A method for optimizing nickel-titanium alloy performance based on laser selective melting

Through multiple laser remelting and adjustment of process parameters in the selective laser melting manufacturing of nickel-titanium alloys, the production difficulties of complex nickel-titanium alloy structures and the narrow process window have been solved, and nickel-titanium alloy manufacturing with high density and strong shape memory characteristics has been achieved. pieces.

CN115703153BActive Publication Date: 2024-10-01FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110943978.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-17
Publication Date
2024-10-01
Estimated Expiration
2041-08-17

AI Technical Summary

Technical Problem

Traditional nickel-titanium alloy manufacturing processes are difficult to produce complex structures. The laser selective melting process window is mutually constrained by phase change characteristics and mechanical properties, resulting in a narrow range of process window options and difficulty in obtaining high-density alloys and shape memory properties at the same time.

Method used

In the process of preparing nickel-titanium alloy by selective laser melting, after laser scanning each layer, the laser is used again to remelt the forming layer without re-powdering, and the process parameters are adjusted to optimize energy density and improve density and mechanical properties. , while maintaining or increasing the phase transition temperature.

Benefits of technology

Through multiple laser remelting, the optional range of NiTi alloy laser selective melting manufacturing process window is expanded, the density and mechanical properties are improved, the shape memory characteristics are enhanced, and internal defects are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115703153B_ABST
    Figure CN115703153B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for optimizing the performance of nickel-titanium alloy based on laser selective melting. The method comprises the following steps: in the process of preparing nickel-titanium alloy by laser selective melting, after laser scanning each layer, the laser is used again to remelt the forming layer without re-spreading powder, and the number of remelting is recorded as N, where N≥1 and is an integer. Through this method, the density of NiTi alloy parts can be improved and the mechanical properties can be optimized during the laser selective melting manufacturing process of NiTi alloy, and the phase transition temperature of NiTi alloy can be not affected, and the phase transition temperature can even be further increased, so that NiTi alloy exhibits a strong shape memory property. Thereby expanding the optional range of the laser selective melting manufacturing process window of NiTi alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nickel-titanium alloys and relates to a method for optimizing the performance of nickel-titanium alloys based on a laser selective melting method. Background Art

[0002] NiTi alloy has attracted wide attention from researchers due to its unique properties, such as shape memory effect (SME) and superelasticity (SE). This is because the martensite (B2) and austenite (B19') in NiTi alloy will transform into each other under the change of ambient temperature, which is related to the phase transition temperature, making it a material with multiple application prospects. In the past few decades, NiTi alloy has been widely used in aerospace, medical orthodontics and cardiovascular stents. However, NiTi alloy parts manufactured by traditional processes are difficult to manufacture highly complex structural shapes, making NiTi products mostly simple geometric shapes, which greatly limits their use.

[0003] Selective laser melting (SLM) technology has great potential in solving the complex molding and manufacturing of NiTi alloy parts. Because selective laser melting is a type of metal 3D printing technology, it is based on the manufacturing concept of "layered manufacturing, layer-by-layer molding", that is, the sequential molding of "points into lines into surfaces into bodies". CAD / CAE software is used for modeling, and then the complex model is sliced ​​in layers through the software. Each slice contains all the geometric information of the layer. Finally, a high-energy laser beam is used to melt the metal powder layer by layer until a complete part is formed.

[0004] However, keyholes or metallurgical holes are usually formed inside the workpiece during the laser selective melting process. These defects will reduce the mechanical properties of NiTi alloys, and the control of properties is weaker than that of traditional manufacturing processes. The material is usually not disturbed by external interference during SLM, and these defects are basically optimized and eliminated by adjusting process parameters such as laser power, scanning speed, scanning spacing and powder layer thickness. Therefore, laser energy input plays a vital role in the SLM process. However, energy density makes it difficult to better match phase change characteristics with mechanical properties in some cases. For example, it has been proved that it is difficult to obtain high-density NiTi alloys with shape memory properties (SME) under high laser power, because the samples mostly show superelasticity (SE) at this time. To obtain NiTi alloys with strong shape memory (SME), it is necessary to reduce the laser scanning speed, but this will make the internal defects of the sample too large, because to manufacture high-density alloys, high laser power and high laser scanning speed need to be matched, so there will be contradictions. Therefore, the SLM process window of NiTi alloy is constrained by the mutual constraints of phase change characteristics and mechanical properties, resulting in a narrow range of optional process windows.

[0005] In summary, NiTi alloy is a unique functional material with shape memory (SME) and superelasticity (SE), which is related to the phase transition temperature and ambient temperature. This material can be used to manufacture shape memory structural parts. However, traditional manufacturing methods are more difficult to control the production of NiTi alloy parts with complex structures because they are affected and restricted by the phase transition temperature and mechanical properties. Selective laser melting has the advantage of accurately manufacturing complex shape structures, but the high-density alloy with shape memory (SME) obtained under high laser power is inconsistent with the superelasticity (SE) characteristics of NiTi alloy manufactured under high laser power, which finally leads to the problem of narrow process window selection range. Summary of the invention

[0006] In order to improve the above-mentioned technical problems existing in the prior art, the present invention provides a method for optimizing the performance of nickel-titanium alloy, the method comprising the following steps: in the process of preparing nickel-titanium alloy by laser selective melting, after laser scanning each layer, the laser is used again to remelt the molded layer without re-powdering, and the number of remelting is recorded as N, N≥1 and is an integer.

[0007] According to an embodiment of the present invention, the selection of N can be adjusted according to demand, for example, N=1, 2, 3, 4, 5, 6, 7, 8, 9, 10.

[0008] According to an embodiment of the present invention, the method includes: placing three-dimensional STL data of the product in a laser selective melting device, first assigning process parameters for the first laser scan as required, and then using the laser again to assign process parameters for N laser remeltings in sequence as required.

[0009] For example, the process conditions of the first laser scanning include: scanning laser power (P) is 10~95W, spot diameter (d) is 30~50μm, scanning speed (v) is 250~800mm / s, scanning spacing (h) is 80~110μm, and powder layer thickness (t) is 25~30μm.

[0010] Preferably, the process conditions of the first laser scanning include: scanning laser power (P) is 40-70W, spot diameter (d) is 35-45μm, scanning speed (v) is 250-500mm / s, scanning spacing (h) is 90-100μm, and powder layer thickness (t) is 25-30μm.

[0011] For example, the energy density of the process parameters used in each remelting laser scan is 72% to 100% of the energy density of the first laser scan, preferably 75% to 100%, for example, 75%, 80%, 85%, 90%, 95%. Further, the range of process parameters used in each remelting laser scan includes: laser power (P) 10 to 95W, spot diameter (d) 30 to 50μm, scanning speed (v) 250 to 800mm / s, scanning spacing (h) 80 to 110μm, and powder layer thickness (t) 25 to 30μm. Preferably, the range of process parameters used in each remelting laser scan includes: scanning laser power (P) 40 to 70W, spot diameter (d) 35 to 45μm, scanning speed (v) 250 to 500mm / s, scanning spacing (h) 90 to 100μm, and powder layer thickness (t) 25 to 30μm.

[0012] Among them, the energy density formula is: E=P / vht.

[0013] According to an embodiment of the present invention, the scanning strategy of the laser scanning may be chessboard scanning or island scanning.

[0014] Exemplarily, the process conditions of the first laser scanning include: scanning laser power (P) of 60 W, scanning speed (v) of 250 mm / s, scanning spacing (h) of 110 μm, powder layer thickness (t) of 25 μm, and scanning strategy of chessboard scanning;

[0015] The number of remelting times N=1, the energy density of the process parameters used by the first remelting laser is 75% of the energy density of the first laser scanning; for example, compared with the process conditions of the first laser scanning, only the scanning laser power (P) is adjusted to 45W, and other conditions remain unchanged;

[0016] Alternatively, the energy density of the process parameters used by the first remelting laser is 100% of the energy density during the first laser scanning; for example, the process conditions used by the first remelting laser are the same as the process conditions of the first laser scanning.

[0017] According to an embodiment of the present invention, the powder is a pre-alloyed near-equiatomic ratio NiTi powder prepared by atomic atomization, the powder particle diameter is distributed in the range of 15 to 53 μm, and is vacuum dried before use, preferably vacuum dried at 60 to 120°C for 4 to 5 hours.

[0018] According to an embodiment of the present invention, the method comprises the step a) using CAD / CAE modeling software to design a model according to requirements.

[0019] According to an embodiment of the present invention, the three-dimensional STL data of the placed articles is set according to the model designed in step a).

[0020] According to the embodiment of the present invention, in laser forming, the laser will preferentially scan the parameters set for the first time, and then perform remelting scanning in sequence according to the set order and process conditions.

[0021] According to an embodiment of the present invention, the laser selective melting device is any laser selective melting device known in the art.

[0022] The present invention also provides a method for preparing a nickel-titanium alloy product, comprising the following steps: using a laser to print and shape a sample processed by the above method for optimizing the performance of the nickel-titanium alloy on a substrate to obtain a nickel-titanium alloy product.

[0023] According to an embodiment of the present invention, during the printing process, the oxygen content must be ensured to be ≤500ppm (i.e., the oxygen content value displayed by the oxygen sensor in the laser selective melting equipment is ≤0.05%), argon gas protection is used, and the gas pressure is maintained at 10-20mbar.

[0024] According to an embodiment of the present invention, the substrate is a NiTi alloy substrate.

[0025] Beneficial effects of the present invention

[0026] In view of the technical problem of narrow process window for manufacturing NiTi alloy parts by laser selective melting, the method for optimizing the performance of nickel-titanium alloy based on laser selective melting technology provided by the present invention utilizes laser selective melting technology and cooperates with CAD / CAE software to perform iterative modeling and slicing. After laser scanning each layer, the laser is used again to remelt the molding layer without re-spreading powder. It can be remelted N times according to demand. Through this method, the density of NiTi alloy parts can be improved and the mechanical properties can be optimized during the laser selective melting manufacturing process, and the phase transition temperature of NiTi alloy can be not affected, and the phase transition temperature can even be further increased, so that NiTi alloy exhibits a strong shape memory property. Thereby expanding the optional range of the laser selective melting manufacturing process window of NiTi alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the remelting scan used in optimizing the NiTi alloy product sample in Example 1;

[0028] Figure 2 It is the metallographic microscopic observation picture of the NiTi alloy sample before and after optimization;

[0029] Figure 3 It is the DSC curve of the NiTi alloy sample before and after optimization;

[0030] Figure 4It is the tensile mechanical curve of NiTi alloy sample before and after optimization. DETAILED DESCRIPTION

[0031] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0032] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0033] The conditions for the phase transition temperature test in the embodiments and comparative examples are as follows: a differential scanning calorimeter of model Netzsch DSC 200F3 is used, the heating / cooling rate is 10°C / min, the test temperature range is -50 to 180°C, and the transition temperature is measured in a nitrogen atmosphere.

[0034] Test conditions of the tensile test: According to the national standard GB / T 228.1-2010, a universal testing machine model INSTRON3369 was used to carry out the tensile test at a constant loading speed of 1 mm / min and room temperature (25°C) (an extensometer was used throughout the process).

[0035] Mechanical properties test conditions: The total elongation at break, tensile strength and yield strength are sorted according to the data processing method of the national standard GB / T 228.1-2010.

[0036] like Figure 1 As shown, it is a schematic diagram of repeated scanning, wherein the path indicated by the arrow of the first scan is the path of the laser scanning, which is a checkerboard scan; for the Nth (such as the second or third or fourth) different remelting scans, the path indicated by the arrow is the path of the laser remelting scan.

[0037] Example 1

[0038] according to Figure 1 The principle shown is to manufacture a nickel-titanium tensile part with only one laser remelting scan.

[0039] The tensile part model was transferred into the laser selective melting equipment, and the process parameters of the first laser scanning were set as follows: laser power 60W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and the energy density was 87.27J / mm 3; Then laser remelting was performed. The process parameters of the first laser remelting scan were set as follows: laser power 45W, and other parameters remained unchanged. At this time, the corresponding energy density was 65.45J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A3-45.

[0040] Through microscopic observation, Figure 2 As shown in (g), there are no large cracks and obvious keyholes; after the phase change temperature test, Figure 3 As shown in (b), the M of sample A3-45 s The temperature is 67.6℃; after the tensile test, Figure 4 As shown in (b), the mechanical properties of the A3-45 sample are: tensile strength 440 MPa, and elongation at break 6.7%.

[0041] Example 2

[0042] Manufacture a tensile part with only one laser remelting scan. The tensile part model is transferred to the laser selective melting equipment, and the process parameters of the first laser scan are set as follows: laser power 60W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy is chessboard scanning, spot diameter (d) is 30μm, and the energy density is 87.27J / mm 3 ; Then laser remelting was performed. The process parameters of the first laser remelting scan were set as follows: laser power 60W, and other parameters remained unchanged. The corresponding energy density at this time was 87.27J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A3-60.

[0043] Through microscopic observation, Figure 2 As shown in (h), there are no large cracks and obvious keyholes; after the phase change temperature test, Figure 3 As shown in (b), the M of the A3-60 sample s The temperature is 73.7℃; after the tensile test, Figure 4 As shown in (b), the mechanical properties of the A3-60 sample are: tensile strength 410 MPa, and elongation at break 6.4%.

[0044] Example 3

[0045] Manufacture a tensile part with only one laser remelting scan. The tensile part model is transferred to the laser selective melting equipment, and the process parameters of the first laser scan are set as follows: laser power 60W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy is chessboard scanning, spot diameter (d) is 30μm, and the energy density is 87.27J / mm 3; Then laser remelting was performed. The process parameters of the first laser remelting scan were set as follows: laser power 30W, and other parameters remained unchanged. At this time, the corresponding energy density was 43.64J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A3-30.

[0046] Through microscopic observation, Figure 2 As shown in (f), there are no large cracks and obvious keyholes; after the phase change temperature test, Figure 3 As shown in (b), the M of sample A3-30 s The temperature is 51.1℃; after the tensile test, Figure 4 As shown in (b), the mechanical properties of the A3-30 sample are: tensile strength 260 MPa, and elongation at break 6.4%.

[0047] Comparative Example 1

[0048] The tensile part was manufactured with only one laser scan. The tensile part model was transferred to the laser selective melting equipment, and the scanning process parameters were set as follows: laser power 60W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and energy density 87.27J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as A3 sample.

[0049] Through microscopic observation, Figure 2 As shown in (c), compared with the remelting scanning optimized sample in Example 1, there are more obvious metallurgical pores; after the phase transition temperature test, as shown in Figure 3 As shown in (a), the M of sample A3 s The temperature is 49.1°C, which is lower than the M of the remelting scanning optimized sample in Example 1. s Temperature; After tensile test, such as Figure 4 As shown in (a), the mechanical properties of the A3 sample are: tensile strength 220 MPa, elongation at break 4.9%, which are poorer than the remelting scanning optimized sample in Example 1.

[0050] Comparative Example 2

[0051] The tensile part was manufactured with only one laser remelting scan. The tensile part model was transferred to the laser selective melting equipment, and the process parameters for the first scan were set as follows: laser power 60W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and the energy density was 87.27J / mm 3The process parameters for the second scan were set to: laser power 15W, and other parameters remained unchanged. The corresponding energy density was 21.82J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A3-15.

[0052] Through microscopic observation, Figure 2 As shown in (e) in the figure, compared with the remelting scanning optimized sample in Example 1, the number of metallurgical pores is not much different; after the phase transition temperature test, as shown in Figure 3 As shown in (b), the M of sample A3-15 s The temperature is 49.1°C, which is lower than the M of the remelting scanning optimized sample in Example 1. s Temperature; After tensile test, such as Figure 4 As described in (b), the mechanical properties of the A3-15 sample are: tensile strength 245 MPa, elongation at break 5.1%, which are inferior to the performance of the remelting scanning optimized sample in Example 1.

[0053] Comparative Example 3

[0054] The tensile part was manufactured with only one laser scan. The tensile part model was transferred to the laser selective melting equipment, and the scanning process parameters were set as follows: laser power 75W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and energy density 109.09J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as A4 sample.

[0055] Through microscopic observation, Figure 2 As shown in (d) in the figure, compared with the remelting scanning optimized sample in Example 1, there are many obvious metallurgical pores; after the phase transition temperature test, as shown in Figure 3 As shown in (a), the M of the A4 sample s The temperature is 62.92°C, which is similar to the M of the remelting scanning optimized sample in Example 1. s The temperature is almost the same; after the tensile test, such as Figure 4 As shown in (a), the mechanical properties of the A4 sample are: tensile strength 150 MPa, elongation at break 3.9%, which are poorer than the remelting scanning optimized sample in Example 1.

[0056] Comparative Example 4

[0057] The tensile part was manufactured with only one laser scan. The tensile part model was transferred to the laser selective melting equipment, and the scanning process parameters were set as follows: laser power 45W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and energy density 65.45J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A2.

[0058] Through microscopic observation, Figure 2 As shown in (b), compared with the remelting scanning optimized sample in Example 1, there are more obvious metallurgical pores; after the phase transition temperature test, as shown in Figure 3 As shown in (a), the M of sample A2 s The temperature is 20°C, which is much lower than the M of the scanned optimized sample in Example 1. s Temperature; After tensile test, such as Figure 4 As shown in (a), the mechanical properties of sample A2 are: tensile strength 460 MPa, elongation at break 6.1%, which are comparable to the performance of the scanning optimized samples in Example 1 and Example 2, proving that the mechanical properties of the sample can be significantly improved under this parameter condition.

[0059] Comparative Example 5

[0060] The tensile part was manufactured with only one laser scan. The tensile part model was transferred to the laser selective melting equipment, and the scanning process parameters were set as follows: laser power 30W, scanning speed 250mm / s, scanning spacing 110μm, powder layer thickness 25μm, scanning strategy chessboard scanning, spot diameter (d) 30μm, and the energy density was 43.64J / mm 3 ; Under argon protection, laser scanning was used for forming; recorded as sample A1.

[0061] Through microscopic observation, Figure 2 As shown in (a), compared with the sample manufactured by remelting scanning optimization in Example 3, there are more obvious unfused macropores; after phase transition temperature test, as shown in Figure 3 As shown in (a), the M of sample A1 s The temperature is 0°C, which is much lower than the M of the remelting scanning optimized sample in Example 3. s Temperature; After tensile test, such as Figure 4 As shown in (a), the mechanical properties of the A1 sample are: tensile strength 370 MPa, elongation at break 1.5%, which is poorer than the elongation of the remelted optimized sample in Example 3.

[0062] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for optimizing the performance of nickel-titanium alloy, It is characterized in that The method comprises the following steps: in the process of preparing nickel-titanium alloy by laser selective melting, after laser scanning each layer, the laser is used again to remelt the formed layer without re-powdering, and the number of remelting is recorded as N, where N≥1 and is an integer; Specifically, the three-dimensional STL data of the product is placed in the laser selective melting equipment, and the process parameters are assigned to the first laser scan according to the requirements, and then the laser is used again to assign process parameters to N laser remeltings in sequence according to the requirements; The process conditions of the first laser scanning include: scanning laser power P is 40-70W, spot diameter d is 30-50μm, scanning speed v is 250-500mm / s, scanning spacing h is 90-100μm, and powder layer thickness t is 25-30μm; The energy density of the process parameters used in each remelting laser scan is 72% to 100% of the energy density of the first laser scan, and the energy density formula is: E = P / vht; the selectable range of the process parameters used in each remelting laser includes: scanning laser power P of 40 to 70 W, spot diameter d of 35 to 45 μm, scanning speed v of 250 to 500 mm / s, scanning spacing h of 90 to 100 μm, and powder layer thickness t of 25 to 30 μm.

2. The method according to claim 1, It is characterized in that The energy density of the process parameters used in each remelting laser scan is 75% to 100% of the energy density during the first laser scan.

3. The method according to claim 1, It is characterized in that The scanning strategy of the laser scanning is chessboard scanning or island scanning.

4. The method according to any one of claims 1 to 3, It is characterized in that The powder used is pre-alloyed NiTi powder with a nearly equiatomic ratio prepared by atomic gas atomization. The powder particle diameter is distributed in the range of 15 to 53 μm and is vacuum dried before use.

5. The method according to claim 1, It is characterized in that The method comprises the steps of a) using CAD / CAE modeling software to design a model according to requirements; The three-dimensional STL data of the placed products are set according to the model designed in step a).

6. A method for preparing a nickel-titanium alloy product, It is characterized in that The preparation method comprises the following steps: using a laser to print and form a sample treated by the method for optimizing the performance of nickel-titanium alloy according to any one of claims 1 to 5 on a substrate to obtain a nickel-titanium alloy product.

7. The preparation method according to claim 6, It is characterized in that During the printing process, the oxygen content must be ensured to be ≤500ppm, argon gas protection is used, and the gas pressure is maintained at 10-20mbar.

8. The preparation method according to claim 6 or 7, It is characterized in that The substrate is a NiTi alloy substrate.