A method for online regeneration of hydrogen sulfide selective oxidation catalyst

Through the online oxygen-enriched oxidation method and gradient regeneration method, the problem of selective oxidation catalyst regeneration is solved, catalyst activity recovery and sulfur recovery rate are improved, and operating costs and flue gas emissions are reduced.

CN115722274BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110988926.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2024-10-01
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

There are few regeneration methods for selective oxidation catalysts in the existing technology, especially the inability to achieve online regeneration, which results in reduced catalyst activity and unstable device operation, affecting sulfur recovery and flue gas emissions.

Method used

By gradually lowering the inlet temperature of the Super Claus reactor, opening the bypass valve, increasing the amount of oxidation air, controlling the bed temperature increase and constant temperature treatment, and adopting the gradient regeneration method in an oxygen-rich environment, the catalyst activity is restored.

Benefits of technology

The catalyst activity is restored to more than 90%, the sulfur recovery rate is improved, the device operating cost and flue gas SO2 emissions are reduced, the regeneration process is simplified, and the frequency of catalyst replacement is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115722274B_ABST
    Figure CN115722274B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of sulfur recovery, and specifically relates to an online regeneration method for a catalyst for sulfur production by selective oxidation of hydrogen sulfide, which can be widely used in selective oxidation devices in industries such as petroleum refining and coal chemical industry. The online regeneration method for the hydrogen sulfide selective oxidation catalyst of the present invention adopts a super Claus bypass mode, and oxygen-enriched regeneration of the catalyst is performed by a blower. The entire regeneration process adopts step control, and each gradient controls the amount of oxidation air and the heating rate to perform oxygen-enriched activation regeneration on the catalyst. The method can realize the online regeneration of the selective oxidation catalyst, and the activity of the catalyst can be restored to more than 90% after regeneration. The entire device can achieve normal production without replacing the catalyst, which effectively improves the sulfur recovery rate of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sulfur recovery, and specifically relates to an online regeneration method for a catalyst for preparing sulfur by selective oxidation of hydrogen sulfide, which can be widely used in selective oxidation devices in industries such as petroleum refining and coal chemical industry. Background Art

[0002] In the traditional sulfur recovery process, the direct oxidation process is to directly catalyze the oxidation of hydrogen sulfide in the process gas into elemental sulfur by using a special catalyst. This process can treat both lean acid gas and conventional Claus tail gas, and has attracted widespread attention for its simple operation and high sulfur recovery rate.

[0003] The Super Claus process and the Euro Claus process are currently the most successful and widely used direct oxidation processes. Among them, the Super Claus sulfur recovery process is an extension of the traditional Claus process, that is, on the basis of the conventional Claus process, a selective catalytic oxidation reaction section is added to selectively oxidize the residual H2S in the process gas from the last Claus section to elemental sulfur. The reaction equation is: H2S+1 / 2O2→S+H2O. Based on this concept, the Claus part of the Super Claus process will no longer control H2S:SO2=2:1, but control the H2S concentration at the outlet of the last Claus reactor. Since the reaction is a thermodynamically complete reaction, a higher sulfur recovery rate can be obtained, which can reach more than 99.0%.

[0004] According to the principle of the Super Claus process, its core technology lies in the use of advanced hydrogen sulfide selective oxidation catalysts in the reaction section. In recent years, with the vigorous development of coal chemical technology, my country's hydrogen sulfide selective oxidation catalysts have also developed rapidly. At present, the new selective oxidation catalyst mainly uses non-toxic and harmless iron oxide as the active component, and adds corresponding promoters at the same time, so that the entire catalyst has high activity. However, in the actual application of the Super Claus process, it is found that the selective oxidation catalyst will become deactivated before the use cycle is reached due to improper operation of the device as the use time increases, resulting in a large decrease in activity. On the one hand, it affects the normal sulfur recovery rate of the device, and on the other hand, it also causes the flue gas SO2 emissions of the device to seriously exceed the standard, resulting in the device being unable to operate normally. Therefore, how to achieve the regeneration of the selective oxidation catalyst plays an important role in the sulfur recovery efficiency.

[0005] However, there are few reports on the regeneration of selective oxidation catalysts in the prior art, and most of them focus on the regeneration of hydrogenation catalysts. For example, the preparation method of the sulfurized regenerated hydrogenation catalyst disclosed in Chinese patent CN112337501A, the carbon-deactivated hydrogenation catalyst is first wetted with an oxygen-containing organic solvent, and then subjected to a mild sulfur-burning and carbon-burning treatment. After cooling, it is vacuum impregnated with a water-soluble sulfur-containing composite solution, and a sulfurized regenerated hydrogenation catalyst is obtained after heat treatment. For another example, the regeneration and revival method of heavy distillate oil hydroprocessing catalyst disclosed in Chinese patent CN112076804A is to place the regenerated catalyst in a solution containing an inorganic auxiliary agent and an organic chelating ligand auxiliary agent, and impregnate it under acoustic field conditions; the sample after impregnation is dried at room temperature; and then an activated catalyst is obtained by two-step heat treatment. However, the above-mentioned regeneration method for hydrogenation catalysts is not suitable for the regeneration of selective oxidation catalysts, and the operation process of this method is relatively complicated, and it is impossible to achieve online regeneration of the catalyst.

[0006] Therefore, it is of positive significance to explore a selective oxidation catalyst regeneration method, especially a method to achieve online regeneration, in order to ensure the catalyst service life, improve the sulfur recovery rate of the device, and reduce the frequency of catalyst replacement in the device. Summary of the invention

[0007] To this end, the technical problem to be solved by the present invention is to provide an online regeneration method for a hydrogen sulfide selective oxidation catalyst, which can regenerate the catalyst online, has a high catalyst regeneration rate, and a simple and easy regeneration process, can reduce the frequency of catalyst replacement in the device, and reduce the operating cost of the device, and has significant economic and social benefits.

[0008] In order to solve the above technical problems, the online regeneration method of a hydrogen sulfide selective oxidation catalyst described in the present invention comprises the following steps:

[0009] (1) gradually lowering the temperature at the inlet of the Super Claus reactor, opening all bypass valves of the Super Claus reactor, and closing all inlet valves of the Super Claus reactor;

[0010] (2) slowly opening the air valve of the Super Claus reactor and gradually increasing the amount of oxidizing air entering the Super Claus reactor until the air valve is fully opened;

[0011] (3) controlling the bed temperature of the Super Claus reactor to continuously increase, and performing a temperature-raising activation and regeneration treatment of the catalyst;

[0012] (4) continuing to control the bed temperature of the Super Claus reactor to rise to a temperature higher than the operating temperature of the catalyst, stopping the temperature increase and maintaining the temperature constant for constant temperature activation and regeneration treatment;

[0013] (5) After the activation treatment is completed, normal production is resumed.

[0014] Specifically, in step (1), the temperature at the inlet of the Super Claus reactor is controlled to be reduced to 180-190° C. The Super Claus inlet temperature needs to be reduced to 180-190° C. This is because regeneration is exothermic, and a too high inlet temperature easily leads to overheating of the catalyst bed. In addition, sulfur has the highest viscosity around 180° C., so a suitable temperature can avoid the high viscosity area of ​​liquid sulfur.

[0015] Specifically, in step (2), the amount of oxidation air needs to be determined according to the degree of catalyst deactivation and the temperature rise of the bed. Generally, the amount of oxidation air entering the Super Claus reactor is controlled to be 100-200 kg / h.

[0016] The method of the present invention first gradually reduces the inlet temperature of the Super Claus reactor to 190° C., and the process gas enters the incinerator through the bypass of the Super Claus reactor. At this time, the Super Claus reactor is operating in an oxygen-rich state, the air valve entering the Super Claus reactor is fully opened, and the Super Claus reactor supplies a maximum amount of oxidizing air.

[0017] Specifically, in step (2), the oxidizing air enters the Super Claus reactor through a blower. The blower of the present invention is mainly used to blow oxidizing air into the Super Claus reactor, because the sulfide in the catalyst is very stable in the process gas and needs to be removed in the oxygen-rich mode, so the blower is used in the Super Claus bypass mode to complete the regeneration of the catalyst.

[0018] Specifically, in step (3), the temperature rise rate of the bed of the Super Claus reactor is controlled to be 10-20° C. / h to avoid incomplete activation due to too fast a temperature rise or too long an activation time due to too slow a temperature rise.

[0019] Specifically, in step (3), the time of the temperature-raising activation and regeneration treatment step is controlled to be 8-10 hours.

[0020] Specifically, it is characterized in that in the step (4), the bed temperature of the Super Claus reactor is controlled to be increased to 10-30° C. higher than the operating temperature of the catalyst.

[0021] Specifically, in step (4), the time of the constant temperature activation and regeneration treatment step is 6-10 hours to ensure sufficient activation.

[0022] In the regeneration process of the present invention, if the Super Claus reactor is overheated, it is necessary to timely adjust the amount of oxidation air entering the Super Claus reactor and perform nitrogen protection on the catalyst.

[0023] Specifically, in the step (5), after the activation treatment is completed, the step further includes slowly reducing the amount of oxidizing air until the oxygen content in the outlet gas of the Super Claus reactor is 0.5% (V), and continuing the production operation under oxygen-rich conditions.

[0024] Specifically, it is characterized in that the hydrogen sulfide selective oxidation catalyst is a catalyst with Fe2O3 as the main active component. Through activation in an oxygen-rich environment, FeS in the catalyst is converted into Fe2O3, and the activation is completed.

[0025] The present invention is mainly applicable to the situation where the Super Claus catalyst is sulfided and loses its catalytic activity due to insufficient oxygen, resulting in excessively high concentrations of SO2 and H2S in the tail gas. The main active component of the Super Claus catalyst is Fe2O3. When the amount of oxygen entering the Super Claus reactor is insufficient, Fe2O3 reacts with H2S to generate FeS, which is an activator of the Claus reverse reaction, prompting sulfur to react with water to generate H2S and SO2, resulting in excessively high concentrations of SO2 and H2S in the tail gas and increased flue gas SO2 emissions.

[0026] In the scheme of the present invention, FeS is an active agent for the Claus reverse reaction:

[0027] 3S+2H2O→2H2S+SO2 (1)

[0028] The regeneration process of the present invention adopts an online oxygen-enriched oxidation method, strictly controls the air volume, adopts a gradient regeneration method, controls the bed temperature rise rate, and revives the catalyst under oxygen-enriched conditions. The reaction formula is as follows:

[0029] 3FeS+7O2→2Fe2O3+4SO2 (2)

[0030] After the above activation and regeneration process, the regeneration method of the present invention can restore the catalyst activity to more than 90%.

[0031] The online regeneration method of the hydrogen sulfide selective oxidation catalyst of the present invention is aimed at the situation that the Fe2O3-based super Claus catalyst is sulfided and loses its catalytic activity due to insufficient oxygen, resulting in excessive concentrations of SO2 and H2S in the tail gas. The super Claus bypass mode is adopted to regenerate the catalyst with oxygen enrichment by means of a blower. The whole regeneration process adopts step control. Each gradient controls the amount of oxidation air and the heating rate to regenerate the catalyst with oxygen enrichment activation. The method can realize the online regeneration of the selective oxidation catalyst. After regeneration, the catalyst activity can be restored to more than 90%. The whole device can realize normal production without replacing the catalyst, which effectively improves the sulfur recovery rate of the device. Moreover, the regeneration method can effectively increase the service life of the catalyst and effectively reduce the frequency of the device agent replacement. The regeneration process is simple and easy, environmentally friendly, and no secondary pollution is generated, which has significant economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0033] Figure 1 The present invention is a process flow chart of the online catalyst regeneration method. DETAILED DESCRIPTION

[0034] Example 1

[0035] The SO2 emission concentration of flue gas from the sulfur recovery unit of a methanol plant remained high, basically maintaining at 1000-2000mg / Nm 3 During operation, based on the sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 25-40%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0036] like Figure 1 The process flow chart shown in FIG. 1 shows, the regeneration of the catalyst in this embodiment comprises the following steps:

[0037] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 185° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0038] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 150 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0039] (3) controlling the bed of the Super Claus reactor to heat up at a heating rate of 10° C. / h to perform a heating activation and regeneration treatment of the catalyst for a total of 8 hours;

[0040] (4) When the bed temperature of the Super Claus reactor rises to 240° C., stop heating, and maintain the temperature to perform constant temperature activation and regeneration of the catalyst for 8 hours;

[0041] (5) During the entire activation process, the FeS in the catalyst is activated and converted into Fe2O3, and the activation is completed; then, the H2S concentration entering the Super Claus reactor of the entire system is adjusted to control the H2S concentration to be below 0.5%.

[0042] After the activation treatment in this embodiment is completed, the normal working condition can be restored. After observation and calculation, the conversion rate of H2S in the whole process reaches more than 95% and the SO2 emission of the flue gas of the device is maintained at 65mg / Nm 3 The following describes that the method has a good effect on the regeneration of the catalyst.

[0043] Example 2

[0044] The SO2 emission concentration of flue gas from the sulfur recovery unit of a fertilizer plant exceeded the standard, exceeding 2000mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 20-35%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0045] like Figure 1 The process flow chart shown in FIG. 1 shows, the regeneration of the catalyst in this embodiment comprises the following steps:

[0046] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 180° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0047] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 100 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0048] (3) controlling the bed of the Super Claus reactor to heat up at a heating rate of 20° C. / h to perform a heating activation and regeneration treatment of the catalyst for a total of 10 hours;

[0049] (4) When the bed temperature of the Super Claus reactor rises to 240° C., stop heating, and maintain the temperature to perform constant temperature activation and regeneration of the catalyst for 10 hours;

[0050] (5) During the entire activation process, the FeS in the catalyst is activated and converted into Fe2O3, and the activation is completed; then, the H2S concentration entering the Super Claus reactor of the entire system is adjusted to control the H2S concentration to be below 0.5%.

[0051] After the activation treatment in this embodiment is completed, the normal working condition can be restored. After observation and calculation, the conversion rate of H2S in the whole process reaches more than 92% after the activation treatment, and the SO2 emission of the flue gas of the device is maintained at 89mg / Nm 3 The following describes that the method has a good effect on the regeneration of the catalyst.

[0052] Example 3

[0053] The SO2 emission concentration of flue gas from a sulfur recovery unit exceeded the standard, exceeding 1200 mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 40-50%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0054] like Figure 1 The process flow chart shown in FIG. 1 shows, the regeneration of the catalyst in this embodiment comprises the following steps:

[0055] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 190° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0056] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 180 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0057] (3) controlling the bed of the Super Claus reactor to heat up at a heating rate of 13° C. / h to perform a heating activation and regeneration treatment of the catalyst for a total of 9 hours;

[0058] (4) When the bed temperature of the Super Claus reactor rises to 220° C., stop heating, and maintain the temperature to perform constant temperature activation and regeneration of the catalyst for 7 hours;

[0059] (5) During the entire activation process, the FeS in the catalyst is activated and converted into Fe2O3, and the activation is completed; then, the H2S concentration entering the Super Claus reactor of the entire system is adjusted to control the H2S concentration to be below 0.5%.

[0060] After the activation treatment in this embodiment is completed, the normal working condition can be restored. After observation and calculation, the conversion rate of H2S in the whole process reaches more than 96% after the activation treatment, and the SO2 emission of the flue gas of the device is maintained at 62mg / Nm 3 The following describes that the method has a good effect on the regeneration of the catalyst.

[0061] Example 4

[0062] The SO2 emission concentration of flue gas from a sulfur recovery unit exceeded the standard, reaching 800mg / Nm 3During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 55-65%, and the catalyst was deactivated, so the catalyst needed to be regenerated.

[0063] like Figure 1 The process flow chart shown in FIG. 1 shows, the regeneration of the catalyst in this embodiment comprises the following steps:

[0064] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 190° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0065] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 200 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0066] (3) controlling the bed of the Super Claus reactor to heat up at a heating rate of 10° C. / h to perform a heating activation and regeneration treatment of the catalyst for a total of 8 hours;

[0067] (4) When the bed temperature of the Super Claus reactor rises to 230° C., stop heating, and maintain the temperature to perform constant temperature activation and regeneration of the catalyst for 6 hours;

[0068] (5) During the entire activation process, the FeS in the catalyst is activated and converted into Fe2O3, and the activation is completed; then, the H2S concentration entering the Super Claus reactor of the entire system is adjusted to control the H2S concentration to be below 0.5%.

[0069] After the activation treatment in this embodiment is completed, the normal working condition can be restored. After observation and calculation, the conversion rate of H2S in the whole process reaches more than 98% and the SO2 emission of the flue gas of the device is maintained at 56mg / Nm 3 The following describes that the method has a good effect on the regeneration of the catalyst.

[0070] Comparative Example 1

[0071] The SO2 emission concentration of flue gas from the sulfur recovery unit of a methanol plant remained high, basically maintaining at 1000-2000mg / Nm 3 During operation, based on the sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 25-40%, and the catalyst was seriously deactivated.

[0072] Due to the long-term excessive flue gas emissions from the device, the entire device was shut down and a new catalyst was replaced. After the device was restored to operation, the catalyst was only used for two and a half years. The entire replacement cost 500,000 yuan, resulting in high operating costs for the device.

[0073] Comparative Example 2

[0074] The SO2 emission concentration of flue gas from a sulfur recovery unit exceeded the standard, reaching 800mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 55-65%, and the catalyst was deactivated.

[0075] After the deactivated catalyst was used for a period of time, the flue gas emission concentration of the device continued to rise and could not meet the environmental protection standards, so the plant had to be shut down for catalyst replacement. After the catalyst was replaced, the flue gas SO2 emission of the device could be maintained at 45mg / Nm 3 However, the entire agent replacement operation cost a total of 420,000 yuan, and the shutdown of the unit for agent replacement caused the upstream unit to produce at low load, which greatly increased the unit operating costs.

[0076] Comparative Example 3

[0077] The SO2 emission concentration of flue gas from a sulfur recovery unit remained high, basically maintained at 1500mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 25-40%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0078] The regeneration of the catalyst described in this comparative example comprises the following steps:

[0079] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 185° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0080] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 150 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0081] (3) controlling the bed of the Super Claus reactor to heat up at a heating rate of 10° C. / h to perform a heating activation and regeneration treatment of the catalyst for a total of 8 hours;

[0082] (4) When the bed temperature of the Super Claus reactor rises to 240° C., heating is stopped and activation is completed;

[0083] (5) Subsequently, the H2S concentration entering the Super Claus reactor is adjusted throughout the system to be controlled below 0.5%.

[0084] After the activation treatment in this embodiment, the normal working condition is restored. After observation and calculation, the conversion rate of H2S is above 60% and the SO2 emission of the flue gas is greater than 800mg / Nm 3 , which shows that the catalyst activation is not complete and still cannot meet the needs of the device.

[0085] Comparative Example 4

[0086] The SO2 emission concentration of flue gas from the sulfur recovery unit of a methanol plant remained high, basically maintained at 1200mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 35-50%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0087] The regeneration of the catalyst described in this comparative example comprises the following steps:

[0088] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 185° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0089] (2) slowly opening the air valve 1 of the Super Claus reactor, controlling the amount of oxidizing air added each time to 150 kg / h, until the air valve 1 is fully opened and the maximum amount of oxidizing air supplied to the Super Claus reactor is reached;

[0090] (3) raising the bed temperature of the Super Claus reactor to 240° C., stopping heating, and maintaining the temperature to perform constant temperature activation and regeneration of the catalyst for 10 hours;

[0091] (4) Subsequently, the H2S concentration entering the Super Claus reactor is adjusted throughout the system to be controlled below 0.5%.

[0092] After the activation treatment in this embodiment, the normal working condition is restored. After observation and calculation, the conversion rate of H2S is above 70% and the SO2 emission of the flue gas is greater than 600mg / Nm 3 This indicates that the catalyst activation is not complete and still cannot meet the device requirements.

[0093] Comparative Example 5

[0094] The SO2 emission concentration of flue gas from a sulfur recovery unit remained high, basically maintaining at 2000mg / Nm 3 During operation, based on sampling and analysis of the H2S concentration at the inlet and outlet of the Super Claus reactor, it was calculated that the hydrogen sulfide conversion rate of the catalyst in the Super Claus reactor was between 30-45%, and the catalyst was severely deactivated, so the catalyst needed to be regenerated.

[0095] The regeneration of the catalyst described in this comparative example comprises the following steps:

[0096] (1) gradually lowering the temperature at the inlet of the Super Claus reactor to 185° C., then opening all bypass valves 3 of the Super Claus reactor and closing all inlet valves 2 of the Super Claus reactor;

[0097] (2) opening all the air valves 1 of the Super Claus reactor to supply the maximum amount of oxidation air to the Super Claus reactor;

[0098] (3) The temperature of the Super Claus reactor is gradually increased to activate the catalyst. At the beginning of the activation, the bed temperature rises slowly. After a certain period of time, the bed temperature rises rapidly and the catalyst experiences a temperature spike. The device urgently takes various measures to cool down and the activation process is forced to terminate.

[0099] After the activation treatment in this embodiment, the normal working condition is restored. After observation and calculation, the conversion rate of H2S is below 20% and the SO2 emission of the flue gas is greater than 8000mg / Nm 3 The reason is that the catalyst was completely deactivated due to the long runaway time, and the unit had to be shut down for catalyst replacement.

[0100] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. An online regeneration method for a hydrogen sulfide selective oxidation catalyst, It is characterized in that The steps include: (1) gradually reducing the temperature at the inlet of the Super Claus reactor, opening all bypass valves of the Super Claus reactor, and closing all inlet valves of the Super Claus reactor; (2) slowly opening the air valve of the Super Claus reactor and gradually increasing the amount of oxidizing air entering the Super Claus reactor until the air valve is fully opened; (3) controlling the bed temperature of the Super Claus reactor to continuously increase, and performing a temperature-raising activation and regeneration treatment of the catalyst; (4) continuing to control the bed temperature of the Super Claus reactor to rise to a temperature higher than the operating temperature of the catalyst, stopping the temperature increase and maintaining the temperature constant for constant temperature activation and regeneration treatment; (5) After the activation treatment is completed, resume normal production; Wherein, in the step (1), the temperature at the inlet of the Super Claus reactor is controlled to be reduced to 180-190°C; in the step (2), the amount of oxidation air entering the Super Claus reactor is controlled to be 100-200 kg / h; in the step (3), the heating rate of the bed of the Super Claus reactor is controlled to be 10-20°C / h; in the step (4), the bed temperature of the Super Claus reactor is controlled to be increased to 10-30°C higher than the operating temperature of the catalyst, and the hydrogen sulfide selective oxidation catalyst is a catalyst with Fe2O3 as the main active component.

2. The online regeneration method of the hydrogen sulfide selective oxidation catalyst according to claim 1, It is characterized in that In the step (2), the oxidizing air enters the Super Claus reactor through a blower.

3. The online regeneration method of the hydrogen sulfide selective oxidation catalyst according to claim 1, It is characterized in that In the step (3), the time of the temperature-raising activation and regeneration treatment step is controlled to be 8-10 hours.

4. The online regeneration method of the hydrogen sulfide selective oxidation catalyst according to claim 1, It is characterized in that In the step (4), the time of the constant temperature activation regeneration treatment step is 6-10 hours.

5. The on-line regeneration method of the hydrogen sulfide selective oxidation catalyst according to claim 1 or 2, It is characterized in that In the step (5), after the activation treatment is completed, the step also includes slowly reducing the amount of oxidizing air until the oxygen content in the outlet gas of the Super Claus reactor is 0.5V%, and continuing the production operation under oxygen-rich conditions.