A method for treating arsenic acid wastewater without generating solid hazardous waste
By treating arsenic acid-containing wastewater by lime milk and a mixture of metal salts containing copper, iron and zinc, low-energy consumption arsenic recovery and gypsum slag stabilization, solving the problems of high oxidation energy consumption and solid waste in the prior art, realizing the The economical and environmentally friendly resource treatment effect is achieved.
Patent Information
- Application Number
- CN202110940373.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-15
- Filing Date
- 2021-08-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-08-17
AI Technical Summary
The prior art has problems such as high energy consumption in the oxidation process, high cost of solid hazardous waste, and unrecycled metal salts when treating arsenic acid-containing wastewater, making it difficult to achieve economical and environmentally friendly resource treatment.
Lime milk is used as a pH regulator, combined with a soluble metal salt mixture containing copper, iron and zinc for precipitation treatment. Through neutralization, arsenic deposit, acid leaching and reduction steps, the recovery of arsenic trioxide and the stabilization of gypsum residue are achieved, and recycling is achieved. Acid soak liquid and composite salt precipitation residue.
The arsenic-containing slag is efficiently recovered under low energy consumption. The resulting gypsum slag can be treated as general solid waste, and the acid soak and composite salt can be recycled. The treatment concentration range is wide, the process is simple, and it has good economic and environmental benefits.
Smart Images

Figure BDA0003214605490000051 
Figure BDA0003214605490000052 
Figure BDA0003214605490000053
Abstract
Description
Technical Field
[0001] The invention relates to a method for resource treatment of arsenic-containing waste acid, and in particular to a method for treating arsenic-containing acidic wastewater without generating solid hazardous wastes. The method uses lime milk as a pH regulator, precipitates the arsenic-containing waste acid with composite salts, and recovers arsenic trioxide and gypsum slag from the arsenic-containing composite salt precipitation residue, belonging to the technical field of wastewater resource utilization. Background Art
[0002] The SO2 flue gas produced during non-ferrous smelting and the preparation of sulfuric acid produces a dilute sulfuric acid waste liquid after washing, which is usually called "dirty acid" in the industry. It contains toxic and harmful substances such as arsenic, mercury, copper, zinc, and lead.
[0003] Arsenic is a carcinogen that is toxic to humans and other organisms. The poisoning dose for humans is 0.01 to 0.052 g, and the lethal dose is 0.06 to 0.2 g. Its toxicity is related to its chemical properties and valence state. Generally, inorganic arsenic compounds are more toxic than organic arsenic compounds. The toxicity of trivalent arsenic is about 60 times higher than that of pentavalent arsenic. Arsenic in aqueous solution mainly exists in the form of arsenite and arsenate. Among them, non-ferrous metallurgy is the main industry that produces arsenic-containing wastewater. Its water quality is characterized by high acidity, high arsenic concentration, and complex heavy metal components. There are still a large number of arsenic pollutants discharged into the water environment, and water is a necessary resource for humans, so the effective treatment of arsenic-containing wastewater is urgent.
[0004] At present, the main methods for treating arsenic-containing waste acid include lime iron salt method, sulfidation method, scoralite precipitation method, etc. However, the lime iron salt method requires aeration treatment, produces a large amount of slag, and has a high risk of secondary pollution. The sulfidation method produces toxic gases such as hydrogen sulfide, which not only corrodes equipment but also affects the health of operators. The scoralite precipitation method has problems such as difficult to control stability and high operating costs. Therefore, it is crucial to choose an economical and environmentally friendly treatment method.
[0005] At present, there are many methods for treating arsenic-containing wastewater. For example, patent CN102718259A discloses a method for converting arsenic-containing wastewater into arsenic trioxide by precipitation. The method uses copper sulfate as a precipitant to treat arsenic-containing wastewater. After treatment, arsenic in the waste residue is recovered in the form of arsenic trioxide, and the precipitant copper sulfate is recycled. Although this method can recover arsenic and realize the recycling of the precipitant, the energy consumption in the reduction leaching process is high. Patent CN107116085A discloses a method for collaboratively treating arsenic-containing gypsum slag and arsenic-containing waste acid. The method uses arsenic-containing waste acid to leach arsenic in arsenic-containing gypsum slag, and then uses lime-iron salt method to treat the acid solution after leaching, so that arsenic in the waste acid and arsenic in the arsenic-containing gypsum slag are converted into stable iron arsenate for stacking treatment. Although this method prevents the harm of arsenic and realizes waste treatment with waste, the iron salt used cannot be recycled, and arsenic is not recovered as a resource. Patent CN110627179A discloses a method for treating arsenic-containing wastewater using a recyclable composite salt precipitant. The method uses a mixture of metal salts of calcium, iron, copper, and zinc to treat arsenic-containing wastewater. The arsenic concentration in the treated effluent is less than 0.5 mg / L, and the precipitate residue is acid-leached. The acid leaching solution can be reduced to recover arsenic trioxide. After the arsenic is recovered, the mother liquor can be recycled for the treatment of arsenic-containing wastewater. However, the acid leaching residue produced by this method cannot be converted into general solid waste for treatment. The amount of metal salt used is too large, and the amount of NaOH used for pH adjustment is large, and the cost of the neutralizer is too high. Patent CN102557222 discloses a method for removing trace arsenic from an aqueous solution. The method adds a copper-containing, iron-containing, or zinc-containing reagent to an arsenic-containing solution containing calcium, magnesium, and carbonate, and removes arsenic from the aqueous solution by adjusting the pH and using the principle of adsorption and co-precipitation. Although the method can effectively remove arsenic, the treatment concentration range is small, the arsenic in the precipitate residue is not recovered, and the added metal salt is not recycled. Patent CN109607872A discloses a method for comprehensive utilization of arsenic-containing waste acid and safe disposal of arsenic. The method uses limestone for pre-neutralization, oxidizes As(III) in the filtrate and adds iron salt to precipitate arsenic, and refluxes part of the scorodite back to the bottom of the arsenic precipitation tank as a seed crystal, while the remaining precipitate bottom flow is open. Although the slag obtained by this method is stable and has a low processing cost, the arsenic is still not recovered and the generated slag still needs to be landfilled. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present method is to provide a method for treating arsenic-containing acidic wastewater without generating solid hazardous wastes. The method can directly treat arsenic-containing waste acid without oxidation, can efficiently recover arsenic in arsenic-containing slag under low energy consumption, the pH regulator used is low-cost and easily available, and the obtained arsenic-containing gypsum slag can be converted into general solid waste, the acid leaching solution and the composite salt can be recycled, the wastewater concentration range is wide, the process is simple, and it has good economic and environmental benefits.
[0007] In order to achieve the above technical objectives, the present invention provides a method for treating arsenic acid wastewater without generating solid hazardous waste, comprising the following steps:
[0008] (1) adding lime milk to the arsenic-containing polluted acid to carry out a neutralization reaction, and filtering to obtain arsenic-containing neutralized gypsum slag and a neutralization filtrate;
[0009] (2) adding a soluble metal salt mixture containing copper, iron and zinc to the neutralized filtrate to perform an arsenic precipitation reaction, and filtering to obtain an arsenic-containing composite salt precipitate residue and an arsenic precipitation filtrate;
[0010] (3) leaching the arsenic-containing composite salt precipitate residue with sulfuric acid, filtering to obtain an arsenic-rich leaching solution and an arsenic-containing gypsum residue, introducing SO2 into the arsenic-rich leaching solution for reduction, and evaporating, concentrating, cooling, crystallizing and filtering to obtain arsenic trioxide and arsenic-free mother liquor;
[0011] (4) The arsenic-neutralized gypsum slag is leached with sulfuric acid, and gypsum and arsenic-containing sulfuric acid leaching solution are obtained by filtration, and the arsenic-containing sulfuric acid leaching solution is reused in step (3).
[0012] The present invention uses a soluble metal salt mixture containing copper, iron and zinc as a precipitant. In the range of pH = 7-10, AsO3 in the solution 3- With AsO4 3- It can react with various metal ions in the solution to form precipitation, playing a synergistic role to precipitate arsenic ions in the solution. 2+ The colloid generated by hydrolysis in water can promote the precipitation and adsorption of arsenic, so that arsenic-containing wastewater can be treated efficiently.
[0013] In a preferred embodiment, in step (1), the lime milk is a 10-50wt% CaO emulsion, the pH of the neutralization reaction is 1-3, and the time is 0.5-3h.
[0014] The inventors have found that the amount of lime milk used has a great influence on the arsenic content in the arsenic-neutralized gypsum slag. The preferred neutralization pH value of the present invention can make the arsenic content of the arsenic-neutralized gypsum slag reach a lower level. At this time, As in the waste acid has not begun to react with other heavy metals to form precipitation, so that the obtained gypsum slag can be made purer, and harmless gypsum can be obtained by subsequent simple acid leaching.
[0015] In a preferred embodiment, in step (2), the ratio of the amount of copper, iron and zinc in the soluble metal salt mixture containing copper, iron and zinc to the amount of total arsenic in the neutralization filtrate is: n(Cu) / n(As)=0.1-4.5, n(Fe) / n(As)=0.6-12, n(Zn) / n(As)=0.4-12.
[0016] In a preferred embodiment, in step (2), the pH of the arsenic precipitation reaction is 7-10, and the reaction time is 0.5-3 hours.
[0017] The inventors used a soluble metal salt mixture containing copper, iron and zinc to carry out arsenic precipitation reaction within a suitable pH range and found that when the pH is too low, it is not conducive to the neutralization of arsenic in the filtrate and the soluble metal salt mixture containing copper, iron and zinc to form a precipitate, resulting in excessively high residual arsenic content in the arsenic precipitation filtrate after treatment; and when the pH is too high, the formed arsenic-containing composite salt precipitate residue will re-dissolve, which is not conducive to the removal of arsenic.
[0018] In a preferred embodiment, in step (2), when the As concentration in the arsenic precipitation filtrate is greater than 0.5 mg / L, arsenic precipitation is repeatedly performed using a soluble metal salt mixture containing copper, iron and zinc, wherein the ratio of the amount of copper, iron and zinc substances to the amount of total arsenic substances in the neutralization filtrate is: n(Cu) / n(As)=0.45~4.5, n(Fe) / n(As)=1.2~12, n(Zn) / n(As)=1.2~12.
[0019] In a preferred embodiment, in step (3), during the sulfuric acid leaching process, the sulfuric acid concentration is 0.9 to 3.5 mol / L, the leaching temperature is 20 to 80° C., the leaching time is 0.5 to 4 h, the liquid-to-solid ratio is 3:1 to 6:1 (mL:g), and the leaching times are 2 to 3 times.
[0020] The inventors found that when the liquid-to-solid ratio is too small, the viscosity of the solution is too large during the reaction, which is difficult to stir and filter, and the leaching rate of the arsenic-containing composite salt precipitate is low; when the liquid-to-solid ratio is too large, it has no significant effect on the leaching of arsenic, and other metals cannot be highly enriched, which is not conducive to the subsequent arsenic recovery and the reuse of the dearsenic mother liquor. When the sulfuric acid concentration is too low, the sulfuric acid does not react fully with the arsenic-containing composite salt precipitate, and the arsenic leaching rate decreases; when the sulfuric acid concentration is too high, the leaching of arsenic in the arsenic-containing composite salt precipitate is not significantly improved, but the acid consumption will increase. When the leaching temperature is too low, the reaction rate slows down; when the leaching temperature is too high, the arsenic leaching rate does not increase significantly. When the leaching time is too short, sulfuric acid cannot fully react with the arsenic-containing composite salt precipitate; when the leaching time is too long, the leaching of arsenic is not significantly improved, and the equipment productivity decreases.
[0021] In a preferred embodiment, in step (3), the sulfur dioxide reduction time is 0.3 to 6 hours, the amount of sulfur dioxide used is 1 to 3 times the amount of pentavalent arsenic in the arsenic-rich leaching solution, and the reduction temperature is 20 to 80°C.
[0022] Arsenic coexists in the arsenic-rich leaching solution in the form of As(V) and As(III). The amount of sulfur dioxide added has a significant effect on the recovery of arsenic. If the amount of sulfur dioxide added is too little, the recovery rate of arsenic will decrease. If the amount of sulfur dioxide added is too much, it will have no significant effect on improving the recovery rate of arsenic. Instead, it will cause a waste of sulfur dioxide, worsen the operating environment, and increase production costs.
[0023] In a preferred embodiment, in step (3), according to the amount of the soluble metal salt mixture containing copper, iron and zinc required in step (2), soluble metal salts containing copper and / or iron and / or zinc are added to the dearsenicizing mother liquor, or the soluble metal salts containing copper and / or iron and / or zinc are recovered and returned to step (2) for recycling.
[0024] In the present invention, when the amount of soluble metal salts containing copper and / or iron and / or zinc in the dearsenicating mother liquor is lower than the lower limit of the ratio of the amount of each metal substance to the amount of total arsenic substances in the neutralization filtrate, it is added to the required range and then recycled; and when the amount of soluble metal salts containing copper and / or iron and / or zinc in the dearsenicating mother liquor is higher than the upper limit of the ratio of the amount of each metal substance to the amount of total arsenic substances in the neutralization filtrate, it is recovered to the required range and then recycled.
[0025] In a preferred embodiment, in step (4), during the sulfuric acid leaching process, the sulfuric acid concentration is 0.9 to 3.5 mol / L, the leaching temperature is 20 to 80° C., the leaching time is 0.5 to 4 h, the liquid-to-solid ratio is 3:1 to 6:1 (mL:g), and the leaching times are 2 to 3 times.
[0026] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0027] (1) The present invention uses lime milk as a pH regulator, and a soluble metal salt mixture containing copper, iron, and zinc is used to precipitate arsenic-containing polluted acid. Lime is low in cost and easily available. The precipitate after the reaction is filtered quickly, and no oxidation is required, so the treatment process is simple.
[0028] (2) The present invention uses lime milk as a pH regulator, and the obtained arsenic-containing neutralized gypsum slag and arsenic-containing composite salt precipitation slag can be transformed into general solid waste after acid leaching treatment, and the CaSO4 content in the gypsum meets the requirements of industrial by-product gypsum.
[0029] (3) The arsenic-containing sulfuric acid leaching solution can be repeatedly used for acid leaching of arsenic-containing composite salt precipitate slag without generating wastewater.
[0030] (4) Arsenic trioxide can be recovered from the arsenic-rich leachate after reduction, evaporation concentration, cooling and crystallization. The As content in the leachate is low, the amount of sulfur dioxide required for reduction is small, the arsenic recovery rate is not less than 75%, and the metal ions in the arsenic-free mother liquor after arsenic recovery can be highly enriched and recovered. DETAILED DESCRIPTION
[0031] The following examples are intended to further illustrate the present invention, rather than to limit the scope of protection of the claims of the present invention.
[0032] Example 1
[0033] 300mL of arsenic-containing waste acid with an arsenic content of 7.67g / L was placed in a beaker, and a 20% mass fraction CaO emulsion was used to neutralize the waste acid to pH=3, and the mixture was filtered after stirring for 30 minutes to obtain a neutralized filtrate and arsenic-containing neutralized gypsum slag. According to the molar ratio of Cu / As=0.45, the molar ratio of Fe / As=1.2, and the molar ratio of Zn / As=1.2, a mixed salt of copper sulfate pentahydrate, zinc chloride and ferrous sulfate heptahydrate was added to the neutralized filtrate, and the solution pH was adjusted to 8.5 with 20wt% CaO emulsion; after stirring for 30 minutes, the mixture was filtered to obtain arsenic-containing composite salt precipitate slag and arsenic precipitation filtrate, and the main components of each filtrate are shown in Table 1.
[0034] Table 1 Main components in each filtrate (mg / L)
[0035]
[0036] CaO was used as the pH regulator. After arsenic precipitation treatment, the As content was 3.91 mg / L. The concentrations of Zn, Cu, and Pb in the arsenic precipitation filtrate were all within the range of the Integrated Wastewater Discharge Standard (GB8978-1996).
[0037] Arsenic-containing neutralized gypsum slag was acid-leached under the conditions of liquid-to-solid ratio of 3:1 (mL:g), sulfuric acid concentration of 0.9 mol / L, leaching temperature of 25°C, and leaching time of 0.5 h. Gypsum and arsenic-containing sulfuric acid leaching solution were obtained by filtration. The main components of the arsenic-containing sulfuric acid leaching solution and gypsum are shown in Tables 2 and 3.
[0038] Table 2 Main components in arsenic-containing sulfuric acid leaching solution (g / L)
[0039]
[0040] Table 3 Main element content in gypsum (%)
[0041]
[0042] The arsenic-containing sulfuric acid leaching solution was mixed and used for the first acid leaching of the arsenic-containing composite salt precipitation slag, and 0.9 mol / L sulfuric acid was used for the second and third acid leaching, wherein the liquid-to-solid ratio of each acid leaching was 3:1, the leaching temperature was 25°C, and the leaching time was 0.5 h. The main components of the obtained arsenic-rich leaching solution and arsenic-containing gypsum slag are shown in Tables 4 and 5.
[0043] Table 4 Main components in arsenic-rich leaching solution (g / L)
[0044]
[0045] Table 5 Main element contents in arsenic-containing gypsum slag (%)
[0046]
[0047] According to "HJ0557-2009 Solid Waste Leaching Toxicity Leaching Method - Horizontal Oscillation Method", the gypsum obtained after acid leaching of arsenic-containing neutralized gypsum slag and the arsenic-containing composite salt precipitation slag obtained after acid leaching were subjected to toxicity leaching experiments. The leaching liquid-solid ratio was 10:1 (L:kg), the oscillation frequency was 110±10 times / min, the amplitude was 40mm, and after oscillation at room temperature for 8h, it was left to stand for 16h. The main components of the leachate are shown in Table 6.
[0048] Table 6 Main components in toxic leachate (mg / L)
[0049]
[0050] Note: Leaching toxicity identification standards: As≤5mg / L, Cu≤100mg / L, Zn≤100mg / L, Pb≤5mg / L.
[0051] As shown in Table 6, after acid leaching of arsenic-containing neutralized gypsum slag, the gypsum obtained was subjected to toxicity leaching test, and the As content in the leachate was 4.79 mg / L. After acid leaching of arsenic-containing composite salt precipitation slag, the arsenic-containing gypsum obtained was subjected to toxicity leaching test, and the As content in the leachate was 0.71 mg / L, both of which were less than the national toxicity leaching identification standard value (As≤5 mg / L) specified in GB 5085.3-2007.
[0052] SO2 was introduced into 300 mL of arsenic-rich leaching solution for 2 h. After reduction, the solution was allowed to stand for 2 h. The As reduction rate was 89.33%. The reduced solution was evaporated and concentrated to 1 / 8 of the original volume. After cooling and crystallization at 25°C, it was filtered and dried to obtain arsenic trioxide and arsenic removal mother liquor. 88.90% of the crystallization residue was As2O3. The main components of the arsenic removal mother liquor are shown in Table 7.
[0053] Table 7 Main components in arsenic removal mother liquor (g / L)
[0054]
[0055] According to the Cu / As molar ratio = 1, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, 5 ml of the arsenic removal mother liquor was reused in 300 mL of the above neutralization filtrate, and 20 wt % CaO was used to adjust the solution pH to 9.0. After the arsenic precipitation reaction, the arsenic concentration dropped from 6.59 g / L to 22 mg / L, and the As removal rate was 99.67%.
[0056] Comparative Example 1
[0057] To process 1m 3 The arsenic content was 7.09 g / L and the filtrate was neutralized for economic cost accounting. Different pH regulators were used to treat 1 m 3 The material costs required for neutralizing the filtrate are shown in Tables 8 and 9.
[0058] Table 8 Material costs using 20wt% NaOH as pH regulator
[0059]
[0060] Table 9 Material cost of using 20wt% CaO as pH regulator
[0061]
[0062] To process 1m 3 The economic cost accounting of the neutralization filtrate with an arsenic content of 7.09 g / L was carried out. Zinc chloride, ferrous sulfate heptahydrate and cupric sulfate pentahydrate were used as precipitants, and lime was used as a pH adjuster. When the pH was 8-10, the arsenic-containing composite salt precipitate residue produced about 26.3 kg of slag after three acid leachings, and the cost was about 204.2 yuan. When sodium hydroxide was used as a pH adjuster, the arsenic-containing composite salt precipitate residue produced about 17.2 kg of slag after three acid leachings, and the cost was about 243.7 yuan.
[0063] Compared with using lime as a pH regulator, using sodium hydroxide as a pH regulator can reduce the amount of slag by 34.6%. However, since the price of lime material is significantly lower than that of sodium hydroxide, the overall cost of using lime as a pH regulator is lower.
[0064] Comparative Example 2
[0065] The arsenic-containing complex salt precipitate residue obtained after precipitation using 20wt% NaOH as a pH regulator was acid-leached three times with a sulfuric acid concentration of 0.9mol / L, a liquid-solid ratio of 3:1, and a time of 0.5h. After three acid leachings, the arsenic precipitation filtrate and arsenic-containing gypsum slag were filtered out. The main components in the arsenic-containing gypsum slag are shown in Table 10.
[0066] Table 10 Main element contents in arsenic-containing gypsum slag (%)
[0067]
[0068] According to "HJ0557-2009 Solid Waste Leaching Toxicity Leaching Method-Horizontal Oscillation Method", the arsenic-containing gypsum slag was subjected to a toxicity leaching experiment, with a leaching liquid-solid ratio of 10:1 (L:kg), an oscillation frequency of 110±10 times / min, an amplitude of 40mm, and after oscillation at room temperature for 8h, it was left to stand for 16h. The main components of the leachate are shown in Table 11.
[0069] Table 11 Main components in toxic leachate (mg / L)
[0070]
[0071] Note: Leaching toxicity identification standards: As≤5mg / L, Cu≤100mg / L, Zn≤100mg / L, Pb≤5mg / L.
[0072] As shown in Table 10, the arsenic-containing composite salt precipitate residue obtained by acid leaching three times with NaOH as the pH regulator still has a high As content of 1.13%. After verification by the toxicity leaching experiment, the As concentration in the leachate is 14.2 mg / L, which cannot be converted into general solid waste.
[0073] Example 2
[0074] Take 1L of arsenic-containing waste acid with an arsenic content of 7.67g / L and place it in a beaker. Use a CaO emulsion with a mass fraction of 20% to neutralize the waste acid to pH = 2. Stir and react for 30 minutes and then filter to obtain a neutralized filtrate and arsenic-containing neutralized gypsum slag. According to the Cu / As molar ratio = 0.45, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, add a mixed salt of copper sulfate pentahydrate, zinc chloride and ferrous sulfate heptahydrate to the neutralized filtrate, and use 20wt% CaO emulsion to adjust the solution pH to 8.5; stir and react for 30 minutes and then filter to obtain an arsenic precipitation filtrate and an arsenic-containing composite salt precipitation slag. The main components in each filtrate are shown in Table 12.
[0075] Table 12 Main components in each filtrate (mg / L)
[0076]
[0077] CaO was used as the pH regulator. After arsenic precipitation treatment, the As content was 2.68 mg / L. The concentrations of Zn, Cu, and Pb in the arsenic precipitation filtrate were all within the range of the Integrated Wastewater Discharge Standard (GB8978-1996).
[0078] The arsenic-containing neutralized gypsum slag was acid-leached under the conditions of liquid-to-solid ratio of 3:1 (mL:g), sulfuric acid concentration of 0.9 mol / L, leaching temperature of 25°C, and leaching time of 0.5 h. Gypsum and arsenic-containing sulfuric acid leaching solution were obtained by filtration. The main components of the arsenic-containing sulfuric acid leaching solution and gypsum are shown in Tables 13 and 14.
[0079] Table 13 Main components in arsenic-containing sulfuric acid leaching solution (g / L)
[0080]
[0081] Table 14 Main element content in gypsum (%)
[0082]
[0083] It can be seen from Table 14 that after two acid leachings, the arsenic content in the gypsum dropped to 0.052%. The arsenic-containing sulfuric acid leaching solution was mixed and used for the first acid leaching of the arsenic-containing composite salt precipitation slag, and 1 mol / L sulfuric acid was used for the second and third acid leachings. The liquid-to-solid ratio of each acid leaching was 3:1, the leaching temperature was 25°C, and the leaching time was 0.5h. The main components of the obtained arsenic-rich leaching solution and the arsenic-containing gypsum slag are shown in Tables 15 and 16.
[0084] Table 15 Main components in arsenic-rich leaching solution (g / L)
[0085]
[0086] Table 16 Main element contents in arsenic-containing gypsum slag (%)
[0087]
[0088] According to "HJ0557-2009 Solid Waste Leaching Toxicity Leaching Method - Horizontal Oscillation Method", the gypsum obtained after acid leaching of arsenic-containing neutralized gypsum slag and the arsenic-containing gypsum slag obtained after acid leaching of arsenic-containing composite salt precipitation slag were subjected to toxicity leaching experiments. The leaching liquid-solid ratio was 10:1 (L:kg), the oscillation frequency was 110±10 times / min, the amplitude was 40mm, and after oscillation at room temperature for 8h, it was left to stand for 16h. The main components of the leachate are shown in Table 17.
[0089] Table 17 Main components in toxic leachate (mg / L)
[0090]
[0091] Note: Leaching toxicity identification standards: As≤5mg / L, Cu≤100mg / L, Zn≤100mg / L, Pb≤5mg / L.
[0092] As shown in Table 17, after acid leaching of arsenic-containing neutralized gypsum slag, the gypsum obtained was subjected to toxicity leaching test, and the As content in the leaching solution was 3.48 mg / L. After acid leaching of arsenic-containing composite salt precipitation slag, the arsenic-containing gypsum slag obtained was subjected to toxicity leaching test, and the As content in the toxic leaching solution was 0.92 mg / L, both of which were less than the national toxicity leaching identification standard value (As≤5 mg / L) specified in GB5085.3-2007.
[0093] Take 300mL of arsenic-rich leaching solution and pass SO2 for 1.5h. The As reduction rate is 79.08%. The reduced solution is evaporated and concentrated to 1 / 8 of the original volume. After cooling and crystallization at 25°C, it is filtered and dried to obtain arsenic trioxide and arsenic removal mother liquor. 83.70% of the crystallization residue is As2O3. The main components of the arsenic removal mother liquor are shown in Table 18.
[0094] Table 18 Main components of arsenic removal mother liquor (g / L)
[0095]
[0096] According to the Cu / As molar ratio = 1, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, 5 mL of arsenic removal mother liquor was added to 300 mL of the above neutralization filtrate, and 20 wt % CaO was used to adjust the solution pH to 9.0. After treatment, the arsenic concentration dropped from 7.09 g / L to 50.78 mg / L, and the As removal rate was 99.28%.
[0097] Example 3
[0098] Take 1L of arsenic-containing waste acid with an arsenic content of 3.08g / L and place it in a beaker. Use a CaO emulsion with a mass fraction of 20% to neutralize the waste acid to pH = 2. Stir and react for 30 minutes and then filter to obtain a neutralized filtrate and arsenic-containing neutralized gypsum slag. According to the Cu / As molar ratio = 1, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, add a mixed salt of copper sulfate pentahydrate, zinc chloride and ferrous sulfate heptahydrate to the neutralized filtrate, and use 20wt% CaO emulsion to adjust the solution pH to 8.5; stir and react for 30 minutes and then filter to obtain an arsenic precipitation filtrate and an arsenic-containing composite salt precipitation slag. The main element contents in each filtrate are shown in Table 19.
[0099] Table 19 Content of each component in each filtrate (mg / L)
[0100]
[0101] CaO was used as the pH regulator. After arsenic precipitation treatment, the As content was 3.55 mg / L. The concentrations of Zn, Cu, and Pb in the arsenic precipitation filtrate were all within the range of the Integrated Wastewater Discharge Standard (GB8978-1996).
[0102] Under the conditions of liquid-to-solid ratio of 3:1 (mL:g), sulfuric acid concentration of 0.9 mol / L, leaching temperature of 25°C, and leaching time of 0.5 h, the arsenic-containing neutralized gypsum slag was leached and then filtered to obtain arsenic-containing sulfuric acid leaching solution and gypsum. The contents of each component in the arsenic-containing sulfuric acid leaching solution and gypsum are shown in Tables 20 and 21.
[0103] Table 20 Main element concentrations in arsenic-containing sulfuric acid leaching solution (g / L)
[0104]
[0105] Table 21 Main element content in gypsum (%)
[0106]
[0107] The arsenic-containing sulfuric acid leaching solution was mixed and used for the first acid leaching of the arsenic-containing composite salt precipitation slag, and 1 mol / L sulfuric acid was used for the second and third acid leaching. The liquid-to-solid ratio of each acid leaching was 3:1, the leaching temperature was 25°C, and the leaching time was 1 h. The concentrations of main elements in the obtained arsenic-rich leaching solution and arsenic-containing gypsum slag are shown in Tables 22 and 23.
[0108] Table 22 Main components in arsenic-rich leaching solution (g / L)
[0109]
[0110] Table 23 Main element contents in arsenic-containing gypsum slag (%)
[0111]
[0112] According to "HJ0557-2009 Solid Waste Leaching Toxicity Leaching Method - Horizontal Oscillation Method", the gypsum obtained after acid leaching of arsenic-containing neutralized gypsum slag and the arsenic-containing gypsum slag obtained after acid leaching of arsenic-containing composite salt precipitation slag were subjected to toxicity leaching experiments. The leaching liquid-solid ratio was 10:1 (L:kg), the oscillation frequency was 110±10 times / min, the amplitude was 40mm, and after oscillation at room temperature for 8h, it was left to stand for 16h. The main components of the leachate are shown in Table 24.
[0113] Table 24 Main element contents in toxic leachate (mg / L)
[0114]
[0115] Note: Leaching toxicity identification standards: As≤5mg / L, Cu≤100mg / L, Zn≤100mg / L, Pb≤5mg / L.
[0116] As shown in Table 24, after acid leaching of arsenic-containing neutralized gypsum slag, the gypsum obtained was subjected to toxicity leaching test, and the As content in the leaching solution was 4.79 mg / L. After acid leaching of arsenic-containing composite salt precipitation slag, the arsenic-containing gypsum slag obtained was subjected to toxicity leaching test, and the As content in the toxic leaching solution obtained was 0.71 mg / L, which was less than the national toxicity leaching identification standard value (As≤5 mg / L) stipulated in GB5085.3-2007.
[0117] Take 500mL of arsenic-rich leaching solution, pass SO2 for 1h, and let it stand for 2h after reduction. The As reduction rate can reach 86.94%. Evaporate and concentrate the reduced solution to 1 / 10 of the original volume. After cooling and crystallization at 25℃, filter and dry to obtain arsenic trioxide and arsenic removal mother liquor. 73.71% of the crystallization residue is As2O3. The main components of the arsenic removal mother liquor are shown in Table 25.
[0118] Table 25 Main components of arsenic removal mother liquor (g / L)
[0119]
[0120] According to the Cu / As molar ratio = 1, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, 10 ml of arsenic removal mother liquor was added to 300 mL of the above neutralization filtrate, and 20 wt % CaO was used to adjust the solution pH to 9.0. After treatment, the arsenic concentration dropped from 2.23 g / L to 17.87 mg / L, and the As removal rate could reach 99.38%.
[0121] Example 4
[0122] 500mL of arsenic-containing waste acid with an arsenic content of 7.67g / L was placed in a beaker, and the waste acid was neutralized to pH=3 with a CaO emulsion of 20% by mass. After stirring for 30 minutes, the neutralized filtrate and arsenic-containing neutralized gypsum slag were obtained. According to the molar ratio of Cu / As=0.45, the molar ratio of Fe / As=0.6, and the molar ratio of Zn / As=0.6, a mixed salt of zinc chloride, ferrous sulfate heptahydrate, and copper sulfate pentahydrate was added to the neutralized filtrate, and the solution pH=7 was adjusted with 20wt% CaO emulsion; after stirring for 30 minutes, the arsenic precipitation filtrate and arsenic-containing composite salt precipitation slag were obtained by filtering. The main components in each filtrate are shown in Table 26.
[0123] Table 26 Main components in each filtrate (mg / L)
[0124]
[0125] CaO was used as the pH regulator. After arsenic precipitation treatment, the As content was 12.52 mg / L. The concentrations of Zn, Cu, and Pb in the filtrate were all within the range of the Integrated Wastewater Discharge Standard (GB8978-1996).
[0126] Arsenic-containing neutralized gypsum slag was leached under the conditions of liquid-to-solid ratio of 3:1 (mL:g), sulfuric acid concentration of 1 mol / L, leaching temperature of 25°C, and leaching time of 0.5 h. Gypsum and arsenic-containing sulfuric acid leaching solution were obtained by filtration. The main components in the arsenic-containing sulfuric acid leaching solution and gypsum are shown in Tables 27 and 28.
[0127] Table 27 Main components in arsenic-containing sulfuric acid leaching solution (g / L)
[0128]
[0129] Table 28 Main element content in gypsum (%)
[0130]
[0131] The arsenic-containing sulfuric acid leachate was mixed and used for the first acid leaching of the arsenic-containing composite salt precipitation slag, and 0.9 mol / L sulfuric acid was used for the second and third acid leaching. The liquid-to-solid ratio of each acid leaching was 3:1, the leaching temperature was 25°C, and the leaching time was 0.5 h. The main components of the obtained arsenic-rich leachate and arsenic-containing gypsum slag are shown in Tables 29 and 30.
[0132] Table 29 Main components in arsenic-rich leaching solution (g / L)
[0133]
[0134] Table 30 Main element content in arsenic-containing gypsum slag (%)
[0135]
[0136] According to "HJ0557-2009 Solid Waste Leaching Toxicity Leaching Method - Horizontal Oscillation Method", the gypsum obtained after acid leaching of arsenic-containing neutralized gypsum slag and the arsenic-containing gypsum slag obtained after acid leaching of arsenic-containing composite salt precipitation slag were subjected to toxicity leaching experiments. The leaching liquid-solid ratio was 10:1 (L:kg), the oscillation frequency was 110±10 times / min, the amplitude was 40mm, and after oscillation at room temperature for 8h, it was left to stand for 16h. The main components of the leachate are shown in Table 31.
[0137] Table 31 Main components in toxic leachate (mg / L)
[0138]
[0139] Note: Leaching toxicity identification standards: As≤5mg / L, Cu≤100mg / L, Zn≤100mg / L, Pb≤5mg / L.
[0140] As shown in Table 31, after acid leaching of arsenic-containing neutralized gypsum slag, the gypsum obtained was subjected to toxicity leaching test, and the As content in the leaching solution was 1.42 mg / L. After acid leaching of arsenic-containing composite salt precipitation slag, the arsenic-containing gypsum slag was subjected to toxicity leaching test, and the As content in the toxic leaching solution was 3.74 mg / L, both of which were less than the national toxicity leaching identification standard value (As≤5 mg / L) specified in GB5085.3-2007.
[0141] Take 300mL of arsenic-rich leaching solution, pass SO2 for 1h, and let it stand for 1h after reduction. The As reduction rate can reach 79.08%. Evaporate and concentrate the reduced solution to 1 / 6 of the original volume. After cooling and crystallization at 25°C, filter and dry to obtain arsenic trioxide and arsenic removal mother liquor. 83.89% of the crystallization residue is As2O3. The main components of the arsenic removal mother liquor are shown in Table 32.
[0142] Table 32 Main components of arsenic removal mother liquor (g / L)
[0143]
[0144] According to the Cu / As molar ratio = 1, Fe / As molar ratio = 1.2, and Zn / As molar ratio = 1.2, 12 ml of arsenic removal mother liquor was added to 300 mL of the above neutralization filtrate, and 20 wt % CaO was used to adjust the solution pH to 8.5-9.0. After arsenic precipitation, the arsenic concentration dropped from 6.59 g / L to 28.59 mg / L, and the As removal rate was 99.72%.
[0145] Take 300mL of arsenic precipitation filtrate containing 12.52mg / L As for repeated arsenic precipitation, add zinc chloride, ferrous sulfate heptahydrate and copper sulfate pentahydrate according to n(Cu) / n(As)=2.3, n(Fe) / n(As)=6, n(Zn) / n(As)=6, and adjust the solution pH to 8 with 20wt% CaO; stir and react for 30min and filter to obtain secondary arsenic-containing composite salt precipitate residue and secondary arsenic precipitation filtrate. The composition of the secondary arsenic precipitation filtrate is shown in Table 33, and the main element content of the secondary arsenic-containing composite salt precipitate residue after drying is shown in Table 34.
[0146] Table 33 Secondary arsenic precipitation filtrate composition (mg / L)
[0147]
[0148] Table 34 Content of each component in secondary arsenic-containing composite salt precipitation slag (%)
[0149]
[0150] It can be seen from Table 33 that after repeated arsenic precipitation treatment, the As in the secondary arsenic precipitation filtrate is 0.40 mg / L, and the concentrations of As, Fe, Cu, Zn, and Pb all meet the emission standards of the "Comprehensive Sewage Discharge Standard" (GB8978-1996).
Claims
1. A method for treating arsenic acid wastewater without generating solid hazardous waste, characterized in that: The steps include: (1) adding lime milk to the arsenic-containing waste acid for neutralization reaction, filtering to obtain arsenic-containing neutralized gypsum slag and neutralization filtrate; the lime milk is 10-50wt% CaO emulsion, the pH of the neutralization reaction is 1-3, and the time is 0.5-3h; (2) adding a soluble metal salt mixture containing copper, iron and zinc to the neutralization filtrate to carry out arsenic precipitation reaction, filtering to obtain arsenic-containing composite salt precipitate residue and arsenic precipitation filtrate; in the soluble metal salt mixture containing copper, iron and zinc, the ratio of the amount of copper, iron and zinc to the amount of total arsenic in the neutralization filtrate is: n(Cu) / n(As)=0.1-4.5, n(Fe) / n(As)=0.6-12, n(Zn) / n(As)=0.4-12; (3) leaching the arsenic-containing composite salt precipitate residue with sulfuric acid, filtering to obtain an arsenic-rich leaching solution and an arsenic-containing gypsum residue, introducing SO2 into the arsenic-rich leaching solution for reduction, and evaporating, concentrating, cooling, crystallizing and filtering to obtain arsenic trioxide and arsenic-free mother liquor; (4) The arsenic-neutralized gypsum slag is leached with sulfuric acid, and the gypsum and arsenic-containing sulfuric acid leaching solution are obtained by filtration, and the arsenic-containing sulfuric acid leaching solution is reused in step (3).
2. A method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (2), the pH of the arsenic precipitation reaction is 7-10, and the time is 0.5-3h.
3. The method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (2), when the As concentration in the arsenic precipitation filtrate is greater than 0.5 mg / L, arsenic precipitation is repeated using a soluble metal salt mixture containing copper, iron and zinc, wherein the ratio of the amount of copper, iron and zinc substances to the amount of total arsenic substances in the neutralization filtrate is: n(Cu) / n(As)=0.45~4.5, n(Fe) / n(As)=1.2~12, n(Zn) / n(As)=1.2~12.
4. The method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (3), during the sulfuric acid leaching process, the sulfuric acid concentration is 0.9-3.5 mol / L, the leaching temperature is 20-80° C., the leaching time is 0.5-4 h, the liquid-to-solid ratio is 3:1-6:1 (mL:g), and the leaching times are 2-3 times.
5. The method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (3), the sulfur dioxide reduction time is 0.3 to 6 hours, the amount of sulfur dioxide used is 1 to 3 times the amount of pentavalent arsenic in the arsenic-rich leaching solution, and the reduction temperature is 20 to 80°C.
6. The method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (3), according to the amount of the soluble metal salt mixture containing copper, iron and zinc required in step (2), the soluble metal salt containing copper and / or iron and / or zinc is added to the dearsenicizing mother liquor, or the soluble metal salt containing copper and / or iron and / or zinc is recovered and returned to step (2) for recycling.
7. The method for treating arsenic acid wastewater without generating solid hazardous waste according to claim 1, characterized in that: In step (4), during the sulfuric acid leaching process, the sulfuric acid concentration is 0.9-3.5 mol / L, the leaching temperature is 20-80° C., the leaching time is 0.5-4 h, the liquid-to-solid ratio is 3:1-6:1 (mL:g), and the leaching times are 2-3 times.