Surface treatment of glass cloth, prepreg and printed wiring board
By controlling the adhesion amount and height of the silane coupling agent in the glass cloth surface treatment layer, the problem of insufficient reliability of the printed wiring board is solved, and the interface adhesion between glass and resin is achieved, and the reliability of the printed wiring board is improved. and productivity.
Patent Information
- Application Number
- CN202180037333.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-27
- Filing Date
- 2021-07-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-07-12
AI Technical Summary
In recent years, the miniaturization and thinning of electronic equipment have led to an increase in the reliability demand for printed wiring boards. It is difficult for the prior art to effectively improve the interface adhesion between glass cloth and resin, resulting in insufficient reliability of printed wiring boards.
By controlling the carbon adhesion amount and arithmetic average height of the silane coupling agent in the glass cloth surface treatment layer, it is ensured that it is within the range of 0.030 to 0.060 mass % and 1.0 to 3.0 nm, and the product is controlled within the range of 0.060 to 0.100 , preferably within the range of 0.075 to 0.097, to improve the interface peeling between the glass and the resin, thereby improving the reliability of the printed wiring board.
By controlling the adhesion amount and height of the silane coupling agent, the reliability of the printed wiring board is significantly improved, the interface adhesion between the glass and the resin is ensured, the mesh deviation and bending are avoided, and the production efficiency is improved.
Smart Images

Figure BDA0003958499870000121 
Figure BDA0003958499870000131
Abstract
Description
Technical Field
[0001] The invention relates to a surface-treated glass cloth, a prepreg and a printed wiring board. Background Art
[0002] Conventionally, as glass cloth used for printed wiring boards, there is known a glass cloth surface-treated with a silane coupling agent in order to improve adhesion with a resin (for example, see Patent Document 1).
[0003] According to the surface-treated glass cloth described in Patent Document 1, the hand feeling does not become hard, and therefore mesh displacement and mesh bending do not occur during winding, and production efficiency is improved.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 5-125663 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, in recent years, due to the miniaturization and thinning of electronic devices, it has been desired to further improve the reliability of printed wiring boards.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a surface-treated glass cloth capable of improving the reliability of a printed wiring board, a prepreg using the surface-treated glass cloth, and a printed wiring board using the surface-treated glass cloth.
[0010] Means for solving problems
[0011] It is known that the reliability of a printed wiring board can be improved by suppressing the surface peeling of glass and resin, and this reliability is closely related to the state of the surface treatment layer of the surface-treated glass cloth. In the past, the state of the surface treatment layer was evaluated by the amount of silane coupling agent attached. The inventors of the present invention have repeatedly conducted in-depth studies on the state of the surface treatment layer of the surface-treated glass cloth, and found that even with the same amount of attachment, the amount of components fixed to the surface of the surface-treated glass cloth and the control of the surface height to a specific range are effective in improving the reliability (whitening distance) of the printed wiring board, thereby completing the present invention.
[0012] Here, the whitening distance is an index indicating the degree of interface peeling between the glass and the resin in the surface treatment layer. Therefore, the smaller the whitening distance is, the higher the reliability of the printed wiring board is.
[0013] Therefore, in order to achieve the above-mentioned object, the technical content of the surface-treated glass cloth of the present invention is as follows. The surface-treated glass cloth has a surface-treated layer on the surface, and the surface-treated glass cloth is characterized in that the surface-treated layer contains a silane coupling agent, the carbon adhesion amount of the fixing component of the surface-treated layer is in the range of 0.030 to 0.060 mass %, the arithmetic mean height of the surface of the fixing component of the surface-treated layer is in the range of 1.0 to 3.0 nm, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is in the range of 0.060 to 0.100.
[0014] According to the surface treated glass cloth of the present invention, by controlling the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component within the range of 0.060 to 0.100, the reliability of the printed wiring board can be improved.
[0015] In the surface treated glass cloth of the present invention, when the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is less than 0.060, the reliability of the printed wiring board cannot be fully improved. In addition, when the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component exceeds 0.100, the fixing component is formed into a block, and a uniform surface treatment cannot be formed, and the interface adhesion is reduced.
[0016] In the surface-treated glass cloth of the present invention, the product of the carbon adhesion amount of the anchor component and the arithmetic mean height of the surface of the anchor component is preferably in the range of 0.075 to 0.097, and more preferably in the range of 0.086 to 0.093.
[0017] In the glass cloth of the present invention, the silane coupling agent is preferably a silane coupling agent having at least one methacryloyl group or at least one acryloyl group, and is more preferably a silane coupling agent having a methacryloyl group.
[0018] Furthermore, the prepreg of the present invention is characterized by comprising the surface-treated glass cloth of the present invention, and the printed wiring board of the present invention is characterized by comprising the surface-treated glass cloth of the present invention. DETAILED DESCRIPTION
[0019] Next, embodiments of the present invention will be described in further detail.
[0020] The surface-treated glass cloth of this embodiment has a surface-treated layer on its surface, the surface-treated layer contains a silane coupling agent, the carbon adhesion amount of the fixing component of the surface-treated layer is in the range of 0.030 to 0.060 mass %, the arithmetic mean height of the surface of the fixing component of the surface-treated layer is in the range of 1.0 to 3.0 nm, the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is in the range of 0.060 to 0.100, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is preferably in the range of 0.075 to 0.097, and more preferably in the range of 0.086 to 0.093.
[0021] The surface-treated glass cloth according to the present embodiment can be produced, for example, in the following manner.
[0022] First, a predetermined glass batch material (glass raw material) is melted and fiberized to obtain glass filaments. The glass composition constituting the glass filaments is not particularly limited, but is preferably a composition of E glass, T glass, NE glass, L glass, or the like. From the perspective of low dielectric constant and low dielectric loss tangent, the above-mentioned glass composition is more preferably NE glass or L glass. Specifically, the following composition is further preferred: relative to the total amount, it contains SiO2 in the range of 48.0 to 62.0 mass%, B2O3 in the range of 17.0 to 26.0 mass%, Al2O3 in the range of 9.0 to 18.0 mass%, MgO in the range of 0 to 6.0 mass%, CaO in the range of 0.1 to 9.0 mass%, Na2O, K2O and Li2O in the range of 0 to 0.5 mass% in total, TiO2 in the range of 0 to 5.0 mass%, SrO in the range of 0 to 6.0 mass%, P2O5 in the range of 0 to 6.0 mass%, and F2 and Cl2 in the range of 0 to 3.0 mass%.
[0023] Here, regarding the measurement of the content of each component of the composition of the glass, Li as a light element can be measured using an ICP emission spectrometer, and other elements can be measured using a wavelength dispersive X-ray fluorescence analyzer.
[0024] The following method can be used as a measurement method. After cutting the glass cloth (in the case where organic matter is attached to the surface of the glass cloth, or in the case where the glass cloth is mainly contained in the organic matter (resin) as a reinforcing material, for example, it is heated in a muffle furnace at a temperature in the range of 300 to 600°C for a time in the range of 2 to 24 hours, etc., and the organic matter is removed before use) into appropriate sizes, it is placed in a platinum crucible, kept at a temperature of 1550°C in an electric furnace for 6 hours, and melted while stirring, thereby obtaining a homogeneous molten glass. Next, the obtained molten glass is poured onto a carbon plate to make glass scraps, which are then crushed and powdered. After the glass powder is heated and decomposed with acid, Li as a light element is quantitatively analyzed using an ICP emission spectrometer. After the glass powder is formed into a disc shape with a press, other elements are quantitatively analyzed using a wavelength dispersive fluorescent X-ray analyzer. After these quantitative analysis results are converted into oxides, the content and total amount of each component are calculated, and the content (mass %) of each of the above components can be calculated based on these numerical values.
[0025] The filament diameter of the glass filament is not particularly limited, but in the application of a printed wiring board, the filament diameter is preferably 10 μm or less, more preferably 8 μm or less, and particularly preferably in the range of 3 to 5 μm.
[0026] The glass filaments are, for example, bundled into glass fiber yarns by a known method, with a number of 25 to 500, and preferably 40 to 300. It should be noted that the following method is called spinning: glass batch material is melted and fiberized to obtain glass filaments, and then a plurality of the glass filaments are bundled into glass fiber yarns.
[0027] The glass fiber yarn preferably has a count of 0.8 to 135 tex, more preferably 1 to 25 tex. The glass fiber yarn count (tex) corresponds to the mass (unit: g) of glass fiber per 1000 m.
[0028] Next, the glass fiber yarn is used as a warp or a weft to weave a glass cloth. The weaving method is not particularly limited, and examples thereof include plain weave, satin weave, and twill weave, and the plain weave is preferably used. The fabric density of the glass fiber yarn during the weaving is not particularly limited, and for example, it is preferably in the range of 10 to 150 strands / 25 mm, and more preferably in the range of 40 to 100 strands / 25 mm.
[0029] During the weaving, a sizing agent is used in bundling the glass filaments, warping the warp yarns, etc. Examples of the sizing agent include a sizing agent whose coating forming agent component is a starch-based or PVA (polyvinyl alcohol)-based sizing agent. The sizing agent may contain an oil or a softener.
[0030] The amount of the sizing agent in the glass cloth is preferably 0.1 to 3 parts by mass, more preferably 0.5 to 1.5 parts by mass, relative to 100 parts by mass of the glass fiber yarn. It should be noted that the range of the amount of the sizing agent, especially the amount of the sizing agent when not specified, represents the average amount of the sizing agent relative to the warp or weft.
[0031] From the viewpoint of use as a substrate for a printed wiring board, the mass per unit area of the glass cloth obtained by the weaving is preferably 110 g / m 2 On the other hand, from the perspective of weavability, the mass per unit area of the glass cloth is 8 g / m 2 above.
[0032] Next, the glass cloth is subjected to a fiber-opening treatment. Examples of the fiber-opening treatment include: a fiber-opening treatment using water flow pressure; a fiber-opening treatment using high-frequency vibration using a liquid as a medium; a fiber-opening treatment using the pressure of a fluid having a surface pressure; a fiber-opening treatment using roller pressure, etc. Among the above fiber-opening treatments, when a fiber-opening treatment using water flow pressure or a fiber-opening treatment using high-frequency vibration using a liquid as a medium is used, it is possible to reduce the deviation of the yarn width after the fiber-opening treatment of the warp and weft yarns, and therefore these two fiber-opening treatments are preferred. In addition, a plurality of fiber-opening treatment methods may be used in combination in the above fiber-opening treatment.
[0033] Next, the glass cloth subjected to the fiber opening treatment is subjected to a deoiling treatment. The deoiling treatment can be performed, for example, by placing the glass cloth in a heating furnace at an ambient temperature in the range of 350 to 450° C. for a period of 40 to 80 hours to heat and decompose the spinning sizing agent and weaving sizing agent attached to the glass cloth.
[0034] Next, the glass cloth subjected to the above-mentioned deoiling treatment is immersed in an aqueous solution of a surface treatment agent, and after removing excess water, it is heated and dried at a temperature range of 80 to 180° C., for example, at 110° C., for a time range of 1 to 30 minutes, for example, for 5 minutes, thereby obtaining the surface-treated glass cloth of the present embodiment.
[0035] The following aqueous solution can be used as the above-mentioned surface treatment agent aqueous solution: relative to the total amount of the surface treatment agent aqueous solution, the solid content contains 0.1-2.0 mass % of a silane coupling agent having at least one methacryloyl group or at least one acryloyl group, and contains 0.5-2.0 mass % of a weak acid (such as acetic acid, citric acid, propionic acid, etc.) as a pH adjuster. The above-mentioned weak acid acts as a catalyst for the hydrolysis reaction of the silane coupling agent. Therefore, when the amount of the weak acid is insufficient, the hydrolysis of the silane coupling agent is insufficient, and the amount of fixation to the glass surface is reduced.
[0036] Examples of the silane coupling agent having at least one methacryloyl group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane. In addition, examples of the silane coupling agent having at least one acryloyl group include 3-acryloxypropylmethyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropylmethyldiethoxysilane, and 3-acryloxypropyltriethoxysilane. The silane coupling agent attached to the glass cloth is preferably in the range of 0.01 to 5 parts by mass relative to 100 parts by mass of the glass fiber yarn.
[0037] Here, the above-mentioned silane coupling agent is attached to the glass surface in the following two cases: the silane coupling agent is firmly fixed to the glass surface chemically; and the silane coupling agent is physically adsorbed to the glass surface. Therefore, in the present invention, the chemically firmly fixed component with the physical adsorption component removed is regarded as the fixing component, and the amount of the fixing component is regarded as the fixing amount.
[0038] Specifically, the fixing component is a component that adheres to the surface-treated glass cloth after the surface-treated glass cloth is immersed in ethanol for 60 seconds and fully dried in a dryer heated to 110° C. for 30 minutes. The carbon adhesion amount of the fixing component is measured using a total nitrogen and total carbon amount measuring device (manufactured by Sumika Analysis Center Co., Ltd., trade name: NC-TRINITY).
[0039] In addition, the arithmetic mean height of the surface of the above-mentioned fixing component was measured by placing a surface-treated glass cloth piece cut into 2 cm squares on the sample stage of an atomic force microscope (AFM, manufactured by Park Systems, trade name: NX20), and measuring the surface shape of the top portion of the monofilament in the surface-treated glass cloth piece. The measurement was performed using an atomic force microscope under the following conditions: the scanning rate was controlled to 0.60 Hz, the number of pixels was set to 256 pixels in the vertical direction and 256 pixels in the horizontal direction, and the surface measurement area was set to 4 μm square.
[0040] From the viewpoint of use as a substrate of a printed wiring board, the thickness of the surface-treated glass cloth is preferably 110 μm or less. On the other hand, from the viewpoint of handleability, the thickness of the surface-treated glass cloth is preferably 8 μm or more.
[0041] Next, examples, comparative examples, and reference examples of the present invention are described.
[0042] Example
[0043] (Example 1)
[0044] In this embodiment, the specification #2116 of IPC 4412 (glass composition: NE glass, yarn used: E250, (fiber diameter 7 μm, yarn weight 20.8 g / 1000 m), warp yarn density: 59 yarns / 25 mm, weft yarn density: 57 yarns / 25 mm, weight per unit area: 95 g / m 2 ) was heated at a temperature of 400-450°C for 60 hours for degreasing treatment, then immersed in an aqueous solution of a glass treatment agent, and after removing excess water, heated and dried at a temperature of 110°C for 5 minutes to obtain a surface-treated glass cloth with a thickness of 90 μm.
[0045] The glass treatment agent aqueous solution was prepared by mixing 1.0 mass % of 3-methacryloxypropyltrimethoxysilane (manufactured by Dow Toray Co., Ltd.) as a silane coupling agent and 0.5 mass % of propionic acid with water, and stirring the mixture with a magnetic stirrer for 1 hour.
[0046] The obtained surface-treated glass cloth was cut into 350 mm×400 mm to obtain a surface-treated glass cloth sheet. At this time, the silane coupling agent attached to the glass cloth was 0.13 parts by mass based on 100 parts by mass of the glass fiber yarn.
[0047] Next, the surface-treated glass cloth sheet was immersed in a polyphenylene ether resin varnish and pre-dried at 150° C. for 10 minutes to obtain a prepreg. The polyphenylene ether resin varnish was composed of 450 parts by mass of oligophenylene ether (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name: OPE-2St), 100 parts by mass of triallyl isocyanurate (manufactured by Evonik Japan Co., Ltd., trade name: TAICROS), 4 parts by mass of α,α'-di(tert-butylperoxy)diisopropylbenzene (manufactured by NOF Corporation, trade name: Perbutyl P), and 250 parts by mass of toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0048] Next, four of the above prepregs were stacked, and fiber membranes were stacked on top of each other. The prepregs were then heated at 205°C and 18 kgf / cm2 using a vacuum hot press (produced by Kitagawa Seiki Co., Ltd.). 2 Under the conditions of , heating and pressing were performed in vacuum for 1 hour to obtain a laminated plate with a thickness of about 0.3 mm.
[0049] Next, the surface-treated glass cloth sheet obtained in this example was immersed in ethanol for 60 seconds, and after being fully dried in a dryer heated to 110° C. for 30 minutes, the carbon adhesion amount of the anchoring component attached to the surface-treated glass cloth sheet was measured using a total nitrogen and total carbon content measuring device (manufactured by Sumika Analysis Center Co., Ltd., trade name: NC-TRINITY). In addition, the surface-treated glass cloth sheet obtained in this example was further cut into 2 cm squares and set on the sample stage of an atomic force microscope (AFM, manufactured by Park Systems, trade name: NX20), the scanning rate was controlled to 0.60 Hz, the number of pixels was set to 256 pixels in the vertical direction and 256 pixels in the horizontal direction, and the surface measurement area was set to 4 μm square. The surface shape of the top part of the monofilament in the surface-treated glass cloth sheet was measured, and the arithmetic mean height of the surface of the above-mentioned anchoring component was measured.
[0050] Next, based on the measurement results, the product of the carbon deposition amount of the anchor component and the arithmetic mean height of the surface of the anchor component is determined.
[0051] Next, the laminate obtained in this embodiment is cut into 7cm×4cm, and a diamond tool is used to cut 2cm long slits in the longitudinal and transverse directions of the laminate to prepare a test piece. A 1 mol / L NaOH (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) aqueous solution is added to a beaker and heated to a temperature of 60°C. After the test piece is immersed in the aqueous solution for 30 hours, a digital microscope (manufactured by KEYENCE Co., Ltd.) is used to measure the whitening distance of the interface peeling between the resin and the glass in the warp direction and the weft direction at a magnification of 100 times. In the measurement, 24 locations in the warp direction and the weft direction are measured respectively, and the average value is calculated and used as the whitening distance. The whitening distance caused by the peeling is correlated with the insulation reliability of the substrate, and the shorter the whitening distance, the better.
[0052] The results are shown in Table 1. In addition, in Table 1, 3-methacryloxypropyltrimethoxysilane is described as "methacryl", and the above-mentioned glass treatment agent aqueous solution is described as a treatment liquid.
[0053] (Example 2)
[0054] In this example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 1, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was controlled to 1.0 mass %.
[0055] Next, except for using the surface treated glass cloth obtained in this example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0056] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this example was used. The results are shown in Table 1.
[0057] (Example 3)
[0058] In this example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 1, except that 3-acryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) was used to replace 3-methacryloxypropyltrimethoxysilane (manufactured by Dow Toray Co., Ltd.) as a silane coupling agent contained in the aqueous solution of the glass treatment agent.
[0059] Next, except for using the surface treated glass cloth obtained in this example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0060] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminate obtained in this example was used. The results are shown in Table 2. In Table 2, 3-acryloxypropyltrimethoxysilane is described as "acrylic" and the glass treating agent aqueous solution is described as treating solution.
[0061] (Example 4)
[0062] In this example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 3, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was controlled to 1.0 mass %.
[0063] Next, except for using the surface treated glass cloth obtained in this example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0064] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this example was used.
[0065] (Example 5)
[0066] In this example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 3, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was controlled to 2.0 mass %.
[0067] Next, except for using the surface treated glass cloth obtained in this example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0068] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this example was used.
[0069] (Comparative Example 1)
[0070] In this comparative example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 1, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was set to 0.1 mass %.
[0071] Next, except for using the surface-treated glass cloth obtained in this comparative example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0072] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this comparative example was used. The results are shown in Table 1.
[0073] (Comparative Example 2)
[0074] In this comparative example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 1, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was controlled to 0.3 mass %.
[0075] Next, except for using the surface-treated glass cloth obtained in this comparative example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0076] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this comparative example was used. The results are shown in Table 1.
[0077] (Comparative Example 3)
[0078] In this comparative example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 3, except that the amount of propionic acid contained in the glass treatment agent aqueous solution was controlled to 0.1 mass %.
[0079] Next, except for using the surface-treated glass cloth obtained in this comparative example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0080] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this comparative example was used.
[0081] (Reference Example 1)
[0082] In this reference example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 1, except that propionic acid was not added to the glass treatment agent aqueous solution.
[0083] Next, except for using the surface-treated glass cloth obtained in this reference example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0084] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this Reference Example was used.
[0085] (Reference Example 2)
[0086] In this reference example, a surface-treated glass cloth, a prepreg, and a laminate were obtained in exactly the same manner as in Example 3, except that propionic acid was not added to the glass treatment agent aqueous solution.
[0087] Next, except for using the surface-treated glass cloth obtained in this reference example, the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component are measured in exactly the same manner as in Example 1, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is calculated based on the measurement results.
[0088] Next, the whitening distance was determined in exactly the same manner as in Example 1 except that the laminated plate obtained in this reference example was used.
[0089] It should be noted that the "whitening distance index" in Tables 1 and 2 is an index that represents the ratio of the whitening distance of the laminated board when no propionic acid is added to the glass treatment agent aqueous solution (acid concentration 0%) is set to 1, and the smaller the whitening distance index, the more improved the reliability of the printed wiring board. Specifically, the whitening distance index of Examples 1 and 2 and Comparative Examples 1 and 2 represents the ratio of the whitening distance when the whitening distance of Reference Example 1 is set to 1, and the whitening distance index of Examples 3 to 5 and Comparative Example 3 represents the ratio of the whitening distance when the whitening distance of Reference Example 2 is set to 1.
[0090] (Table 1)
[0091]
[0092] (Table 2)
[0093]
[0094] As is apparent from Tables 1 and 2, the laminates using the surface treated glass cloths of Examples 1 to 5 have a smaller whitening distance index and improved reliability than the laminates using the surface treated glass cloths of Comparative Examples 1 to 3. In the above Examples 1 to 5, the carbon adhesion amount of the fixing component of the surface treated layer is in the range of 0.030 to 0.060 mass %, the arithmetic mean height of the surface of the fixing component of the surface treated layer is in the range of 1.0 to 3.0 nm, and the product of the carbon adhesion amount of the fixing component and the arithmetic mean height of the surface of the fixing component is in the range of 0.060 to 0.100.
Claims
1. A surface treated glass cloth, characterized in that: The surface treated glass cloth has a surface treated layer on its surface. The surface treatment layer comprises a silane coupling agent, wherein the silane coupling agent has at least one methacryloyl group or at least one acryloyl group. The fixing component of the surface treatment layer is a component attached to the surface treated glass cloth after the surface treated glass cloth is immersed in ethanol for 60 seconds and fully dried in a dryer heated to 110° C. for 30 minutes, and the carbon attachment amount of the fixing component of the surface treatment layer is in the range of 0.030 mass % to 0.060 mass %, The arithmetic mean height of the surface of the anchor component of the surface treatment layer is in the range of 1.0 nm to 3.0 nm, The product of the carbon deposition amount, which is the total carbon amount of the fixing component, and the arithmetic mean height of the surface, which is the average value of the surface heights of the fixing component, is in the range of 0.060 to 0.
100.
2. The surface treated glass cloth according to claim 1, characterized in that: The product of the carbon deposition amount of the fixing component and the arithmetic mean height of the surface of the fixing component is in the range of 0.086 to 0.
093.
3. A prepreg, characterized in that: The invention comprises the surface treated glass cloth according to claim 1 or 2.
4. A printed wiring board, characterized in that The invention comprises the surface treated glass cloth according to claim 1 or 2.