A method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomers

The polycarboxylic acid water reducing agent monomer is synthesized through microchannels, and the design of sulfonic acid groups is used to solve the problem of insufficient concrete and ease, improve the flowability, cohesion and water retention of concrete, and enhance the engineering structure. Strength and durability.

CN115725067BActive Publication Date: 2024-11-15FUSHUN DONGKE FINE CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211632394.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-11-15
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the flowability, cohesion and water retention of concrete, especially when natural sand and gravel mining is limited and machine sand quality management is poor, which affects the concrete and easy performance.

Method used

Polycarboxylic acid water reducer monomers are synthesized through microchannels, and the sulfonic acid groups are linked to the monomers using molecular structure design. Unsaturated esters containing hydroxybenzene ring react with epoxides to combine with the T of the microchannel reactor The structure of type hedging and Zig-zag mixer is precisely contacted with functional groups and improves the efficiency of polycarboxylic acid water reducing agent.

Benefits of technology

It significantly improves the and ease of concrete, enhances the strength and durability of the engineering structure, delays the hydration reaction, improves the dispersed slump retention effect, and improves the flowability and water retention of concrete.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-workability sulfonic acid group monomer for a microchannel synthetic polycarboxylic acid water-reducing agent monomer, comprising the following steps: ① synthesis of unsaturated esters containing hydroxyl benzene rings; ② preparation of macromonomers containing benzene rings; ③ synthesis of workability monomers. The invention uses p-hydroxybenzoic acid and unsaturated ene alcohol to obtain an unsaturated ester initiator containing hydroxyl benzene rings under acidic catalyst conditions, and the initiator is then ring-opened polymerized with epoxide in two steps to generate a crude monomer, and then the crude monomer containing a benzene ring structure is sulfonated to obtain a monomer with a sulfonic acid group. The polycarboxylic acid water-reducing agent prepared by the monomer improves the strength of concrete engineering structures and the durability requirements of engineering structures on the basis of maintaining the original performance of conventional PCE due to the presence of the benzene sulfonic acid group structure, and at the same time, the sulfonic acid group can stably adsorb the surface of adhesive cement particles, which can effectively delay the hydration reaction, enhance the dispersion and collapse protection effect in medium and low strength grade concrete, and also improve the workability of concrete mixtures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polycarboxylate water-reducing agent monomer synthesis, and relates to a method for preparing a high-workability sulfonic acid group monomer for microchannel synthesis of polycarboxylate water-reducing agent monomers. Background Art

[0002] With the development of social construction, projects are getting bigger and bigger, and the structures are getting more and more complex. The requirements for the workability of concrete mixtures are getting higher and higher. At the same time, most of the concrete is pumped concrete. Pumped concrete is concrete that is transported and poured along the pipeline under the push of a pump. Therefore, in addition to meeting the strength, durability and other properties specified in the design, the requirements for concrete also need to improve the workability of the concrete mixture. Make the concrete have good fluidity and water retention. The workability of concrete mainly includes three aspects, namely fluidity, cohesion and water retention. Fluidity refers to the performance of fresh concrete that can flow and fill the formwork evenly and densely under the action of its own weight or mechanical vibration; cohesion refers to the performance that the constituent materials of fresh concrete have a certain cohesion, and it is not easy to have stratification and segregation during the construction process; water retention refers to the performance that fresh concrete has a certain water retention capacity and will not produce serious water seepage during the construction process.

[0003] Generally speaking, when preparing concrete, if well-graded aggregates and a reasonable sand ratio are used, the workability of concrete can be easily guaranteed. However, in recent years, due to environmental pressure, the mining of natural sand and gravel has been gradually restricted, and high-quality natural sand and gravel has become less and less. Problems such as poor grading, high mud content and harmful impurities have become more and more common. At the same time, machine-made sand also has problems such as lack of quality management and control system, high production cost pressure, insufficient processing technology and processing equipment, and uneven parent rock varieties and quality. These factors seriously affect the workability of concrete, such as fluidity, cohesion and water retention. Therefore, some academic papers and patents have begun to focus on and study methods to improve the workability of concrete.

[0004] Lu Zhiming et al. (Lu Zhiming, Zeng Shijiao, Deng Huanyou, Zhong Yilin, Wei Chaodan. Synthesis and performance study of a polycarboxylic acid-based high-performance water-reducing agent that significantly improves the workability and slump retention of concrete [J]. Guangdong Building Materials, 2020, (9): 4-8.) used ethylene glycol monovinyl polyglycol ether, acrylic acid, and isomeric esters (Clariant, Germany) as polymerization monomers, and introduced isomeric esterified monomers with special structures on the side chains through free radical copolymerization to give it good workability.

[0005] Wan Tianming et al. (Wan Tianming, Ling Chao, Yang Zhifei. Research on the synthesis of low water seepage, high workability and collapse-preserving polycarboxylic acid water reducer [J]. New Building Materials, 2021, (2): 18-22.) used new 2+2 structure macromonomers ethylene glycol monovinyl polyoxyethylene ether, acrylic acid, hydroxypropyl acrylate and 2-acrylamide-2-methylpropane sulfonic acid as the main raw materials, and used a low-temperature initiation system to carry out free radical polymerization in aqueous solution to prepare a low-sensitivity, high workability and collapse-preserving polycarboxylic acid water reducer.

[0006] Huang Zhen et al. (Huang Zhen, Yang Yong, Wang Tao, Xia Zhengyi, Zhou Dongliang. Synthesis and performance study of a new concrete workability improver [J]. New Building Materials, 2021, (10): 100-103.) used acrylic acid, 2-allyl-2-methylpropanesulfonic acid, N,N-dimethylacrylamide and isopentanol polyoxyethylene ether as copolymer monomers and azobisisobutylamidine hydrochloride as initiator to synthesize a workability improver with good compatibility with polycarboxylic acid water reducer and which can significantly improve the segregation and bleeding phenomenon of concrete through aqueous solution free radical copolymerization.

[0007] Patent publication number CN105271883A discloses a water-reducing composite modified starch thickener, its preparation method and its application. It mentions that maltodextrin molecules are etherified and modified, and then sulfonic acid groups are introduced. The functional groups are used to make concrete admixtures, which are added to concrete to thicken the concrete and improve the workability of the concrete.

[0008] Comparative papers and patents show that the main measures to improve the workability of polycarboxylic acid water-reducing agent are to compound a certain substance with the polycarboxylic acid water-reducing agent mother liquor, or to use vinyl acetate, polypropylene glycol diacrylate, ethylene glycol monovinyl polyethylene glycol ether, functional esters, acrylamide or 2-acrylamide-2-methylpropane sulfonic acid, etc. to react with acrylic acid and polyether macromonomers for free radical copolymerization, and to introduce functional raw materials in the synthesis process of preparing water-reducing agent to solve the problem. The present invention links the functional group to the monomer through molecular structure design, so that the monomer has functionality, thereby enabling the synthesized water-reducing agent to have the ability to improve the workability of concrete. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing a high-workability sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomers. The method links a functional group to the polycarboxylic acid water-reducing agent monomer through molecular structure design, so that the polycarboxylic acid water-reducing agent monomer has functionality, thereby enabling the synthesized water-reducing agent to have the ability to improve the workability of concrete.

[0010] The technical solution adopted by the present invention is: the method comprises the following steps:

[0011] ①Synthesis of unsaturated esters containing hydroxyl benzene rings: Add p-hydroxybenzoic acid into a container, add an acid catalyst, dropwise add unsaturated enol at room temperature at a uniform rate, and obtain unsaturated esters containing hydroxyl benzene rings after reduced pressure distillation at 110°C;

[0012] ② Preparation of a benzene ring-containing macromonomer: add the unsaturated ester containing a hydroxyl benzene ring obtained in step ① into a reaction kettle, and then add an appropriate alkaline catalyst in a certain proportion; seal the kettle and replace it with high-purity nitrogen three times, raise the temperature to 80-90° C., introduce 10% of the total amount of epoxy compound to initiate ring-opening and connect to the para-hydroxyl group of the unsaturated ester, and when the pressure drops to 0 MPa, slowly introduce the remaining epoxide to continue ring-opening polymerization to form a polyether, and control the temperature at 110-130° C. and the pressure at no more than 0.5 MPa. After the feeding is completed, mature for 2 hours, remove the lightness at 90-110° C. for 0.5 hour, and neutralize with an organic acid to obtain a crude monomer;

[0013] ③ Synthesis of workability monomer: Add purified water to the crude monomer obtained in step ② to prepare a 30% aqueous solution, heat it to 70°C and then pump it into the microchannel reactor using a flow pump. After 1 minute, turn on the dilute sulfuric acid flow pump to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. A 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 5.50-7.00; after the insulation reaction is completed, maintain 90°C for reduced pressure distillation for 2 hours until no low-boiling fraction is removed, cool it to below 60°C and discharge it. Gas chromatography is used for analysis and detection, and the content of high workability functional monomers is more than 98%.

[0014] The unsaturated ene alcohol used in the above step ① is one or a mixture of allyl alcohol, methacryl alcohol, isopentenol, and the molar ratio of p-hydroxybenzoic acid to the unsaturated ene alcohol is 1:1-1.3, preferably 1:1.05-1.15.

[0015] The acid catalyst used in the above step ① is concentrated sulfuric acid or phosphoric acid, and the acid catalyst accounts for 1% to 1.5% of the total mass, preferably 1.05 to 1.25%.

[0016] The alkaline catalyst used in the above step ② is an alkali metal, an alkali metal hydroxide, an alkali metal hydride, an alkaline earth metal hydroxide, an alkali metal alkoxide, an alkaline earth metal oxide, an organic base and two or more thereof; wherein the alkali metal is sodium or potassium; the alkali metal hydroxide is potassium hydroxide, sodium hydroxide or lithium hydroxide; the alkali metal hydride is sodium hydride or potassium hydride; the alkaline earth metal hydroxide is magnesium hydroxide or calcium hydroxide; the alkali metal alkoxide is sodium methoxide, sodium ethoxide, potassium methoxide or potassium glycerolate; the alkaline earth metal oxide is magnesium oxide or calcium oxide; the organic base is ethanolamine, diethanolamine, triethanolamine, dimethylamine, trimethylamine, diethylamine or triethylamine; the alkaline catalyst accounts for 0.5% to 1.5% of the total mass, preferably 1% to 1.2%.

[0017] In the above step ②, the epoxide introduced is ethylene oxide or a mixture of ethylene oxide and propylene oxide, and its initiating amount does not exceed 5% of the total feed amount; wherein propylene oxide accounts for 0% to 20% of the total mass of the epoxide, preferably 5% to 10%.

[0018] In the above step ②, the mass ratio of the unsaturated ester containing a benzene ring to the epoxide is 1:11-20, preferably 1:13-16.

[0019] The organic acid used in the above step ② is one or more of oxalic acid, citric acid, glacial acetic acid, and benzoic acid, preferably glacial acetic acid. After neutralization, the system pH is 6.50-7.00.

[0020] The neutralization time in the above step ② is 10 to 90 minutes and the temperature is 70 to 90°C, preferably 30 to 40 minutes and the temperature is 70 to 80°C.

[0021] In the above step ③, the concentration of the dilute sulfuric acid pumped into the microchannel reactor is 5.0% to 10.0%, and the pumping flow rate of the dilute sulfuric acid is 15 ml / min to 25 ml / min.

[0022] In the above step ③, the molar ratio of crude monomer, dilute sulfuric acid and sodium hydroxide is 1:1-1.05:1.05-1.15, preferably 1:1.03-1.05:1.05-1.08.

[0023] In the above step ③, the microchannel reactor must adopt a T-type hedge and Zig-zag combined mixer structure, which can accurately connect the functional group to the ortho position of the etherification group of the benzene ring, greatly improving the double bond retention rate of the product and ensuring the effective content of the synthetic water reducer.

[0024] The invention provides a method for preparing a high-workability sulfonic acid group monomer for a microchannel synthesized polycarboxylic acid water-reducing agent monomer. The method comprises the following steps: using p-hydroxybenzoic acid and an unsaturated ene alcohol to obtain an unsaturated ester initiator containing a hydroxyl benzene ring under an acidic catalyst condition; the initiator and an epoxide are subjected to two-step ring-opening polymerization to generate a crude monomer; and the crude monomer containing a benzene ring structure is sulfonated to obtain a monomer with a sulfonic acid group. The polycarboxylic acid water-reducing agent prepared by the monomer improves the strength of a concrete engineering structure and the durability requirements of the engineering structure on the basis of maintaining the original performance of a conventional PCE due to the presence of a benzene sulfonic acid group structure. At the same time, the sulfonic acid group can stably adsorb the surface of adhesive cement particles, effectively delay the hydration reaction, enhance the dispersion and collapse protection effect in medium and low strength grade concrete, and also improve the workability of the concrete mixture.

[0025] The present invention has the following advantages:

[0026] 1. The present invention adopts a process of reacting an unsaturated olefin ester containing a benzene ring with a mixture of ethylene oxide and propylene oxide in the synthesis process of a benzene ring-containing macromonomer. The polycarboxylic acid monomer obtained by this process has a benzene ring structure. During sulfonation, the sulfonic acid group can be linked to the ortho position of the benzene ring, and the functional group is stable. When used in concrete, the functionality is more prominent.

[0027] 2. The present invention uses a microchannel reactor as a reaction vessel in the synthesis process of the workable monomer, and utilizes the T-type hedging and Zig-zag combined mixer structure of the microchannel to accurately connect the functional group to the ortho position of the etherification group of the benzene ring. The efficient temperature control of the microchannel makes the reaction more stable, the by-products of the reaction are lower, and the double bond retention rate of the product is greatly improved. The content of high workability functional monomers is more than 98%, ensuring the effective content of the synthetic water reducer.

[0028] 3. The synthesis method provided by the present invention has simple process, convenient operation, short reaction cycle and excellent product performance, which is of great significance for the promotion and application of concrete. DETAILED DESCRIPTION

[0029] Embodiment 1:

[0030] ① Synthesis of unsaturated esters containing hydroxybenzene rings: 240 g of p-hydroxybenzoic acid was added to a four-necked bottle, and 4.13 g of concentrated sulfuric acid as a catalyst was added, 135.2 g of methyl propylene alcohol was added dropwise at a uniform rate at room temperature, and 334 g of methyl propylene p-hydroxybenzoate was obtained after reduced pressure distillation at 110°C.

[0031] ② Preparation of a macromonomer containing a benzene ring: 160 g of methyl acrylate obtained in step ① was added to a reactor, and then 25.6 g of potassium hydroxide was added. The reactor was sealed and replaced with high-purity nitrogen three times, and the temperature was raised to 80-90 ° C. 96 g of epoxy compound was introduced for initiation, and the pressure was controlled not to be higher than 0.1 MPa to initiate the reaction; after the reaction was successfully initiated, the reaction temperature was raised to 120 ° C., and the reaction pressure was controlled not to be higher than 0.5 MPa to continue the remaining 2304 g of epoxy compound (144 g of propylene oxide and 2256 g of ethylene oxide in the total epoxide). After the feeding was completed, it was aged for 2 hours, and the light was removed at 90-110 ° C for 0.5 hour, and 27.4 g of glacial acetic acid was added for neutralization to obtain 2560 g of a crude monomer with a molecular weight of 3072;

[0032] ③ Synthesis of workability monomer solution: 150g of the crude monomer with a molecular weight of 3072 obtained in step ② is added with 350g of pure water to prepare a 30% aqueous solution, and the solution is pumped into the microchannel reactor using a flow pump after heating to 70°C. 100g of 5% dilute sulfuric acid is prepared in advance. One minute after the monomer solution is pumped into the microreactor, the dilute sulfuric acid flow pump is turned on to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. 22.5g of 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 6.47. After the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed. Cool down to below 60°C and discharge. Gas chromatography is used for analysis and detection, and the content of high workability functional monomer is 98.72%.

[0033] Embodiment 2:

[0034] ① Synthesis of unsaturated esters containing hydroxybenzene rings: Add 240 g of p-hydroxybenzoic acid into a four-necked bottle, add 4.13 g of concentrated sulfuric acid as a catalyst, add 165.1 g of isopentenol dropwise at a uniform rate at room temperature, and obtain 355 g of isopentenyl p-hydroxybenzoate after reduced pressure distillation at 110°C.

[0035] ② Preparation of macromonomer containing benzene ring: 160g of isopentyl p-hydroxybenzoate obtained in step ① is added into the reaction kettle, and then 15.7g of sodium hydroxide is added, the kettle is sealed and replaced with high-purity nitrogen three times, the temperature is raised to 80-90°C, 83g of epoxy compound is introduced for initiation, and the pressure is controlled not to be higher than 0.1MPa to initiate the reaction; after the reaction is successfully initiated, the reaction temperature is raised to 125°C, and the reaction pressure is controlled not to be higher than 0.5MPa to continue the remaining 1997g of epoxy compound (125g of propylene oxide and 1955g of ethylene oxide in the total epoxide), and after the feeding is completed, it is aged for 2 hours, and the light is removed at 90-110°C for 0.5 hour, and 47.8g of benzoic acid is added for neutralization to obtain 2240g of crude monomer with a molecular weight of 2856;

[0036] ③ Synthesis of workability monomer solution: 150g of the crude monomer with a molecular weight of 2856 obtained in step ② is added with 350g of pure water to prepare a 30% aqueous solution, and the temperature is raised to 70°C and then pumped into the microchannel reactor using a flow pump. 106g of 5% dilute sulfuric acid is prepared in advance. One minute after the monomer solution is pumped into the microreactor, the dilute sulfuric acid flow pump is turned on to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. 22.7g of 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 6.38. After the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed. Cool down to below 60°C and discharge. Gas chromatography is used for analysis and detection, and the content of high workability functional monomer is 99.15%.

[0037] Embodiment 3:

[0038] ① Synthesis of unsaturated esters containing hydroxybenzene rings: Add 240 g of p-hydroxybenzoic acid into a four-necked bottle, add 3.83 g of phosphoric acid as a catalyst, add 111 g of allyl alcohol dropwise at room temperature, and obtain 310 g of allyl p-hydroxybenzoate after reduced pressure distillation at 110°C.

[0039] ② Preparation of macromonomer containing benzene ring: 160g of propylene p-hydroxybenzoate obtained in step ① is added into a reactor, and then 26.4g of sodium hydride is added, the reactor is sealed and replaced with high-purity nitrogen three times, the temperature is raised to 80-90°C, 90g of epoxy compound is introduced for initiation, and the pressure is controlled not to be higher than 0.1MPa to initially initiate the reaction; after the reaction is successfully initiated, the reaction temperature is raised to 123°C, and the reaction pressure is controlled not to be higher than 0.5MPa to continue the remaining 2150g of epoxy compound (157g of propylene oxide and 2083g of ethylene oxide in the total epoxide), and after the feeding is completed, it is aged for 2 hours, and the light removal is carried out at 90-110°C for 0.5 hour, and 66g of glacial acetic acid is used for neutralization to obtain 2400g of crude monomer with a molecular weight of 2670;

[0040] ③ Synthesis of workability monomer solution: 150g of the crude monomer with a molecular weight of 2670 obtained in step ② is added with 350g of pure water to prepare a 30% aqueous solution, and the temperature is raised to 70°C and then pumped into the microchannel reactor using a flow pump. 115g of 5% dilute sulfuric acid is prepared in advance. One minute after the monomer solution is pumped into the microreactor, the dilute sulfuric acid flow pump is turned on to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. 23.8g of 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 6.77. After the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed. Cool down to below 60°C and discharge. Gas chromatography is used for analysis and detection, and the content of high workability functional monomer is 99.06%.

[0041] Embodiment 4:

[0042] ① Synthesis of unsaturated esters containing hydroxybenzene rings: Add 240 g of p-hydroxybenzoic acid into a four-necked bottle, add 4.88 g of phosphoric acid as a catalyst, add 164 g of isopentenol dropwise at a uniform rate at room temperature, and obtain 355 g of isopentenyl p-hydroxybenzoate after reduced pressure distillation at 110°C.

[0043] ② Preparation of a macromonomer containing a benzene ring: 160g of the isopentyl p-hydroxybenzoate obtained in step ① is added to a reactor, and then 24.8g of potassium hydroxide is added, the reactor is sealed and replaced with high-purity nitrogen three times, the temperature is raised to 80-90°C, 93g of an epoxy compound is introduced for initiation, and the pressure is controlled to be no higher than 0.1MPa to initiate the reaction; after the reaction is successfully initiated, the reaction temperature is raised to 122°C, and the reaction pressure is controlled to be no higher than 0.5MPa to continue the remaining 2227g of epoxy compound (209g of propylene oxide and 2111g of ethylene oxide in the total epoxide). After the feeding is completed, it is aged for 2 hours, and the light removal is carried out at 90-110°C for 0.5 hour, and 54g of benzoic acid is added for neutralization to obtain 2480g of a crude monomer with a molecular weight of 3162;

[0044] ③ Synthesis of workability monomer solution: 150g of the crude monomer with a molecular weight of 3162 obtained in step ② is added with 350g of pure water to prepare a 30% aqueous solution, and the temperature is raised to 70°C and then pumped into the microchannel reactor using a flow pump. 96g of 5% dilute sulfuric acid is prepared in advance. One minute after the monomer solution is pumped into the microreactor, the dilute sulfuric acid flow pump is turned on to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. 20.5g of 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 6.56. After the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed. Cool down to below 60°C and discharge. Gas chromatography is used for analysis and detection, and the content of high workability functional monomer is 98.58%.

[0045] Embodiment 5:

[0046] ① Synthesis of unsaturated esters containing hydroxybenzene rings: 240 g of p-hydroxybenzoic acid was added to a four-necked bottle, and 4.12 g of phosphoric acid as a catalyst was added, 138 g of methyl allyl alcohol was added dropwise at a uniform rate at room temperature, and 334 g of methyl allyl p-hydroxybenzoate was obtained after reduced pressure distillation at 110°C.

[0047] ② Preparation of macromonomer containing benzene ring: 160g of methyl allyl p-hydroxybenzoate obtained in step ① is added into the reaction kettle, and then 24.8g of sodium methoxide is added, the kettle is sealed and replaced with high-purity nitrogen three times, the temperature is raised to 80-90°C, 102g of epoxy compound is introduced for initiation, and the pressure is controlled not to be higher than 0.1MPa to initiate the reaction; after the reaction is successfully initiated, the reaction temperature is raised to 122°C, and the reaction pressure is controlled not to be higher than 0.5MPa to continue the remaining 2458g of epoxy compound (128g of propylene oxide and 2432g of ethylene oxide in the total epoxide), and after the feeding is completed, it is aged for 2 hours, and the light removal is carried out at 90-110°C for 0.5 hour, and 97g of citric acid is added for neutralization to obtain 2720g of crude monomer with a molecular weight of 3264;

[0048] ③ Synthesis of workability monomer solution: 150g of the crude monomer with a molecular weight of 3264 obtained in step ② is added with 350g of pure water to prepare a 30% aqueous solution, and the temperature is raised to 70°C and then pumped into the microchannel reactor using a flow pump. 93.7g of 5% dilute sulfuric acid is prepared in advance. One minute after the monomer solution is pumped into the microreactor, the dilute sulfuric acid flow pump is turned on to pump the dilute sulfuric acid solution into the microchannel reactor. The temperature of the microchannel reactor is controlled between 80 and 90°C. 19.7g of 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution to pH = 6.23. After the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed. Cool down to below 60°C and discharge. Gas chromatography is used for analysis and detection, and the content of high workability functional monomer is 98.88%.

Claims

1. A method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylate water-reducing agent monomers, the method comprising the following steps: ① Synthesis of unsaturated esters containing hydroxyl benzene rings: p-hydroxybenzoic acid is added to a container, and an acid catalyst is added, and unsaturated enol is added dropwise at a uniform rate at room temperature, and unsaturated esters containing hydroxyl benzene rings are obtained after reduced pressure distillation at 110°C; ② Preparation of a benzene ring-containing macromonomer: add the unsaturated ester containing a hydroxyl benzene ring obtained in step ① into a reaction kettle, and then add an appropriate alkaline catalyst in a certain proportion; seal the kettle and replace it with high-purity nitrogen three times, raise the temperature to 80-90° C., introduce 10% of the total amount of epoxy compound to initiate ring-opening and connect to the para-hydroxyl group of the unsaturated ester, and when the pressure drops to 0 MPa, slowly introduce the remaining epoxide to continue ring-opening polymerization to form a polyether, and control the temperature at 110-130° C. and the pressure at no more than 0.5 MPa. After the feeding is completed, mature for 2 hours, remove the lightness at 90-110° C. for 0.5 hour, and neutralize with an organic acid to obtain a crude monomer; ③ Synthesis of workability monomer: Add purified water to the crude monomer obtained in step ② to prepare a 30% aqueous solution, heat it to 70°C and then pump it into the microchannel reactor using a flow pump, start the dilute sulfuric acid flow pump 1 minute later to pump the dilute sulfuric acid solution into the microchannel reactor, the temperature of the microchannel reactor is controlled between 80 and 90°C, and 10% sodium hydroxide solution is pumped into the end of the microchannel to neutralize the system solution pH = 5.50-7.00; after the insulation reaction is completed, maintain 90°C for 2 hours of reduced pressure distillation until no low-boiling fraction is removed, cool it to below 60°C and discharge it, analyze and detect it by gas chromatography, and the content of high workability functional monomer is more than 98%; In the step ③, the microchannel reactor must adopt a T-type hedge and Zig-zag combined mixer structure.

2. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The unsaturated ene alcohol used in step ① is one or a mixture of propylene alcohol, methyl propylene alcohol and isopentenol; the molar ratio of p-hydroxybenzoic acid to the unsaturated ene alcohol is 1:1-1.

3.

3. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The acid catalyst used in step ① is concentrated sulfuric acid or phosphoric acid, and the acid catalyst accounts for 1% to 1.5% of the total mass.

4. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The alkaline catalyst used in step ② is an alkali metal, an alkali metal hydroxide, an alkali metal hydride, an alkaline earth metal hydroxide, an alkali metal alkoxide, an alkaline earth metal oxide, an organic base and two or more thereof; wherein the alkali metal is sodium or potassium; the alkali metal hydroxide is potassium hydroxide, sodium hydroxide or lithium hydroxide; the alkali metal hydride is sodium hydride or potassium hydride; the alkaline earth metal hydroxide is magnesium hydroxide or calcium hydroxide; the alkali metal alkoxide is sodium methoxide, sodium ethoxide, potassium methoxide or potassium glycerolate; the alkaline earth metal oxide is magnesium oxide or calcium oxide; the organic base is ethanolamine, diethanolamine, triethanolamine, dimethylamine, trimethylamine, diethylamine or triethylamine; and the alkaline catalyst accounts for 0.5% to 1.5% of the total mass.

5. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The epoxide introduced in step ② is ethylene oxide or a mixture of ethylene oxide and propylene oxide, and its initiating amount does not exceed 5% of the total feed amount; wherein propylene oxide accounts for 0% to 20% of the total mass of the epoxide.

6. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: In the step ②, the mass ratio of the unsaturated ester containing a benzene ring to the epoxide is 1:11-20.

7. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The organic acid used in step ② is one or more of oxalic acid, citric acid, glacial acetic acid, and benzoic acid; after neutralization, the system pH is 6.50-7.

00.

8. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: The concentration of the dilute sulfuric acid pumped into the microchannel reactor in step ③ is 5.0% to 10.0%, and the pumping flow rate of the dilute sulfuric acid is 15 ml / min to 25 ml / min.

9. The method for preparing a highly workable sulfonic acid group monomer for microchannel synthesis of polycarboxylic acid water-reducing agent monomer according to claim 1, characterized in that: In step ③, the molar ratio of the crude monomer, dilute sulfuric acid and sodium hydroxide is 1:1-1.05:1.05-1.15.