealing tests showed that a solution annealing temperature of 1121°C / 2050°F was suitable for this type of material, followed by rapid cooling / quenching (in order to form a metastable FCC solid solution structure at room temperature). In order to enable the production of crevice corrosion test specimens, annealed sheets with a thickness of 3.2 mm / 0.125 inches were produced. In order to enable the production of pins and blocks for galling tests, annealed plates with a thickness of 25.4 mm / 1 inch were produced. Since a single batch of material was insufficient for both types of tests, two batches of Alloy 1 and two batches of Alloy 3 were produced.
[0019] Table 1 gives the actual (analyzed) compositions of the experimental alloys.
[0020] Table 1: Composition of experimental deformation alloys
[0021]
[0022] The experimental steps taken in this work are as follows:
[0023] 1. An experimental version of the commercial embodiment of US 5,002,731 (Alloy 1) was melted and tested, using the same melting, hot working and testing procedures as expected for all other experimental alloys. Two batches were required to make all the required samples.
[0024] 2. Melt and test a reduced (about 3 wt%) nickel version (Alloy 2), with all other elements at Alloy 1 levels.
[0025] 3. Melt and test an increased (about 0.25 wt%) nitrogen version (Alloy 3) with nickel at about 3 wt% and all other elements at Alloy 1 levels. Two batches were required to make all the required samples.
[0026] 4. A further reduced (about 1 wt%) nickel version (Alloy 4) was melted and tested with nitrogen at about 0.25 wt% and all other elements at Alloy 1 levels.
[0027] 5. A medium (about 5 wt%) nickel version (Alloy 5) was melted and tested with nitrogen at about 0.25 wt% and all other elements at Alloy 1 levels.
[0028] 6. A further increased (about 0.35 wt%) nitrogen version (Alloy 6) was melted and tested with nickel at about 3 wt% and all other elements at Alloy 1 levels.
[0029] 7. A further increased (about 0.40 wt%) nitrogen version (Alloy 7) was melted and tested, with nickel at about 3 wt% and all other elements at Alloy 1 levels.
[0030] 8. A version (Alloy 8) was melted and tested in which all elements except nickel (about 3 wt %) and nitrogen (about 0.10 wt %) were at the low end of the range for commercial embodiments of US Pat. No. 5,002,731.
[0031] 9. A version (Alloy 9) was melted and tested in which all elements except nickel (about 3 wt. %) and nitrogen (about 0.40 wt. %) were at the high end of the range for commercial embodiments of U.S. Pat. No. 5,002,731.
[0032] It should be noted that the higher the nitrogen content of the experimental alloys, the higher their chromium content. This was not intentional but is thought to be due to higher chromium recovery rates (than previously experienced) during melting of the material. This may be related to the use of a "chromium nitride" charge as a means of adding nitrogen.
[0033] It is also the case that the actual nitrogen content during this work was often higher than the target nitrogen content. For example, the target nitrogen content for Alloys 1 and 2 was 0.08 wt %, while the actual contents were 0.114 wt % (Alloy 1, Batch A), 0.127 wt % (Alloy 1, Batch B), and 0.109 wt % (Alloy 2). These differences are attributed to the unexpectedly higher nitrogen recoveries during the VIM / ESR melting and remelting of the alloys.
[0034] Aluminum is added to the experimental alloys to react with oxygen and remove oxygen during primary melting (in a laboratory VIM furnace). Aluminum is very important in production-scale air melting, and in addition to being a deoxidizer, it is also used to maintain the extremely high temperatures required during argon-oxygen decarburization (AOD). Manganese is added to help remove sulfur during melting, reaching the levels recommended by U.S. Patent No. 5,002,731. The silicon and carbon levels used in the alloys of the present invention are similar to the levels required in U.S. Patent No. 5,002,731. In these years, such levels have provided excellent welding capabilities. The additional benefits of these levels of carbon, namely excellent cavitation and corrosion resistance, are described in U.S. Patent No. 5,002,731. The dual benefits of chromium, molybdenum and tungsten in terms of resistance to certain forms of wear and corrosion are described in the background section of this article; all three elements (during this work) are kept within the same range required in U.S. Patent No. 5,002,731. Iron is also added to the alloy of the present invention within the range claimed in US Pat. No. 5,002,731, with the major benefit of allowing scrap contaminated with iron to be tolerated during furnace charging, with significant economic benefits.
[0035] The key additions to the deformed cobalt-based alloys described herein are nickel and nitrogen. As previously mentioned, the most important and surprising finding of this work is that reducing the nickel content in the commercial embodiment of U.S. Pat. No. 5,002,731 to below 3.17 wt. % has a strong positive effect on the resistance to chloride-induced crevice corrosion. In addition, considering the prior art (particularly U.S. Pat. No. 5,002,731), it is unexpected that alloys with nitrogen contents above about 0.12 wt. % can be processed into deformed products without difficulty, indicating that lower nickel contents may have a positive effect on the deformability of these high nitrogen alloys.
[0036] The cracking during forging of the three alloys (6, 7, and 9) with the highest nitrogen contents (0.367 wt.%, 0.415 wt.%, and 0.413 wt.%, respectively) may indicate that the solubility of nitrogen has been exceeded, resulting in the presence of one or more additional phases in the ingot microstructure at elevated temperatures. These modified alloys 6, 7, and 9 may not crack if the nitrogen content of these alloys is reduced to levels within the range of alloys 3(A), 3(B), and 4, i.e., 0.262 to 0.278 wt.% (plus or minus the normal manufacturing tolerance for nitrogen is 0.02 wt.%).
[0037] With regard to the effects of reduced nickel content on scratch resistance, these appear to be non-linear (something not predicted by current wear theory). In fact, only at nickel levels of 3.17 wt. % and below does the scratch resistance exceed that of Alloy 1 (the commercial embodiment of U.S. Pat. No. 5,002,731, however with slightly higher nitrogen content due to the above mentioned melting differences).
[0038] Melting this type of alloy under large-scale production conditions requires not only a target content of each element, but also a practical range, taking into account differences caused by element segregation in the casting (real-time) analysis sample, differences caused by secondary melting (such as ESR), and differences caused by chemical analysis. To accommodate these differences, the "plus or minus" tolerances for each intentional addition to the commercial embodiment of U.S. Patent No. 5,002,731 during melting are as follows: chromium ± 1.5 wt%; nickel ± 1.25 wt%; molybdenum ± 0.5 wt%; tungsten ± 0.5 wt%; iron ± 1 wt%; manganese ± 0.25 wt%; silicon ± 0.2 wt%; aluminum ± 0.075 wt%, carbon ± 0.02 wt%; nitrogen ± 0.02 wt%. As a balance, cobalt does not require such a tolerance. For cobalt-based alloys (such as HAYNES 6B alloy) with a nickel content lower than the commercial embodiment of U.S. Patent No. 5,002,731, the plus or minus tolerance for nickel is 0.375 wt%.
[0039] Although the compositions were tested in wrought form, improvements in resistance to chloride-induced crevice corrosion and galling are also found in other product forms such as castings, weldments, and powder products (for use in powder metallurgy processing, additive manufacturing, thermal spraying, and welding).
[0040] Test Results
[0041] The crevice corrosion test used in this work is described in ASTM standard G48 Method D. It involves sheet samples with dimensions of 50.8×25.4×3.2 mm / 2×1×0.125 inches, with a TEFLON crevice assembly attached. Method D enables the determination of the critical crevice temperature (CCT) of the material, i.e., the lowest temperature at which crevice corrosion is observed in a solution of 6 wt. % ferric chloride + 1 wt. % hydrochloric acid over a period of 72 hours (uninterrupted). In this work, the test temperature was limited to 100°C / 212°F, since the ASTM standard does not cover the equipment (i.e., autoclave) required for testing at higher temperatures.
[0042] In order to differentiate the experimental alloys under conditions favorable to galling, wear scars were studied using a modern 3-D surface measurement system based on a laser (LASER), together with galling testing hardware and procedures established in 1980. These procedures involved twisting a pin (15.9 mm / 0.625 in. in diameter) against a fixed block (12.7 mm / 0.5 in. in thickness) ten times through an arc of 121°, using a hand-cranked back-and-forth motion. A load of 2722 kg / 6000 lb was applied by a tensile unit (in compression mode) coupled to a (greased) ball bearing seated on a concave cone machined on top of the pin.
[0043] The scratch test involves self-paired samples (i.e. the pin and block are of the same material), and a laser-based high-precision measurement of the root mean square (RMS) roughness of the block scar.
[0044] All tests covered in this work were repeated under identical conditions. The RMS values given in Table 2 are the average of two abrasion tests. The CCT values given in Table 2 are the lowest temperatures at which crevice corrosion was observed, regardless of whether one or both samples exhibited corrosion at that temperature.
[0045] A higher CCT indicates a higher resistance to chloride-induced crevice corrosion. A lower RMS indicates a higher resistance to galling during (self-coupled) high load / low speed, metal-to-metal sliding.
[0046] Table 2: Crevice corrosion and galling test results
[0047]
[0048] The results in Table 2 are shown in graphical form. Figure 1 middle.
[0049] Table 3 contains broad and preferred ranges for chromium, iron, molybdenum, tungsten, silicon, manganese, and carbon in the alloys disclosed in U.S. Pat. No. 5,002,731. Because the alloys of the present invention are derived from commercial embodiments of U.S. Pat. No. 5,002,731, we expect that any alloy having the following composition will have the same improved resistance to galling and chloride-induced crevice corrosion as the test alloys disclosed herein: up to 3.17 wt. % nickel (normal manufacturing tolerance of plus 0.375 wt. %), 0.262 to 0.278 wt. % nitrogen (normal manufacturing tolerance of plus or minus 0.02 wt. % nitrogen), and 0.08 to 0.13 wt. % aluminum (normal manufacturing tolerance of plus or minus 0.075 wt. % aluminum), and chromium, iron, molybdenum, tungsten, silicon, manganese, and carbon in the ranges disclosed in U.S. Pat. No. 5,002,731.
[0050] Table 3: Ranges of Cr, Fe, Mo, W, Si, Mn and C (weight percentage)
[0051]
[0052] The above manufacturing tolerances / allowances can be applied to the amounts of chromium, iron, molybdenum, tungsten, silicon, manganese, carbon and aluminum in the test alloys of the present invention to determine the acceptable ranges of these elements in our alloys. In addition, if the amounts of chromium, iron, molybdenum, tungsten, silicon, manganese and carbon are the same as required in U.S. Patent No. 5,002,731, we expect that alloys with up to 3.545 wt. % nickel and 0.242 to 0.298 wt. % nitrogen will have the same improved resistance to galling and chloride-induced crevice corrosion.
[0053] While we have described certain presently preferred embodiments of our alloy, it should be understood that the invention is not limited thereto but may be variously embodied within the following claims.
Claims
1. A chromium-containing cobalt-based alloy suitable for deformation processing, which has improved resistance to chloride-induced crevice corrosion and galling, the chromium-containing cobalt-based alloy consisting of: composition: 0.695 to 3.545 wt. % nickel; 0.242 to 0.298 wt % nitrogen; 22.0 to 30.0 wt. % chromium; 3.0 to 10 wt. % molybdenum; Up to 5.0 wt. % tungsten; 1.71 to 7 wt. % iron; 0.05 to 2.0 wt. % manganese; 0.05 to 2.0 wt. % silicon; 0.02 to 0.11 wt. % carbon; 0.005 to 0.205 wt % aluminum; and The remainder is cobalt plus impurities.
2. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy is composed of the following: composition: 1.07 to 3.17 wt. % nickel; 27.96 to 28.12 wt. % chromium; 4.90 to 6.84 wt. % molybdenum; 2.04 to 2.26 wt. % tungsten; 2.71 to 2.92 wt. % iron; 0.77 to 0.90 wt. % manganese; 0.24 to 0.29 wt % silicon; 0.058 to 0.067 wt. % carbon; 0.262 to 0.278 wt % nitrogen; 0.08 to 0.13 wt % aluminum; and The remainder is cobalt plus impurities.
3. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy comprises the following: composition: 0.695 to 3.545 wt. % nickel; 26.46 to 29.62 wt. % chromium; 4.40 to 7.34 wt. % molybdenum; 1.54 to 2.76 wt. % tungsten; 1.71 to 3.92 wt. % iron; 0.52 to 1.15 wt. % manganese; 0.05 to 2.0 wt. % silicon; 0.038 to 0.087 wt. % carbon; 0.242 to 0.298 wt % nitrogen; 0.005 to 0.205 wt % aluminum; and The remainder is cobalt plus impurities.
4. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy comprises the following: composition: 0.695 to 3.545 wt. % nickel; 0.242 to 0.298 wt % nitrogen; 24.0 to 27.0 wt. % chromium; 4.5 to 5.5 wt. % molybdenum; 1.5 to 2.50 wt. % tungsten; 2.0 to 4.0 wt. % iron; 0.5 to 1.0 wt. % manganese; 0.30 to 0.50 wt. % silicon; 0.04 to 0.08 wt.% carbon; 0.005 to 0.205 wt % aluminum; and The remainder is cobalt plus impurities.
5. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy is in the form of a wrought product.
6. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy is in the form of a casting.
7. The chromium-containing cobalt-based alloy of claim 1, wherein the chromium-containing cobalt-based alloy is in the form of a weldment.
8. The chromium-containing cobalt-based alloy according to claim 1, wherein the chromium-containing cobalt-based alloy is in the form of a powder product.